Preparation method and application of a radiation cooling coating with self-cleaning function
By calcining titanium source compounds and silicates in an oxygen-rich environment, combined with nano-molybdenum oxide and silane coupling agents, a radiation refrigeration coating with self-cleaning function is formed, which solves the problem of dust adhesion in traditional coatings and improves photocatalytic activity. and service life.
Patent Information
- Application Number
- CN202311706478.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-12
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-12-12
AI Technical Summary
Traditional radiation refrigeration coatings lack self-cleaning functions, causing dust and dirty substances to easily adhere, reducing the refrigeration effect.
The titanium source compound and silicate are heated and calcined in an oxygen-rich environment to form titanium dioxide-silica composite nanoparticles, which are combined with nano-molybdenum oxide and silane coupling agent to form a network structure to enhance photocatalytic activity and self-cleaning performance.
The photocatalytic activity, anti-reflection rate and self-cleaning effect of the coating are improved, the service life is extended, and the photocatalytic degradation performance and bacteriostasis are enhanced.
Smart Images

Figure CN117586653B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of radiation refrigeration materials, and in particular relates to a preparation method and application of a radiation refrigeration coating with a self-cleaning function. Background Art
[0002] Global warming and energy crisis have become important issues that restrict human development, and energy conservation and emission reduction are important ways to solve the above problems. Radiative cooling, as a non-energy-consuming cooling method, has gradually attracted the attention of researchers. Radiating energy to outer space is an important mechanism for maintaining the temperature of the earth. The efficiency of radiative cooling depends on the spectral emissivity of the surface of the object. By adjusting the surface emissivity to improve the efficiency, it can become an important passive cooling method and can be widely used in temperature regulation of buildings, electronic heat dissipation and cooling of solar cells. Relying on the "atmospheric window" band (8-13μm), the energy emitted from the earth by radiative cooling accounts for 87% of the total radiative emission energy, and this band happens to be in the far infrared region of the normal temperature radiation of ground objects. The surface of the object can directly exchange heat with the space cold source close to 0K through the "atmospheric window". The radiative cooling surface emits strongly in this band, has high transmittance in the visible light band, and strongly reflects other bands. In this way, the imbalance between the output and incoming thermal radiation achieves a lower steady-state temperature than the surrounding environment.
[0003] However, the traditional radiation cooling coating lacks the self-cleaning function, which makes it easy for dust and dirty substances to adhere to the surface of the radiation cooling coating, reducing the cooling effect of the radiation cooling coating. Summary of the invention
[0004] In view of this, the purpose of the present invention is to provide a method for preparing a radiation cooling coating with a self-cleaning function and its application, aiming to solve the technical problem that the existing radiation cooling coating does not have a self-cleaning function.
[0005] In order to achieve the above object, the present invention provides the following technical solutions:
[0006] The present invention provides the following technical solution: a method for preparing a radiation cooling coating with a self-cleaning function, comprising the following steps:
[0007] S01: Mix the titanium source compound and the silicate in a mortar, heat and calcine them at 400-500° C. in an oxygen-rich environment for a certain period of time, and then perform rapid cooling to obtain a mixture A;
[0008] S02: ultrasonically dispersing mixture A into an organic solvent to obtain mixture B;
[0009] S03: Stirring the silane coupling agent, anhydrous ethanol and water in a certain mass ratio, ultrasonically vibrating for a certain period of time, adding the nano-molybdenum oxide dispersion, and mixing to obtain a mixture D, wherein the mass percentage content of the nano-molybdenum oxide in the mixture D is 8%-10%;
[0010] S04: coating the mixture D on the surface of the substrate, standing for a period of time, spraying the mixture B on the mixture D, and obtaining a radiation cooling coating with a self-cleaning function after drying.
[0011] Furthermore, the oxygen content in the oxygen-rich environment is greater than 30%.
[0012] Furthermore, the step S01 includes the following steps:
[0013] a. Mix the titanium source compound and the silicate in a mortar and heat and calcine at 500°C in an oxygen-rich environment for 4-5h;
[0014] b. Place the calcined product in an oil pan and cool for 2 hours, then place in ice water and cool for 2-3 hours.
[0015] Furthermore, the step S02 further includes the following steps:
[0016] Ultrasonic dispersion of the mixture A in an organic solvent, and addition of a surfactant and a steric hindrance agent, and sufficient dissolution at room temperature to obtain a mixture sol B1;
[0017] The mixture sol B1 is heat treated to obtain nanoparticles of the mixture B.
[0018] Furthermore, the particle size of the nanoparticles in the mixture B is 0.003 to 0.3 micrometers.
[0019] Furthermore, in the step of heat-treating the mixture sol B1 to obtain the nanoparticles of the mixture B, the heat treatment temperature is 500-550° C., and the heat treatment time is 2-3 hours.
[0020] Furthermore, the step S04 includes:
[0021] The mixture D is coated on the surface of the substrate and allowed to stand for 2-3 hours. The mixture B is sprayed on the mixture D by powder spraying, and then dried to obtain a radiation cooling coating with a self-cleaning function.
[0022] Furthermore, the silane coupling agent is one of γ-aminopropyltriethoxysilane, γ-glycidyloxypropyltrimethoxysilane and γ-methacryloxypropyltrimethoxysilane.
[0023] Furthermore, the titanium source compound is one or a mixed solution of any of butyl titanate, methyl titanate, ethyl titanate, titanium tetraisopropoxide, and titanium tetrachloride.
[0024] The present invention also provides an application of the radiation refrigeration material prepared by the above-mentioned radiation refrigeration material preparation method in application devices, and the application devices include solar cells, building glass, car windows, greenhouse films or communication equipment.
[0025] The beneficial effects of the present invention are as follows: compared with the prior art, the preparation method of a radiation cooling coating with a self-cleaning function in the present invention can obtain titanium dioxide-silicon dioxide composite nanoparticles by mixing a titanium source compound with a silicate and calcining them at a high temperature in an oxygen-rich environment. Moreover, by calcining in an oxygen-rich atmosphere, there is less chance of forming oxygen vacancies, so that the obtained titanium dioxide-silicon dioxide composite nanoparticles have a higher concentration of photogenerated holes, thereby enhancing the photocatalytic activity of the coating; on the other hand, by taking advantage of the high porosity of the silicon dioxide nanoparticles, the refractive index of the coating is reduced, and at the same time At the same time, the photo-induced hydrophilic property of titanium dioxide is also utilized, so that the coating can have both anti-reflection and self-cleaning effects; by using silane coupling agent as a binder, the firmness between molybdenum oxides is ensured, the service life of the coating is extended, and molybdenum oxide is combined with silane coupling agent to form a network structure to support titanium dioxide-silicon dioxide composite nanoparticles, avoid particle loss, and increase the service life of the coating. By using molybdenum oxide, the curing temperature can be reduced. On the other hand, it will not have a negative impact on the light transmittance of the self-cleaning film after film formation, but will help to improve the photocatalytic degradation performance and antibacterial properties of the self-cleaning film.
[0026] Other advantages, objectives and features of the present invention will be described in the following description and will be apparent to those skilled in the art to some extent, or those skilled in the art may be taught from the practice of the present invention. The objectives and other advantages of the present invention may be realized and obtained through the following description. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to make the purpose, technical solution and beneficial effects of the present invention clearer, the present invention provides the following drawings for illustration:
[0028] Figure 1 A flow chart of a method for preparing a radiation cooling coating with a self-cleaning function proposed in one embodiment of the present invention;
[0029] Figure 2 A flowchart of step S01 proposed in another embodiment of the present invention;
[0030] Figure 3 This is a flow chart of step S02 proposed in yet another embodiment of the present invention. DETAILED DESCRIPTION
[0031] like Figures 1 to 3 As shown, this embodiment proposes a method for preparing a radiation cooling coating with a self-cleaning function, comprising the following steps:
[0032] S01: Mix the titanium source compound and the silicate in a mortar, heat and calcine them at 400-500° C. in an oxygen-rich environment for a certain period of time, and then perform rapid cooling to obtain a mixture A;
[0033] S02: ultrasonically dispersing mixture A into an organic solvent to obtain mixture B;
[0034] S03: Stirring the silane coupling agent, anhydrous ethanol and water in a certain mass ratio, ultrasonically vibrating for a certain period of time, adding the nano-molybdenum oxide dispersion, and mixing to obtain a mixture D, wherein the mass percentage content of the nano-molybdenum oxide in the mixture D is 8%-10%;
[0035] S04: coating the mixture D on the surface of the substrate, standing for a period of time, spraying the mixture B on the mixture D, and obtaining a radiation cooling coating with a self-cleaning function after drying.
[0036] By mixing a titanium source compound with a silicate and calcining at a high temperature in an oxygen-rich environment, titanium dioxide-silicon dioxide composite nanoparticles can be obtained on the one hand, and calcining in an oxygen-rich atmosphere reduces the chance of forming oxygen vacancies, so that the obtained titanium dioxide-silicon dioxide composite nanoparticles have a higher concentration of photogenerated holes, and the photocatalytic activity of the coating is enhanced; on the other hand, by utilizing the advantage of the high porosity of the silicon dioxide nanoparticles, the refractive index of the coating is reduced, and at the same time, the photo-induced hydrophilicity of titanium dioxide is also utilized, so that the coating can have both anti-reflection and self-cleaning effects; by using a silane coupling agent as a binder, the firmness between molybdenum oxides is guaranteed, and the service life of the coating is extended, and a network structure is formed by combining molybdenum oxide and the silane coupling agent to support the titanium dioxide-silicon dioxide composite nanoparticles, avoid particle loss, and improve the service life of the coating, and by using molybdenum oxide, the curing temperature can be reduced, and on the other hand, it will not have a negative impact on the light transmittance of the self-cleaning film layer after film formation, but instead help to improve the photocatalytic degradation performance and antibacterial property of the self-cleaning film layer.
[0037] Preferably, the oxygen content in the oxygen-rich environment is greater than 30%. Specifically, the oxygen content of the oxygen-rich environment is 35%, 35%, 40%, 45%, 50%, 55%, etc. In this embodiment, by setting the oxygen content to be greater than 30%, it is guaranteed to be conducive to the formation of the titanium dioxide-silicon dioxide composite; at the same time, through the oxygen-rich environment, there is less chance of forming oxygen vacancies, so that the obtained titanium dioxide-silicon dioxide composite nanoparticles have a higher concentration of photogenerated holes, so that the photocatalytic activity of the coating is enhanced.
[0038] Furthermore, the step S01 includes the following steps:
[0039] a. Mix the titanium source compound and the silicate in a mortar and heat and calcine at 500°C in an oxygen-rich environment for 4-5h;
[0040] b. Place the calcined product in an oil pan and cool for 2 hours, then place in ice water and cool for 2-3 hours.
[0041] In this embodiment, the titanium source compound and the silicate are heated and calcined at 500°C for 4-5h to obtain a titanium dioxide-silicon dioxide composite nanoparticle precursor. The calcined titanium dioxide-silicon dioxide composite nanoparticle precursor is placed in an oil pan and ice water for cooling, thereby reducing the energy of the nanoparticle grain boundary growth, inhibiting the agglomeration of the nanoparticles, and obtaining titanium dioxide-silicon dioxide composite nanoparticles with smaller particle sizes, thereby significantly improving the anti-reflection and self-cleaning effects of the coating. In addition, by pre-oil cooling and subsequent ice water cooling, the "quenching" stress of the titanium dioxide-silicon dioxide composite nanoparticle precursor can be reduced, thereby avoiding the appearance of cracks in the titanium dioxide-silicon dioxide composite nanoparticles.
[0042] Preferably, the silane coupling agent is one of γ-aminopropyltriethoxysilane, γ-glycidyloxypropyltrimethoxysilane and γ-methacryloxypropyltrimethoxysilane.
[0043] Preferably, the titanium source compound is one or a mixed solution of any of butyl titanate, methyl titanate, ethyl titanate, titanium tetraisopropoxide, and titanium tetrachloride.
[0044] Furthermore, the step S02 further includes the following steps:
[0045] Ultrasonic dispersion of the mixture A in an organic solvent, and addition of a surfactant and a steric hindrance agent, and sufficient dissolution at room temperature to obtain a mixture sol B1;
[0046] The mixture sol B1 is heat treated to obtain nanoparticles of the mixture B.
[0047] In this embodiment, by ultrasonically dispersing mixture A, i.e., titanium dioxide-silicon dioxide composite nanoparticle solution, into an organic solvent, and adding surfactants and steric hindrances, an oil phase material can be formed, which provides a guarantee for the subsequent coating to be better spread on the substrate. At the same time, the volatilization loss caused by thermal decomposition of mixture A during the subsequent heat treatment is reduced; through heat treatment, smaller-sized nanoparticles can be obtained, and more titanium dioxide-silicon dioxide composite nanoparticles per unit area can be obtained, which significantly improves the photocatalytic activity of the coating, and significantly improves the anti-reflection and self-cleaning effects of the coating.
[0048] Preferably, the surfactant is any one of dodecyltrimethylammonium chloride or hexadecyltrimethylammonium bromide. Of course, in this embodiment, the surfactant may also be other materials, which is not limited here.
[0049] In this embodiment, the mixture A is titanium dioxide-silicon dioxide composite nanoparticles; the mixture B1 is a titanium dioxide-silicon dioxide composite nanoparticle sol precursor; and the mixture B is a titanium dioxide-silicon dioxide composite nanoparticle sol.
[0050] Preferably, the particle size of the nanoparticles of the mixture B is 0.003-0.3 micrometers. Specifically, the particle size of the nanoparticles of the mixture B is 0.003 micrometers, 0.01 micrometers, 0.02 micrometers, 0.03 micrometers, 0.1 micrometers, 0.2 micrometers, 0.3 micrometers, etc.
[0051] Furthermore, in the step of heat-treating the mixture sol B1 to obtain the nanoparticles of the mixture B, the heat treatment temperature is 500-550° C., and the heat treatment time is 2-3 hours.
[0052] Furthermore, the step S04 includes:
[0053] The mixture D is coated on the surface of the substrate and allowed to stand for 2-3 hours. The mixture B is sprayed on the mixture D by powder spraying, and then dried to obtain a radiation cooling coating with a self-cleaning function.
[0054] In this embodiment, powder spraying is adopted to spray on mixture D, so that the bonding force between mixture B and mixture D can be improved, titanium dioxide-silicon dioxide composite nanoparticles can be effectively supported, particle loss can be avoided, and the service life of the coating can be improved.
[0055] The present application also provides an application of the radiation refrigeration material prepared by the above-mentioned radiation refrigeration material preparation method in an application device, and the application device includes a solar cell, building glass, car window, greenhouse coating or communication equipment.
[0056] Finally, it should be noted that the above preferred embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail through the above preferred embodiments, those skilled in the art should understand that various changes can be made in form and details without departing from the scope defined by the claims of the present invention.
Claims
1. A method for preparing a radiation cooling coating with a self-cleaning function, characterized in that: The steps include: S01: Mix the titanium source compound and the silicate in a mortar and heat and calcine at 500°C for 4-5 hours with an oxygen content greater than 30%, and then cool the calcined product in an oil pan for 2 hours, and then cool it in ice water for 2-3 hours to obtain a mixture A; S02: ultrasonically dispersing mixture A into an organic solvent to obtain mixture B; S03: Stirring the silane coupling agent, anhydrous ethanol and water in a certain mass ratio, ultrasonically vibrating for a certain period of time, adding the nano-molybdenum oxide dispersion, and mixing evenly to obtain a mixture D, wherein the mass percentage content of the nano-molybdenum oxide in the mixture D is 8%-10%; S04: coating the mixture D on the surface of the substrate, leaving it to stand for a period of time, spraying the mixture B on the mixture D, and obtaining a radiation cooling coating with a self-cleaning function after drying; The mixture A is ultrasonically dispersed in an organic solvent, and a surfactant and a steric hindrance agent are added and fully dissolved at room temperature to obtain a mixture sol B1; The mixture sol B1 is heat treated at a temperature of 500-550° C. for 2-3 hours to obtain nanoparticles of the mixture B. The particle size of the nanoparticles of the mixture B is 0.003-0.3 μm.
2. The method for preparing a radiation cooling coating with a self-cleaning function according to claim 1, characterized in that: The step S04 comprises: The mixture D is coated on the surface of the substrate and allowed to stand for 2-3 hours. The mixture B is sprayed on the mixture D by powder spraying, and then dried to obtain a radiation cooling coating with a self-cleaning function.
3. The method for preparing a radiation cooling coating with a self-cleaning function according to claim 1, characterized in that: The silane coupling agent is one of gamma-aminopropyl triethoxysilane, gamma-glycidyloxypropyl trimethoxysilane and gamma-methacryloxypropyl trimethoxysilane.
4. The method for preparing a radiation cooling coating with a self-cleaning function according to claim 1, characterized in that: The titanium source compound is one of butyl titanate, methyl titanate, ethyl titanate, titanium tetraisopropoxide and titanium tetrachloride or a mixed solution of any of them.
5. Application of a radiation cooling material prepared by the method for preparing a radiation cooling coating with a self-cleaning function according to any one of claims 1 to 4 in an application device, characterized in that: The application device is a solar cell, building glass, a greenhouse or a communication device.