A kind of aluminum oxide coated silicon carbon material and its preparation method and application

Preparation of aluminum oxide-covered silicon carbon materials through sol-gel method solves the problems of poor uniformity and dispersion in the coating process of silicon carbon materials, and improves the cycle stability and electrochemical performance in lithium-ion batteries. It is suitable for industrial production .

CN117613209BActive Publication Date: 2024-11-26SHENZHEN SOLID ADVANCED MATERIALS TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202311376166.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-23
Publication Date
2024-11-26
Estimated Expiration
2043-10-23

AI Technical Summary

Technical Problem

The prior art has problems of uniformity and poor particle dispersion in the coating process of silicon carbon materials in lithium-ion batteries, making it difficult to achieve large-scale industrial production. At the same time, nano-silicon materials are prone to oxidation and deterioration, affecting cycle stability.

Method used

The aluminum oxide-coated silicon carbon material was prepared by sol-gel method, and Al(OH)3 gel was generated by the reaction of aluminum nitrate and urea solution. It was converted into an Al2O3 coating layer after calcination, and the coating layer thickness was controlled at the nano-level to improve the Cycling performance and stability of silicon-carbon materials.

Benefits of technology

It improves the cyclic stability and electrochemical performance of silicon carbon materials in lithium-ion batteries, slows down volume expansion, improves the transmission efficiency and voltage stability of lithium ions, and is suitable for commercial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117613209B_ABST
    Figure CN117613209B_ABST
Patent Text Reader

Abstract

The present invention discloses an aluminum oxide coated silicon-carbon material and its preparation method and application. The preparation method includes: providing a silicon-carbon material, an aluminum nitrate solution and a urea solution; dispersing the silicon-carbon material in an organic solvent, performing ultrasonic treatment, and obtaining a first mixed solution; mixing the first mixed solution with the aluminum nitrate solution, stirring, and obtaining a second mixed solution; mixing the second mixed solution with the urea solution, stirring, and obtaining a precursor solution; subjecting the precursor solution to a water bath treatment, and obtaining a precursor gel; subjecting the precursor gel to a calcination treatment, and then cooling treatment, and obtaining the aluminum oxide coated carbon silicon material. The preparation method adopted by the present invention solves the problem of uncontrollable coating process, and under the coating protection of aluminum oxide, the volume expansion of the silicon-carbon material is improved, the voltage decay rate is slowed down, and the cycle stability is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to an aluminum oxide-coated silicon-carbon material and a preparation method and application thereof. Background Art

[0002] In the past 10 years, lithium-ion batteries have occupied a dominant position in the field of portable electronic devices. In recent years, they have also played an increasingly important role in the field of electric vehicles. At present, in the field of electric vehicles, the energy density of automotive batteries is increasing at a rate of 7% to 10% per year. Therefore, higher requirements are placed on the energy density of lithium-ion batteries and their industrialization. Graphite, as a commercial negative electrode material, has almost reached the limit of its theoretical specific capacity. The specific capacity it can provide is 150Wh / kg, which is not enough to meet the increasing demand for energy density. Silicon (Si) has a high theoretical weight capacity (4200mAh g -1 , while graphite is 372 mAh g -1 ), low operating voltage (about 0.28V, while graphite is about 0.18V) and high abundance (the second most abundant element on earth). However, Si has an intrinsic problem that the volume changes by up to 400% during the Li alloying-dealloying process. This poses a major challenge to the practical application of lithium-ion batteries. In addition, since the volume expansion caused by lithium insertion / de-lithiation during the silicon cycle can reduce the stability of the solid electrolyte interface (SEI) or even rupture it, it is extremely important to explore effective solutions to the problems existing in the current battery system in order to promote the further development of silicon-carbon negative electrode lithium-ion batteries.

[0003] Some researchers have used small-particle nano-silicon materials to compound with graphite and carbon to reduce the distance of lithium ion transmission and inhibit the breakage caused by volume expansion during the silicon cycle. However, in actual production, the active material silicon is very easy to oxidize and deteriorate when using nano-silicon as raw material, making it difficult to ensure product yield, and the improvement of the long-cycle stability of silicon-carbon materials is not obvious. Some researchers have also used surface coating and other means to prevent direct contact between the negative electrode material and the organic electrolyte, and to form a stable interfacial electrolyte layer by reducing harmful side reactions to improve the cycle stability of silicon-carbon materials. At the same time, the coating layer structure can also inhibit the volume expansion generated during the cycle of the silicon-carbon negative electrode. Among them, the use of alumina coating has been proven to be an effective coating technology. However, there are many problems in coating and modifying nanostructured silicon-carbon materials, such as the difficulty in controlling the uniformity of the coating during the coating process and the difficulties faced by the poor dispersion of particles, making it difficult to carry out large-scale industrial production.

[0004] Therefore, the prior art still needs to be improved and developed. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the present invention provides an alumina-coated silicon-carbon material and a preparation method and application thereof to solve the problems of poor coating uniformity and particle dispersion in the existing coating process for silicon-carbon materials.

[0006] In experimental research, atomic layer deposition (ALD) is used to prepare alumina-coated carbon silicon materials. Atomic layer deposition equipment is required, and aluminum-containing organic matter (such as trimethylaluminum) is used as a precursor. It is entrained by a protective gas (such as nitrogen) and enters a customized reaction chamber for deposition. However, due to the environmental pollution and flammability of the precursor substances used in the deposition process, and the high cost of equipment and raw materials, it is hindered in large-scale production.

[0007] Based on this, the technical solution adopted by the present invention is as follows:

[0008] A first aspect of the present invention provides a method for preparing an aluminum oxide-coated silicon-carbon material, comprising the steps of:

[0009] Provide silicon-carbon materials, aluminum nitrate solution and urea solution;

[0010] Dispersing the silicon-carbon material in an organic solvent and performing ultrasonic treatment to obtain a first mixed solution;

[0011] Mixing the first mixed solution with the aluminum nitrate solution and stirring to obtain a second mixed solution;

[0012] Mixing the second mixed liquid with the urea solution and stirring to obtain a precursor solution;

[0013] treating the precursor solution in a water bath to obtain a precursor gel;

[0014] The precursor gel is calcined and then cooled to obtain the alumina-coated carbon silicon material.

[0015] Specifically, the urea in the present invention undergoes the following reactions in aqueous solution: CO(NH2)2+H2O→NH2COONH4, NH2COONH4+H2O→(NH4)2CO3; and aluminum nitrate is completely ionized into Al 3+ , adding urea to aluminum nitrate solution will increase the pH of the mixed solution. 3+ With OH -The ions combine to form a gel-like Al(OH)3, which will be coated on the surface of the silicon-carbon material due to the strong adsorption of the gel. Water bath heating can promote the above reaction, make the reaction more complete, and can concentrate the mixed solution. During the high-temperature calcination process, Al(OH)3 is converted into the final product Al2O3 to obtain a silicon-carbon material coated with aluminum oxide. Thanks to this special structure, the surface-coated aluminum oxide can inhibit the volume expansion of the silicon-carbon material during the cycle, which can improve the cycle performance of the silicon-carbon material. In addition, under the protection of aluminum oxide, the silicon-carbon material can be isolated from the electrolyte to reduce side reactions to stabilize the surface interface layer. Specifically, the aluminum oxide on the surface will be transformed into a fast ion conductor during the battery cycle, allowing lithium ions to maintain a high pass rate. Its room temperature ion conductivity is as high as 1.36*10~(-5)S / cm, thereby promoting the migration of lithium ions between the silicon-carbon material and the electrolyte. Under the protective effect of aluminum oxide coating, the volume expansion of the silicon-carbon material is improved, the voltage decay rate is slowed down, and the cycle stability is greatly improved.

[0016] Moreover, compared with the atomic layer deposition (ALD) method, the experimental equipment used in the method of the present invention is less expensive, does not require expensive experimental equipment assistance, and can better meet the needs of commercial applications. The raw materials such as aluminum nitrate used in the initial stage of the sol-gel synthesis process in the method of the present invention have good dispersibility in the solvent and can form a uniformly distributed solution in a short time. Therefore, it is easier to form a uniform and stable gel at the molecular level when forming a gel. During the process, as the solution is concentrated, the concentration of the solute continues to rise, and the gel can be more uniformly adsorbed on the surface of the silicon-carbon material. Further, compared with the direct chemical reaction to generate the Al2O3 coating layer, in this method, the metal compound is solidified through the solution and gel, and then calcined to generate nanoparticles. Thanks to the uniformity and adsorption of the gel, the coating thickness can be controlled at the nanometer level. The nanometer-level coating will not affect the transmission of electrons and lithium ions in the battery, thereby achieving better electrochemical performance. Compared with other synthetic processes, this method avoids the uncontrollable influencing factors caused by too many production processes, and the product prepared by the sol-gel method makes the coating layer more uniform due to the good adhesion of the gel.

[0017] Preferably, in the water bath treatment of the precursor solution, the water bath temperature is 60 to 80° C., and the water bath time is 1 to 5 hours.

[0018] Preferably, in the calcination treatment of the precursor gel, the calcination temperature is 500-800° C. and the calcination time is 3-5 hours.

[0019] Preferably, the temperature is increased to 500-800° C. at a heating rate of 2-15° C. / min.

[0020] Preferably, the aluminum nitrate solution consists of aluminum nitrate and water, and the mass ratio of the aluminum nitrate to water is (100-800):100000.

[0021] Preferably, in the second mixed liquid, the mass ratio of the carbon silicon material to the aluminum nitrate solution is 1:(30-100).

[0022] Specifically, the present invention explores the optimal coating content range of aluminum oxide on silicon-carbon materials, and because the coating thickness of the aluminum oxide coating material affects the transmission of lithium ions to the negative electrode, thereby reducing the rate performance of the silicon-carbon material, under the mass ratio of the present invention, a better coating content and coating thickness can be obtained, thereby improving the rate performance of the silicon-carbon material.

[0023] Preferably, in the precursor solution, the mass ratio of aluminum nitrate to urea is 10:1 to 1:5.

[0024] Preferably, the mixing of the second mixed liquid and the urea solution specifically comprises: adding the urea solution dropwise into the second mixed liquid at a dropping rate of 1 to 4 ml / min.

[0025] Specifically, the present application controls the dripping rate to ensure that the pH value in the solution environment does not undergo regional mutations to cause uneven local coating layers, and controls the dripping rate to ensure that the coating process reacts completely.

[0026] The third aspect of the present application provides an alumina-coated silicon-carbon material prepared by the above-mentioned preparation method.

[0027] The fourth aspect of the present application provides an application of an aluminum oxide-coated silicon-carbon material in the preparation of a negative electrode for a lithium-ion battery.

[0028] Beneficial effects:

[0029] The present invention discloses an aluminum oxide-coated silicon-carbon material and a preparation method and application thereof. The present invention selects to compound aluminum oxide formed by aluminum nitrate with a silicon-carbon material to obtain an aluminum oxide-coated silicon-carbon material structure. Thanks to this special structure, the aluminum oxide coated on the surface can inhibit the volume expansion of the silicon-carbon material during the cycle, and can improve the cycle performance of the silicon-carbon material. In addition, under the protection of aluminum oxide, the silicon-carbon material can be isolated from the electrolyte to reduce side reactions to stabilize the surface interface layer. Specifically, the aluminum oxide on the surface will be transformed into a fast ion conductor during the battery cycle, so that lithium ions can maintain a high pass rate, thereby promoting the migration of lithium ions between the silicon-carbon material and the electrolyte. Under the protective effect of the aluminum oxide coating, the volume expansion of the silicon-carbon material is improved, the voltage decay rate is slowed down, and the cycle stability is greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 A flow chart of preparing alumina-coated silicon-carbon material according to the present invention;

[0031] Figure 2 The first cycle charge and discharge curves of Pristine Si-C, Si-C@A-0.5, Si-C@A-1, and Si-C@A-3 at a current density of 100 mA / g in the embodiments of the present invention and the comparative examples;

[0032] Figure 3 The performance curves of Pristine Si-C, Si-C@A-0.5, Si-C@A-1, and Si-C@A-3 in the embodiments of the present invention and the comparative examples after 200 charge-discharge cycle tests at a current density of 500 mA / g;

[0033] Figure 4 The rate performance test results of Pristine Si-C, Si-C@A-0.5, Si-C@A-1 and Si-C@A-3 in the embodiments of the present invention and the comparative examples in the voltage range of 0.005-1.5V and the current density of 100, 200, 300, 500, 800, 1000, 1500 and 2000 mA / g;

[0034] Figure 5 The figure shows the expansion test results of the pole piece cross section before and after coating of the present invention. DETAILED DESCRIPTION

[0035] The present invention provides an aluminum oxide coated silicon carbon material and a preparation method and application thereof. To make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0036] The present invention provides a method for preparing an alumina-coated silicon-carbon material, comprising the steps of:

[0037] Provide silicon-carbon materials, aluminum nitrate solution and urea solution;

[0038] Dispersing the silicon-carbon material in an organic solvent and performing ultrasonic treatment to obtain a first mixed solution;

[0039] Mixing the first mixed solution with the aluminum nitrate solution and stirring to obtain a second mixed solution;

[0040] Mixing the second mixed liquid with the urea solution and stirring to obtain a precursor solution;

[0041] treating the precursor solution in a water bath to obtain a precursor gel;

[0042] The precursor gel is calcined and then cooled to obtain the alumina-coated carbon silicon material.

[0043] In some embodiments, when the precursor solution is subjected to water bath treatment, the water bath temperature is 60-80° C., and the water bath time is 1-5 hours. For example, the water bath temperature can be 60° C., 70° C., 80° C., and the water bath time is 1 hour, 2 hours, 3 hours, 4 hours, or 5 hours.

[0044] In some preferred embodiments, in the water bath treatment of the precursor solution, the water bath temperature is 65° C. and the water bath time is 5 hours.

[0045] In some embodiments, the precursor gel is calcined at a temperature of 500-800°C and a calcination time of 3-5 hours. For example, the calcination temperature is 500°C, 600°C, 700°C, 800°C, and the calcination time is 3 hours, 4 hours, or 5 hours.

[0046] In some preferred embodiments, in the calcination treatment of the precursor gel, the calcination temperature is 600° C. and the calcination time is 4 hours.

[0047] In some embodiments, the temperature is increased to 500-800° C. at a heating rate of 2-10° C. / min.

[0048] In some preferred embodiments, the temperature is increased to 500-800° C. at a heating rate of 5° C. / min.

[0049] In some embodiments, the aluminum nitrate solution is composed of aluminum nitrate and water, and the mass ratio of aluminum nitrate to water is (100-800): 100000. For example, the mass ratio of aluminum nitrate to water can be 100:100000, 200:100000, 300:100000, 400:100000, 500:100000, 600:100000, 700:100000, 800:100000.

[0050] In some preferred embodiments, the aluminum nitrate solution consists of aluminum nitrate and water, and the mass ratio of aluminum nitrate to water is 1:670.

[0051] In some embodiments, in the second mixed solution, the mass ratio of the carbon silicon material to the aluminum nitrate solution is 1:(30-100).

[0052] In some preferred embodiments, in the second mixed solution, the mass ratio of the carbon silicon material to the aluminum nitrate solution is 1:50.

[0053] In some embodiments, in the precursor solution, the mass ratio of aluminum nitrate to urea is 10:1 to 1:5.

[0054] In some preferred embodiments, in the precursor solution, the mass ratio of aluminum nitrate to urea is 7:1.

[0055] In some embodiments, the mixing of the second mixed liquid and the urea solution specifically includes: adding the urea solution dropwise to the second mixed liquid at a dropping rate of 1 to 4 ml / min.

[0056] In some preferred embodiments, the mixing of the second mixed liquid and the urea solution specifically includes: dropping the urea solution into the second mixed liquid at a dropping rate of 3 ml / min.

[0057] In some embodiments, an aluminum oxide-coated silicon-carbon material is prepared by the above-mentioned preparation method.

[0058] In some embodiments, the above-mentioned alumina-coated silicon-carbon material is used in preparing a negative electrode of a lithium-ion battery.

[0059] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments, and are only used to illustrate the present invention but not to limit the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0060] Example 1

[0061] A method for preparing an alumina-coated silicon-carbon material comprises the following steps:

[0062] S1. Disperse the silicon-carbon material Si-C950 in anhydrous ethanol and perform ultrasonic treatment on it at room temperature to make the silicon-carbon composite material Si-C950 evenly dispersed in the anhydrous ethanol, dissolve aluminum nitrate nonahydrate in deionized water at a mass ratio of 75.74:100000 to obtain an aluminum nitrate solution, and dissolve urea in deionized water at a mass ratio of 11.78:100000 to obtain a urea solution.

[0063] S2. The dispersed carbon-silicon composite material Si-C950 and the aluminum nitrate solution were mixed in a mass ratio of 1:50, stirred for 30 minutes, and then placed in a 65° C. water bath environment and continued to stir to obtain a mixed solution.

[0064] S3. Add the urea solution dropwise to the mixed solution of S2 at a mass ratio of 1:1 to obtain a precursor solution, wherein the dropping rate is controlled to be completed within 30 minutes.

[0065] S4. Place the precursor solution in a water bath at 65°C until only a gel-like substance remains in the solution, collect the gel-like substance to obtain a precursor gel; crush the precursor gel and move it to a tubular furnace, pass Ar (99.9%) gas into the reaction chamber at a rate of 100 ml / min in the tubular furnace, heat the tubular furnace to 600°C at a heating rate of 5°C / min and keep warm for 4 hours, then naturally cool to room temperature, collect the gray powder, and obtain the alumina-coated carbon silicon material Si-C@A-0.5.

[0066] Example 2

[0067] A method for preparing an alumina-coated silicon-carbon material. The method of this embodiment is basically the same as that of Example 1, except that: in S1, the mass ratio of aluminum nitrate nonahydrate to deionized water in the aluminum nitrate solution is 151.09:100000, and the mass ratio of urea to deionized water in the urea solution is 23.56:100000, thereby obtaining an alumina-coated carbon silicon material Si-C@A-1.

[0068] Example 3

[0069] A method for preparing an alumina-coated silicon-carbon material. The method of this embodiment is basically the same as that of Example 1, except that: in S1, the mass ratio of aluminum nitrate nonahydrate to deionized water in the aluminum nitrate solution is 453.27:100000, and the mass ratio of urea to deionized water in the urea solution is 70.69:100000, thereby obtaining an alumina-coated carbon silicon material Si-C@A-3.

[0070] Comparative Example 1

[0071] The carbon-silicon composite material is not coated with aluminum oxide to obtain the carbon-silicon material Pristine Si-C.

[0072] Performance testing

[0073] Experiment 1: Capacity retention rate test

[0074] The first cycle charge and discharge test of the materials prepared in Examples 1-3 and Comparative Example 1 at a current density of 100mA / g is shown in Table 1 below. The first cycle charge capacity of Si-C is 949.6mAh / g, and the first cycle coulomb efficiency is 77.86%; the first cycle charge specific capacity and first cycle coulomb efficiency of Si-C@A-0.5, Si-C@A-1, and Si-C@A-3 are 1040.14mAh / g, 994.05mAh / g, 868.7mAh / g, and 80.14%, 78.82%, and 78.59%, respectively. Figure 2 The first cycle charge and discharge results show that the first cycle charge specific capacity and first cycle coulomb efficiency of Si-C@A-0.5 and Si-C@A-1 are higher than those of Pristine Si-C, while when the coating content increases to 3%, the performance decreases compared with Comparative Example 1.

[0075] Pristine Si-C Si-C@A-0.5 Si-C@A-1 Si-C@A-3 First effect (%) 77.86 80.14 78.82 78.59 Capacity (mAh / g) 949.6 1040.14 994.05 868.7

[0076] Table 1

[0077] Figure 3 The performance curves of Pristine Si-C, Si-C@A-0.5, Si-C@A-1, and Si-C@A-3 after 200 charge and discharge cycle tests at a current density of 500 mA / g, wherein each battery was previously charged and discharged three times at a current density of 100 mA / g to activate the negative electrode material. The results in Table 2 below show that after 200 cycles, the discharge specific capacities of Pristine Si-C, Si-C@A-0.5, Si-C@A-1, and Si-C@A-3 are 616.7 mAh / g, 642.8 mAh / g, 780.3 mAh / g, and 683.9 mAh / g, respectively, and the corresponding capacity retention rates are 62.04%, 57.38%, 69.35%, and 68.42%, respectively. Among them, Si-C@A-1 and Si-C@A-3 have higher capacity retention rates, and Si-C@A-1 exhibits the best cycle stability. The improvement in the cycle stability of the alumina-coated silicon-carbon negative electrode is attributed to the fact that alumina promotes the transfer of lithium ions to the silicon-carbon negative electrode during the cycle and assists in the formation of a stable solid electrolyte interphase.

[0078]

[0079]

[0080] Table 2

[0081] Experimental 2x performance test

[0082] Figure 4The rate performance test results of Pristine Si-C, Si-C@A-0.5, Si-C@A-1 and Si-C@A-3 in the voltage range of 0.005-1.5V and at current densities of 100, 200, 300, 500, 800, 1000, 1500 and 2000mA / g are shown in Figure 1. The discharge capacities of Si-C are 1000.5, 989.3, 962.5, 910.9, 846.7, 764.6, 713.6 and 618.9mAh / g respectively; the discharge capacities of Si-C@A-0.5 are 1034.2, 1015.5, 986.6, 931.3, 891.3, 870.7, 825.5 and 797.4mAh / g respectively. g; the corresponding discharge capacities of Si-C@A-1 are 1041.8, 1024.8, 1005.3, 975.2, 950.7, 928, 896.7, 864.1 mAh / g; the corresponding discharge capacities of Si-C@A-3 are 991.9, 954.1, 913.1, 855.5, 800.8, 756.5, 733.6, 703.8 mAh / g. The three alumina-coated silicon-carbon materials have higher discharge specific capacities than Si-C at high current density, and Si-C@A-1 has the best comprehensive rate performance, which proves that the silicon-carbon material has a higher lithium ion conductivity after alumina coating. The higher ion conductivity of the coated material is attributed to the uniformly distributed fast ion conductor alumina. The alumina distributed on the surface of the negative electrode particles provides a large number of fast ion transmission channels for the lithium ions inside the particles, so the transmission rate of lithium ions can be greatly improved.

[0083] Experiment 3: Pole expansion test

[0084] Figure 5 The results of the expansion test of the electrode section before and after coating. Among them, the electrode section thickness of the material before coating is 12.4 microns, the thickness after 5 cycles is 25.6 microns, and the electrode expansion rate is 106.4%; the electrode section thickness of the material after coating is 12.2 microns, the thickness after 5 cycles is 14.2 microns, and the electrode expansion rate is 16.4%. The expansion of the silicon-carbon negative electrode electrode after coating with alumina shows obvious relief, proving that the mechanical properties after coating with alumina can effectively inhibit the expansion of the electrode caused by the volume expansion of silicon during the cycle, making the silicon-carbon negative electrode material electrode more stable, which also corresponds well to the improvement of electrochemical performance.

[0085] In summary, an alumina-coated silicon-carbon material and its preparation method and application, the present invention selects to compound alumina formed by aluminum nitrate with a silicon-carbon material to obtain an alumina-coated silicon-carbon material structure. Thanks to this special structure, the surface-coated alumina can inhibit the volume expansion of the silicon-carbon material during the cycle, and can improve the cycle performance of the silicon-carbon material. In addition, under the protection of alumina, the silicon-carbon material can be isolated from the electrolyte to reduce side reactions to stabilize the surface interface layer. Specifically, the surface alumina will be transformed into a fast ion conductor during the battery cycle, so that lithium ions can maintain a high pass rate, thereby promoting the migration of lithium ions between the silicon-carbon material and the electrolyte. Under the protective effect of the coating of alumina, the volume expansion of the silicon-carbon material is improved, the voltage decay rate is slowed down, and the cycle stability is greatly improved.

[0086] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.

Claims

1. A method for preparing an alumina-coated silicon-carbon material, characterized in that: Includes steps: S1. Dispersing the silicon-carbon material Si-C950 in anhydrous ethanol and subjecting it to ultrasonic treatment at room temperature to uniformly disperse the silicon-carbon composite material Si-C950 in the anhydrous ethanol, dissolving aluminum nitrate nonahydrate in deionized water at a mass ratio of 151.09:100000 to obtain an aluminum nitrate solution, and dissolving urea in deionized water at a mass ratio of 23.56:100000 to obtain a urea solution; S2, mixing the dispersed carbon-silicon composite material Si-C950 with the aluminum nitrate solution in a mass ratio of 1:50, stirring for 30 minutes, and then placing it in a 65° C. water bath environment and continuing to stir to obtain a mixed solution; S3, adding the urea solution dropwise to the mixed solution of S2 at a mass ratio of 1:1 to obtain a precursor solution, wherein the dropping rate is controlled to be completed within 30 minutes; S4. Place the precursor solution in a water bath at 65°C until only a gel-like substance remains in the solution, collect the gel-like substance to obtain a precursor gel; crush the precursor gel and move it to a tubular furnace, pass 99.9% Ar gas into the reaction chamber at a rate of 100 ml / min, heat the tubular furnace to 600°C at a heating rate of 5°C / min and keep warm for 4 hours, then naturally cool to room temperature, collect the gray powder, and obtain an alumina-coated carbon silicon material.

2. An alumina-coated silicon-carbon material prepared by the preparation method described in claim 1.

3. Use of the alumina-coated silicon-carbon material according to claim 2 in preparing a negative electrode for a lithium-ion battery.

Citation Information

Cited By

  • Preparation method of composite silicon-carbon negative electrode material

    CN121849968A