A composite hydrogel loaded with nano-antibacterial materials, its preparation method and application

By preparing chitosan/sodium alginate composite hydrogels loaded with silver nanoparticles, and combining AgNPs and active components of traditional Chinese medicine, the antibacterial and mechanical properties of the hydrogels were improved, solving the problems of limited functionality and stability of existing dressings, and making them suitable for the field of biomedical materials.

CN117618638BActive Publication Date: 2026-11-17CHONGQING UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311612038.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-29
Publication Date
2026-11-17
Estimated Expiration
2043-11-29

AI Technical Summary

Technical Problem

Existing wound dressings have relatively limited functions and poor mechanical properties, making it difficult to meet the multi-stage needs of skin wound healing. Furthermore, they are difficult to fix when used on active areas, which can easily lead to prolonged healing time and bacterial infection.

Method used

By mixing chitosan with sodium alginate to form a composite hydrogel membrane, and then crosslinking it in a calcium salt solution, the membrane is soaked in a solution of active components of traditional Chinese medicine containing silver salts and polyphenol groups to prepare a composite hydrogel loaded with silver nanoparticles. The synergistic antibacterial ability of AgNPs and active components of traditional Chinese medicine is utilized to improve antibacterial and mechanical properties.

Benefits of technology

The prepared composite hydrogel loaded with nano-antibacterial materials has excellent broad-spectrum antibacterial properties and mechanical properties, which solves the problems of single function and stability of existing dressings and is suitable for the field of biomedical materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117618638B_ABST
    Figure CN117618638B_ABST
Patent Text Reader

Abstract

This invention relates to a composite hydrogel loaded with nano-antibacterial materials, its preparation method, and its application. The preparation method of the composite hydrogel loaded with nano-antibacterial materials includes the following steps: mixing chitosan with sodium alginate to obtain a hydrogel membrane; immersing the hydrogel membrane in a calcium salt solution to obtain a calcium-crosslinked hydrogel membrane; immersing the calcium-crosslinked hydrogel membrane once in a silver salt solution, and then immersing it a second time in a solution of active components of traditional Chinese medicine rich in polyphenol groups to obtain the composite hydrogel. This invention also provides a composite hydrogel loaded with nano-antibacterial materials prepared by the method described herein. Furthermore, this invention provides an application of the composite hydrogel loaded with nano-antibacterial materials prepared by the method described herein, specifically its application in the preparation of antibacterial dressings. This invention solves the problems of relatively limited functionality and poor mechanical properties in existing wound dressings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of biomedical materials technology, specifically to a composite hydrogel loaded with nano-antibacterial materials, its preparation method, and its application. Background Technology

[0002] As the body's first line of defense, the skin effectively blocks various external threats. However, millions of skin injuries require treatment each year due to accidental trauma or surgery. Therefore, wound dressings have become an important branch of biomedical materials research. Wound dressings are crucial materials for repairing damaged skin and restoring its function. Hydrogels, due to their superior biocompatibility, controllable physical properties, and multifunctionality, are gradually becoming common medical wound dressings. Hydrogel wound dressings have been successfully used to treat various tissue injuries, such as skin defects, infected wounds, diabetic ulcers, and burn wounds.

[0003] Chitosan (CS), derived from deacetylated chitin, is a natural polysaccharide biomass rich in amino and hydroxyl functional groups. It possesses excellent biocompatibility, biodegradability, hemostatic properties, mucosal adsorption, non-toxicity, and antibacterial properties. Therefore, chitosan hydrogels exhibit good hydrophilicity, a unique three-dimensional network structure, and good biocompatibility. While chitosan hydrogels can be used as wound dressings to protect wound surfaces from bacterial infection, they often require combination with other bactericides to achieve better antibacterial effects. The most common strategy is to incorporate antibiotics into the chitosan hydrogel; however, the overuse of antibiotics can lead to the emergence of drug-resistant bacteria. Chitosan composite hydrogels loaded with nano-antibacterial materials exhibit excellent antibacterial properties and show promising application prospects in treating infected wounds. Wound healing involves a complex process, generally requiring four stages: hemostasis, inflammation, proliferation, and tissue remodeling. Wound dressings need to simultaneously possess antioxidant, anti-inflammatory, antibacterial, and hemostatic functions; however, existing wound dressings have relatively limited functionality, failing to meet the needs of skin wound healing. Furthermore, the frequent movement and unevenness of active wound sites make it difficult to fix wound dressings properly and result in incomplete coverage, leading to prolonged wound healing time and bacterial infection. Therefore, it is essential to develop a wound dressing loaded with nano-antibacterial materials that is multifunctional, has good mechanical properties, excellent antibacterial properties, and can prevent the growth of drug-resistant bacteria. Summary of the Invention

[0004] This invention provides a composite hydrogel loaded with nano-antibacterial materials, its preparation method, and its application, in order to solve the problems of relatively simple functions and poor mechanical properties of existing wound dressings.

[0005] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0006] A method for preparing a composite hydrogel loaded with nano-antibacterial materials includes the following steps:

[0007] S1. Chitosan and sodium alginate are mixed to prepare a chitosan / sodium alginate composite hydrogel membrane;

[0008] S2. The hydrogel membrane prepared in S1 is immersed in a calcium salt solution to obtain a calcium-crosslinked chitosan / sodium alginate hydrogel membrane.

[0009] S3. The calcium-crosslinked chitosan / sodium alginate hydrogel membrane prepared in S2 is immersed in a silver salt solution once, and then immersed in a solution of traditional Chinese medicine active ingredients containing polyphenol groups a second time to obtain a composite hydrogel loaded with nano-antibacterial materials.

[0010] Based on the above technical methods, a chitosan / sodium alginate composite hydrogel membrane was prepared by mixing water-soluble chitosan and sodium alginate. Then, the chitosan / sodium alginate composite hydrogel membrane was immersed in a calcium salt solution to form a calcium-crosslinked chitosan / sodium alginate hydrogel membrane. Subsequently, the calcium-crosslinked chitosan / sodium alginate hydrogel membrane was thoroughly immersed in a silver salt solution and a solution of traditional Chinese medicine active ingredients rich in polyphenol groups. Ag... + In situ reduction to AgNPs. Simultaneously, the polyphenol-containing active components of traditional Chinese medicine can coordinate with metal ions to form complexes. Relying on hydrogen bonds and electrostatic interactions within the hydrogel's internal network, the resulting composite hydrogel membrane exhibits excellent mechanical and swelling properties. Due to the synergistic antibacterial ability of AgNPs and the active components of traditional Chinese medicine, the prepared composite hydrogel loaded with nano-antibacterial materials possesses good broad-spectrum antibacterial properties, effectively solving the problems of poor anti-infection efficacy and unstable mechanical properties in existing wound dressings.

[0011] Among these findings, research revealed that when immersed in a solution of active components of traditional Chinese medicine containing polyphenol groups, the components not only coordinate with metal ions to form complexes, but also exhibit hydrogen bonding and electrostatic interactions, effectively improving the mechanical strength of the hydrogel membrane; the phenolic hydroxyl groups participate in redox reactions and donate electrons, Ag... + It accepts electrons to transform into Ag atoms and grows to form AgNPs.

[0012] Preferably, in S1, the chitosan is water-soluble chitosan.

[0013] Preferably, in S2, the calcium salt is selected from calcium chloride.

[0014] Preferably, in S3, the silver salt is silver nitrate.

[0015] Preferably, the method for preparing the water-soluble chitosan is as follows: dissolve chitosan in acetic acid solution, then add hydroxyethyl acrylate, and continuously stir at 50℃~70℃ to obtain a reaction solution; adjust the pH of the reaction solution to neutral, add acetone, and dry to obtain water-soluble chitosan.

[0016] Research has shown that chitosan has low solubility and is difficult to mix evenly with sodium alginate. Therefore, hydroxyethyl acrylate was first used to modify chitosan into water-soluble chitosan, thereby ensuring the uniform mixing of water-soluble chitosan and sodium alginate and improving the stability of the composite hydrogel.

[0017] Preferably, the method for preparing the water-soluble chitosan specifically includes: adding 3g of chitosan to 300mL of 1% w / v acetic acid solution to obtain a chitosan solution with a concentration of 1% w / v; then adding 12g of hydroxyethyl acrylate to the 1% w / v chitosan solution and stirring continuously for 48h in a water bath at 60°C to obtain a reaction solution; adjusting the pH of the reaction solution to 7 with a 10% w / v sodium hydroxide solution; then adding the pH-adjusted reaction solution dropwise into acetone to precipitate water-soluble chitosan; drying the precipitated water-soluble chitosan at 60°C, collecting the water-soluble chitosan, and grinding it into powder to obtain water-soluble chitosan.

[0018] Preferably, step S1 specifically includes: mixing and stirring chitosan aqueous solution with sodium alginate until sodium alginate is completely dissolved, allowing it to stand, and drying it to obtain a chitosan / sodium alginate composite hydrogel membrane.

[0019] Preferably, the mass concentration of the chitosan aqueous solution is 1-5%.

[0020] Preferably, the chitosan aqueous solution contains 1% chitosan by mass.

[0021] Preferably, the mass ratio of the chitosan aqueous solution to sodium alginate is 1:3 to 1:5.

[0022] Preferably, the mass ratio of the chitosan aqueous solution to sodium alginate is 1:3.

[0023] Preferably, step S1 specifically includes: dissolving water-soluble chitosan in water to obtain a water-soluble chitosan aqueous solution, mixing and stirring it with sodium alginate overnight until the sodium alginate is completely dissolved, then letting it stand for more than 12 hours to defoam, and then drying it at 40°C for 12 hours to obtain a chitosan-sodium alginate hydrogel film.

[0024] Preferably, step S1 specifically includes: dissolving 1g of water-soluble chitosan in distilled water and continuously stirring at 70°C to obtain an HCS solution with a concentration of 1% w / v; mixing the obtained HCS solution with sodium alginate (SA) at a mass ratio of 1:3 to obtain a mixed solution, and continuously stirring the mixed solution overnight until the sodium alginate (SA) is completely dissolved, then letting it stand for 12h to defoam, transferring it to a glass culture dish, and then drying it at 40°C for 12h to obtain an HCS / SA hydrogel membrane.

[0025] Preferably, in step S2, the concentration of calcium salt in the calcium salt solution is 0.25M to 0.5M.

[0026] Preferably, in step S2, the concentration of calcium salt in the calcium salt solution is 0.25M.

[0027] Preferably, the soaking time in the calcium salt solution is 30 min to 2 h.

[0028] Preferably, the soaking time in the calcium salt solution is 30 minutes.

[0029] Preferably, step S2 specifically includes: immersing the HCS / SA hydrogel membrane in a CaCl2 solution (0.25M) for 30 minutes, then washing it several times with distilled water, and finally drying it in an oven at 40°C to obtain a calcium-crosslinked water-soluble chitosan / sodium alginate (HCS / SA-Ca) hydrogel membrane.

[0030] Preferably, in step S3, the concentration of silver salt in the silver salt solution is 0.5–10 mM.

[0031] Preferably, in step S3, the concentration of tannic acid in the tannic acid solution is 0.05M.

[0032] Preferably, in step S3, the solution of active components of traditional Chinese medicine contains 2 to 100 ortho-diphenol hydroxyl groups.

[0033] Preferably, in step S3, the solution of active components of traditional Chinese medicine is selected from at least one of tannic acid solution, curcumin solution and chlorogenic acid solution.

[0034] The active components of the traditional Chinese medicine (TCM) in the solution include, but are not limited to, at least one of tannic acid, curcumin, and chlorogenic acid. Because these active components are rich in o-dihydroxyl groups, they can not only coordinate with metal ions to form complexes, but also exhibit hydrogen bonding and electrostatic interactions, effectively improving the mechanical strength of the hydrogel membrane. The o-dihydroxyl groups participate in redox reactions and donate electrons, Ag... + It accepts electrons to transform into Ag atoms and grows to form AgNPs.

[0035] Preferably, the pH value of the solution of the active components of the traditional Chinese medicine is between 6 and 10.

[0036] Studies have found that solutions of active components of traditional Chinese medicine (TCM) at different pH values ​​can form different forms of TCM active component-Ca complexes, namely mono-component complexes, binary complexes, and ternary complexes. This is because as the pH value increases, the phenolic hydroxyl groups undergo deprotonation, allowing more TCM active components to combine with Ca. 2+ Coordination bonds are formed. Specifically, for example, tannic acid (TA) solutions at different pH values ​​can form different forms of TA-Ca complexes, namely monobasic, binary, and ternary complexes. As the pH value increases, the phenolic hydroxyl groups are deprotonated, allowing more TA to form with Ca. 2+ Coordinate bonds are formed.

[0037] Preferably, step S3 specifically includes: completely immersing the calcium-crosslinked water-soluble chitosan / sodium alginate hydrogel membrane in an AgNO3 solution for 24–48 hours, then immersing it in a 0.05M tannic acid solution for 2–4 hours, and adjusting the pH of the tannic acid solution to 6–10 so that the AgNO3 membrane can be fully immersed in the solution. + It is reduced in situ to silver nanoparticles (AgNPs) on the hydrogel membrane.

[0038] The present invention also provides a composite hydrogel loaded with nano-antibacterial materials prepared by the preparation method described in the present invention.

[0039] The present invention also provides an application of the composite hydrogel loaded with nano-antibacterial materials prepared by the preparation method described in the present invention, wherein the composite hydrogel loaded with nano-antibacterial materials is used in the preparation of antibacterial dressings.

[0040] The beneficial effects of this invention are:

[0041] The preparation method of the composite hydrogel loaded with nano-antibacterial materials of the present invention firstly prepares a chitosan / sodium alginate composite hydrogel membrane by mixing water-soluble chitosan and sodium alginate; then, the chitosan / sodium alginate composite hydrogel membrane is immersed in a calcium salt solution to form a calcium-crosslinked chitosan / sodium alginate hydrogel membrane, and then it is sequentially and thoroughly immersed in a silver salt solution and a solution of traditional Chinese medicine active ingredients containing polyphenol groups, so that the traditional Chinese medicine active ingredients containing polyphenol groups can transfer Ag +In situ reduction to AgNPs, the active components of traditional Chinese medicine containing polyphenol groups can coordinate with metal ions to form polyphenol-containing active components-metal complexes. They can also form hydrogen bonds and electrostatic interactions with various polymers, resulting in composite hydrogel films with excellent mechanical and swelling properties. Furthermore, antibacterial activity tests show good broad-spectrum antibacterial properties, solving the problems of relatively single function and poor mechanical properties of existing wound dressings. This has potential application value in the field of biomedical materials technology. Attached Figure Description

[0042] Figure 1 The images are FTIR spectra, where (A) are FTIR spectra of chitosan (CS), sodium alginate (SA), and water-soluble chitosan (HCS); and (B) are FTIR spectra of TA, HCS / SA membrane, HCS / SA-Ca membrane, and TA-HCS / SA-Ca / Ag membrane.

[0043] Figure 2 X-ray diffraction patterns of HCS / SA-Ca membrane and TA-HCS / SA-Ca / Ag membrane;

[0044] Figure 3 The images are electron microscope images and spectra. (A) is a scanning electron microscope image of HCS / SA and TA8-HCS / SA-Ca / Ag0.5 hydrogel membranes; (B) is an EDS surface scan spectrum of TA8-HCS / SA-Ca / Ag0.5 hydrogel membrane.

[0045] Figure 4 The graph shows the results of the stability and swelling of the hydrogel membrane. (A) represents the gel content (distilled water, 37℃); (B) represents the equilibrium swelling degree (distilled water, 37℃); and (C) represents the maximum swelling ratio of the hydrogel membrane (PBS, pH 7.4, 37℃).

[0046] Figure 5 The graph shows the mechanical properties of the hydrogel membrane, where (A) represents compressive strength (kPa); (B) represents elongation at break (%); and (C) represents Young's modulus (kPa). The letter "ad" indicates a significant difference (p<0.05).

[0047] Figure 6 Comparison of hemolysis rate test results for HCS / SA-Ca and TA-HCS / SA-Ca / Ag0.5 hydrogel membranes;

[0048] Figure 7 Antibacterial effects of silver-loaded hydrogel membranes prepared by immersion in AgNO3 solutions of different concentrations on S. aureus, E. coli and P. aeruginosa. Detailed Implementation

[0049] The embodiments of the present invention will be described below with reference to the accompanying drawings and preferred embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and various details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention. It should be understood that the preferred embodiments are only for illustrating the present invention and not for limiting the scope of protection of the present invention.

[0050] Example 1

[0051] A method for preparing a composite hydrogel loaded with nano-antibacterial materials includes the following steps:

[0052] S1. Chitosan and sodium alginate are mixed to prepare a chitosan / sodium alginate composite hydrogel membrane, specifically including:

[0053] S11. The detailed synthesis route is as follows: First, add 3g of chitosan to 300mL of 1% w / v acetic acid solution to prepare a 1% w / v chitosan solution; then stir the chitosan solution until completely dissolved; then add 12g of hydroxyethyl acrylate to the 1% w / v chitosan solution and stir continuously for 48h in a water bath at 60℃ to allow chitosan and hydroxyethyl acrylate to undergo a Michael addition reaction to obtain a reaction solution; then adjust the pH of the reaction solution to 7 with 10% w / v sodium hydroxide solution; then add the reaction solution dropwise to acetone to precipitate water-soluble chitosan; dry the precipitated water-soluble chitosan at 60℃, collect the water-soluble chitosan and grind it into powder to obtain water-soluble chitosan (HCS);

[0054] S12. Dissolve 1g of the water-soluble chitosan (HCS) prepared in S11 in distilled water and stir continuously at 70℃ to obtain a 1% w / v water-soluble chitosan solution; then mix the obtained water-soluble chitosan solution with sodium alginate at a mass ratio of 1:3 to obtain a mixed solution; stir the mixed solution continuously overnight until the sodium alginate is completely dissolved; let the mixture of water-soluble chitosan and sodium alginate stand for 12h to defoam, then transfer it to a glass petri dish and dry it at 40℃ for 12h to obtain a chitosan / sodium alginate (HCS / SA) composite hydrogel membrane;

[0055] S2. The chitosan / sodium alginate (HCS / SA) composite hydrogel membrane prepared in S1 is immersed in a calcium salt solution to obtain a calcium-crosslinked chitosan / sodium alginate hydrogel membrane, specifically including:

[0056] The chitosan / sodium alginate (HCS / SA) composite hydrogel membrane prepared in S12 was immersed in 0.25M CaCl2 solution for 30 minutes, then washed several times with distilled water, and then dried in an oven at 40℃ to obtain calcium crosslinked water-soluble chitosan / sodium alginate (HCS / SA-Ca) hydrogel membrane.

[0057] S3. The calcium-crosslinked chitosan / sodium alginate hydrogel membrane prepared in S2 is immersed once in a silver salt solution, and then immersed a second time in a solution of active components of traditional Chinese medicine containing polyphenol groups to obtain a composite hydrogel loaded with nano-antibacterial materials, specifically including:

[0058] The calcium-crosslinked water-soluble chitosan / sodium alginate (HCS / SA-Ca) hydrogel membrane prepared in step S2 was completely immersed in a 0.5 mM AgNO3 solution for 24 hours. Then, the hydrogel membrane was immersed in a 0.05 M tannic acid (TA) solution for 2 hours. The pH of the tannic acid solution was adjusted to 8 using alkali, thus allowing the AgNO3 to... + The nanoparticles (AgNPs) were reduced in situ to silver nanoparticles on the hydrogel membrane to obtain a composite hydrogel membrane (TA8-HCS / SA-Ca / Ag0.5) loaded with silver nanoparticles.

[0059] Example 2

[0060] A method for preparing a composite hydrogel loaded with nano-antibacterial materials includes the following steps:

[0061] S1. Chitosan and sodium alginate are mixed to prepare a chitosan / sodium alginate composite hydrogel membrane, specifically including:

[0062] S11. The detailed synthesis route is as follows: First, add 3g of chitosan to 300mL of 1% w / v acetic acid solution to prepare a 1% w / v chitosan solution; then stir the chitosan solution until completely dissolved; then add 12g of hydroxyethyl acrylate to the 1% w / v chitosan solution and stir continuously for 48h in a water bath at 60℃ to allow chitosan and hydroxyethyl acrylate to undergo a Michael addition reaction to obtain a reaction solution; then adjust the pH of the reaction solution to 7 with 10% w / v sodium hydroxide solution; then add the reaction solution dropwise to acetone to precipitate water-soluble chitosan; dry the precipitated water-soluble chitosan at 60℃, collect the water-soluble chitosan and grind it into powder to obtain water-soluble chitosan (HCS);

[0063] S12. Dissolve 1g of the water-soluble chitosan (HCS) prepared in S11 in distilled water and stir continuously at 70℃ to obtain a 1% w / v water-soluble chitosan solution; then mix the obtained water-soluble chitosan solution with sodium alginate at a mass ratio of 1:3 to obtain a mixed solution; stir the mixed solution continuously overnight until the sodium alginate is completely dissolved; let the mixture of water-soluble chitosan and sodium alginate stand for 12h to defoam, then transfer it to a glass petri dish and dry it at 40℃ for 12h to obtain a chitosan / sodium alginate (HCS / SA) composite hydrogel membrane;

[0064] S2. The chitosan / sodium alginate (HCS / SA) composite hydrogel membrane prepared in S1 is immersed in a calcium salt solution to obtain a calcium-crosslinked chitosan / sodium alginate hydrogel membrane, specifically including:

[0065] The chitosan / sodium alginate (HCS / SA) composite hydrogel membrane prepared in S12 was immersed in 0.25M CaCl2 solution for 30 minutes, then washed several times with distilled water, and then dried in an oven at 40℃ to obtain calcium crosslinked water-soluble chitosan / sodium alginate (HCS / SA-Ca) hydrogel membrane.

[0066] S3. The calcium-crosslinked chitosan / sodium alginate hydrogel membrane prepared in S2 is immersed once in a silver salt solution, and then immersed a second time in a solution of active components of traditional Chinese medicine containing polyphenol groups to obtain a composite hydrogel loaded with nano-antibacterial materials, specifically including:

[0067] The calcium-crosslinked water-soluble chitosan / sodium alginate (HCS / SA-Ca) hydrogel membrane prepared in step S2 was completely immersed in a 1 mM AgNO3 solution for 24 hours. Then, the hydrogel membrane was immersed in a 0.05 M tannic acid (TA) solution for 2 hours. The pH of the tannic acid solution was adjusted to 8 using alkali, thus allowing the AgNO3 to... + The nanoparticles (AgNPs) were reduced in situ to form nano-silver on the hydrogel membrane, thus preparing a composite hydrogel membrane (TA8-HCS / SA-Ca / Ag1) loaded with nano-silver particles.

[0068] Example 3

[0069] A method for preparing a composite hydrogel loaded with nano-antibacterial materials includes the following steps:

[0070] S1. Chitosan and sodium alginate are mixed to prepare a chitosan / sodium alginate composite hydrogel membrane, specifically including:

[0071] S11. The detailed synthesis route is as follows: First, add 3g of chitosan to 300mL of 1% w / v acetic acid solution to prepare a 1% w / v chitosan solution; then stir the chitosan solution until completely dissolved; then add 12g of hydroxyethyl acrylate to the 1% w / v chitosan solution and stir continuously for 48h in a water bath at 60℃ to allow chitosan and hydroxyethyl acrylate to undergo a Michael addition reaction to obtain a reaction solution; then adjust the pH of the reaction solution to 7 with 10% w / v sodium hydroxide solution; then add the reaction solution dropwise to acetone to precipitate water-soluble chitosan; dry the precipitated water-soluble chitosan at 60℃, collect the water-soluble chitosan and grind it into powder to obtain water-soluble chitosan (HCS);

[0072] S12. Dissolve 1g of the water-soluble chitosan (HCS) prepared in S11 in distilled water and stir continuously at 70℃ to obtain a 1% w / v water-soluble chitosan solution; then mix the obtained water-soluble chitosan solution with sodium alginate at a mass ratio of 1:3 to obtain a mixed solution; stir the mixed solution continuously overnight until the sodium alginate is completely dissolved; let the mixture of water-soluble chitosan and sodium alginate stand for 12h to defoam, then transfer it to a glass petri dish and dry it at 40℃ for 12h to obtain a chitosan / sodium alginate (HCS / SA) composite hydrogel membrane;

[0073] S2. The chitosan / sodium alginate (HCS / SA) composite hydrogel membrane prepared in S1 is immersed in a calcium salt solution.

[0074] The preparation of calcium-crosslinked chitosan / sodium alginate hydrogel membranes specifically includes:

[0075] The chitosan / sodium alginate (HCS / SA) composite hydrogel membrane prepared in S12 was immersed in 0.25M CaCl2 solution for 30 minutes, then washed several times with distilled water, and then dried in an oven at 40℃ to obtain calcium crosslinked water-soluble chitosan / sodium alginate (HCS / SA-Ca) hydrogel membrane.

[0076] S3. The calcium-crosslinked chitosan / sodium alginate hydrogel membrane prepared in S2 is immersed once in a silver salt solution, and then immersed a second time in a solution of active components of traditional Chinese medicine containing polyphenol groups to obtain a composite hydrogel loaded with nano-antibacterial materials, specifically including:

[0077] The calcium-crosslinked water-soluble chitosan / sodium alginate (HCS / SA-Ca) hydrogel membrane prepared in step S2 was completely immersed in a 5 mM AgNO3 solution for 24 hours. Then, the hydrogel membrane was immersed in a 0.05 M tannic acid (TA) solution for 2 hours. The pH of the tannic acid solution was adjusted to 8 using alkali, thus allowing the AgNO3 to...+ The nano-silver (AgNPs) on the hydrogel membrane were reduced in situ to obtain a composite hydrogel membrane (TA8-HCS / SA-Ca / Ag5).

[0078] Example 4

[0079] A method for preparing a composite hydrogel loaded with nano-antibacterial materials includes the following steps:

[0080] S1. Chitosan and sodium alginate are mixed to prepare a chitosan / sodium alginate composite hydrogel membrane, specifically including:

[0081] S11. The detailed synthesis route is as follows: First, add 3g of chitosan to 300mL of 1% w / v acetic acid solution to prepare a 1% w / v chitosan solution; then stir the chitosan solution until completely dissolved; then add 12g of hydroxyethyl acrylate to the 1% w / v chitosan solution and stir continuously for 48h in a water bath at 60℃ to allow chitosan and hydroxyethyl acrylate to undergo a Michael addition reaction to obtain a reaction solution; then adjust the pH of the reaction solution to 7 with 10% w / v sodium hydroxide solution; then add the reaction solution dropwise to acetone to precipitate water-soluble chitosan; dry the precipitated water-soluble chitosan at 60℃, collect the water-soluble chitosan and grind it into powder to obtain water-soluble chitosan (HCS);

[0082] S12. Dissolve 1g of the water-soluble chitosan (HCS) prepared in S11 in distilled water and stir continuously at 70℃ to obtain a 1% w / v water-soluble chitosan solution; then mix the obtained water-soluble chitosan solution with sodium alginate at a mass ratio of 1:3 to obtain a mixed solution; stir the mixed solution continuously overnight until the sodium alginate is completely dissolved; let the mixture of water-soluble chitosan and sodium alginate stand for 12h to defoam, then transfer it to a glass petri dish and dry it at 40℃ for 12h to obtain a chitosan / sodium alginate (HCS / SA) composite hydrogel membrane; S2. Immerse the chitosan / sodium alginate (HCS / SA) composite hydrogel membrane obtained in S1 in a calcium salt solution to obtain a calcium crosslinked chitosan / sodium alginate hydrogel membrane, specifically including:

[0083] The chitosan / sodium alginate (HCS / SA) composite hydrogel membrane prepared in S12 was placed in 0.25M CaCl₂ solution. l2 Soak in the solution for 30 minutes, then wash several times with distilled water, and then dry in an oven at 40°C to obtain a calcium cross-linked water-soluble chitosan / sodium alginate (HCS / SA-Ca) hydrogel membrane.

[0084] S3. The calcium-crosslinked chitosan / sodium alginate hydrogel membrane prepared in S2 is immersed once in a silver salt solution, and then immersed a second time in a solution of active components of traditional Chinese medicine containing polyphenol groups to obtain a composite hydrogel loaded with nano-antibacterial materials, specifically including:

[0085] The calcium-crosslinked water-soluble chitosan / sodium alginate (HCS / SA-Ca) hydrogel membrane prepared in S2 was completely immersed in a 10 mM AgNO3 solution for 24 h. Then, the hydrogel membrane was immersed in a 0.05 M tannic acid (TA) solution for 2 h. The pH of the tannic acid solution was adjusted to 8 using alkali, so that Ag+ was reduced in situ to nano-silver (AgNPs) on the hydrogel membrane, thus obtaining a composite hydrogel membrane (TA8-HCS / SA-Ca / Ag10).

[0086] Example 5

[0087] A method for preparing a composite hydrogel loaded with nano-antibacterial materials includes the following steps:

[0088] S1. Chitosan and sodium alginate are mixed to prepare a chitosan / sodium alginate composite hydrogel membrane, specifically including:

[0089] S11. The detailed synthesis route is as follows: First, add 3g of chitosan to 300mL of 1% w / v acetic acid solution to prepare a 1% w / v chitosan solution; then stir the chitosan solution until completely dissolved; then add 12g of hydroxyethyl acrylate to the 1% w / v chitosan solution and stir continuously for 48h in a water bath at 60℃ to allow chitosan and hydroxyethyl acrylate to undergo a Michael addition reaction to obtain a reaction solution; then adjust the pH of the reaction solution to 7 with 10% w / v sodium hydroxide solution; then add the reaction solution dropwise to acetone to precipitate water-soluble chitosan; dry the precipitated water-soluble chitosan at 60℃, collect the water-soluble chitosan and grind it into powder to obtain water-soluble chitosan (HCS);

[0090] S12. Dissolve 1g of the water-soluble chitosan (HCS) prepared in S11 in distilled water and stir continuously at 70℃ to obtain a 1% w / v water-soluble chitosan solution; then mix the obtained water-soluble chitosan solution with sodium alginate at a mass ratio of 1:3 to obtain a mixed solution; stir the mixed solution continuously overnight until the sodium alginate is completely dissolved; let the mixture of water-soluble chitosan and sodium alginate stand for 12h to defoam, then transfer it to a glass petri dish and dry it at 40℃ for 12h to obtain a chitosan / sodium alginate (HCS / SA) composite hydrogel membrane; S2. Immerse the chitosan / sodium alginate (HCS / SA) composite hydrogel membrane obtained in S1 in a calcium salt solution to obtain a calcium crosslinked hydrogel membrane, specifically including:

[0091] The chitosan / sodium alginate (HCS / SA) composite hydrogel membrane prepared in S12 was immersed in 0.25M CaCl2 solution for 30 minutes, then washed several times with distilled water, and then dried in an oven at 40℃ to obtain calcium crosslinked water-soluble chitosan / sodium alginate (HCS / SA-Ca) hydrogel membrane.

[0092] S3. The calcium-crosslinked chitosan / sodium alginate hydrogel membrane prepared in S2 is immersed once in a silver salt solution, and then immersed a second time in a solution of active components of traditional Chinese medicine containing polyphenol groups to obtain a composite hydrogel loaded with nano-antibacterial materials, specifically including:

[0093] The calcium-crosslinked water-soluble chitosan / sodium alginate (HCS / SA-Ca) hydrogel membrane prepared in step S2 was completely immersed in a 0.5 mM AgNO3 solution for 24 hours. Then, the hydrogel membrane was immersed in a 0.05 M tannic acid (TA) solution for 2 hours. The pH of the tannic acid solution was adjusted to 6 using alkali, thus allowing the AgNO3 to... + The nanoparticles (AgNPs) were reduced in situ to silver nanoparticles on the hydrogel membrane to obtain a composite hydrogel membrane (TA6-HCS / SA-Ca / Ag0.5) loaded with silver nanoparticles.

[0094] Example 6

[0095] A method for preparing a composite hydrogel loaded with nano-antibacterial materials includes the following steps:

[0096] S1. Chitosan and sodium alginate are mixed to prepare a chitosan / sodium alginate composite hydrogel membrane, specifically including:

[0097] S11. The detailed synthesis route is as follows: First, add 3g of chitosan to 300mL of 1% w / v acetic acid solution to prepare a 1% w / v chitosan solution; then stir the chitosan solution until completely dissolved; then add 12g of hydroxyethyl acrylate to the 1% w / v chitosan solution and stir continuously for 48h in a water bath at 60℃ to allow chitosan and hydroxyethyl acrylate to undergo a Michael addition reaction to obtain a reaction solution; then adjust the pH of the reaction solution to 7 with 10% w / v sodium hydroxide solution; then add the reaction solution dropwise to acetone to precipitate water-soluble chitosan; dry the precipitated water-soluble chitosan at 60℃, collect the water-soluble chitosan and grind it into powder to obtain water-soluble chitosan (HCS);

[0098] S12. Dissolve 1g of the water-soluble chitosan (HCS) prepared in S11 in distilled water and stir continuously at 70℃ to obtain a 1% w / v water-soluble chitosan solution; then mix the obtained water-soluble chitosan solution with sodium alginate at a mass ratio of 1:3 to obtain a mixed solution; stir the mixed solution continuously overnight until the sodium alginate is completely dissolved; let the mixture of water-soluble chitosan and sodium alginate stand for 12h to defoam, then transfer it to a glass petri dish and dry it at 40℃ for 12h to obtain a chitosan / sodium alginate (HCS / SA) composite hydrogel membrane; S2. Immerse the chitosan / sodium alginate (HCS / SA) composite hydrogel membrane obtained in S1 in a calcium salt solution to obtain a calcium crosslinked chitosan / sodium alginate hydrogel membrane, specifically including:

[0099] The chitosan / sodium alginate (HCS / SA) composite hydrogel membrane prepared in S12 was immersed in 0.25M CaCl2 solution for 30 minutes, then washed several times with distilled water, and then dried in an oven at 40℃ to obtain calcium crosslinked water-soluble chitosan / sodium alginate (HCS / SA-Ca) hydrogel membrane.

[0100] S3. The calcium-crosslinked chitosan / sodium alginate hydrogel membrane prepared in S2 is immersed once in a silver salt solution, and then immersed a second time in a solution of active components of traditional Chinese medicine containing polyphenol groups to obtain a composite hydrogel loaded with nano-antibacterial materials, specifically including:

[0101] The calcium-crosslinked water-soluble chitosan / sodium alginate (HCS / SA-Ca) hydrogel membrane prepared in step S2 was completely immersed in a 0.5 mM AgNO3 solution for 24 hours. Then, the hydrogel membrane was immersed in a 0.05 M tannic acid (TA) solution for 2 hours. The pH of the tannic acid solution was adjusted to 7 using alkali, thereby allowing the AgNO3 to... + The nanoparticles (AgNPs) were reduced in situ to silver nanoparticles on the hydrogel membrane to obtain a composite hydrogel membrane (TA7-HCS / SA-Ca / Ag0.5) loaded with silver nanoparticles.

[0102] Example 7

[0103] A method for preparing a composite hydrogel loaded with nano-antibacterial materials includes the following steps:

[0104] S1. Chitosan and sodium alginate are mixed to prepare a chitosan / sodium alginate composite hydrogel membrane, specifically including:

[0105] S11. The detailed synthesis route is as follows: First, add 3g of chitosan to 300mL of 1% w / v acetic acid solution to prepare a 1% w / v chitosan solution; then stir the chitosan solution until completely dissolved; then add 12g of hydroxyethyl acrylate to the 1% w / v chitosan solution and stir continuously for 48h in a water bath at 60℃ to allow chitosan and hydroxyethyl acrylate to undergo a Michael addition reaction to obtain a reaction solution; then adjust the pH of the reaction solution to 7 with 10% w / v sodium hydroxide solution; then add the reaction solution dropwise to acetone to precipitate water-soluble chitosan; dry the precipitated water-soluble chitosan at 60℃, collect the water-soluble chitosan and grind it into powder to obtain water-soluble chitosan (HCS);

[0106] S12. Dissolve 1g of the water-soluble chitosan (HCS) prepared in S11 in distilled water and stir continuously at 70℃ to obtain a 1% w / v water-soluble chitosan solution; then mix the obtained water-soluble chitosan solution with sodium alginate at a mass ratio of 1:3 to obtain a mixed solution; stir the mixed solution continuously overnight until the sodium alginate is completely dissolved; let the mixture of water-soluble chitosan and sodium alginate stand for 12h to defoam, then transfer it to a glass petri dish and dry it at 40℃ for 12h to obtain a chitosan / sodium alginate (HCS / SA) composite hydrogel membrane; S2. Immerse the chitosan / sodium alginate (HCS / SA) composite hydrogel membrane obtained in S1 in a calcium salt solution to obtain a calcium crosslinked chitosan / sodium alginate hydrogel membrane, specifically including:

[0107] The chitosan / sodium alginate (HCS / SA) composite hydrogel membrane prepared in S12 was immersed in 0.25M CaCl2 solution for 30 minutes, then washed several times with distilled water, and then dried in an oven at 40℃ to obtain calcium crosslinked water-soluble chitosan / sodium alginate (HCS / SA-Ca) hydrogel membrane.

[0108] S3. The calcium-crosslinked chitosan / sodium alginate hydrogel membrane prepared in S2 is immersed once in a silver salt solution, and then immersed a second time in a solution of active components of traditional Chinese medicine containing polyphenol groups to obtain a composite hydrogel loaded with nano-antibacterial materials, specifically including:

[0109] The calcium-crosslinked water-soluble chitosan / sodium alginate (HCS / SA-Ca) hydrogel membrane prepared in step S2 was completely immersed in a 0.5 mM AgNO3 solution for 24 hours. Then, the hydrogel membrane was immersed in a 0.05 M tannic acid (TA) solution for 2 hours. The pH of the tannic acid solution was adjusted to 10 using alkali, thus allowing the AgNO3 to... +

[0110] The nanoparticles (AgNPs) were reduced in situ to silver nanoparticles on the hydrogel membrane to prepare a composite hydrogel membrane (TA10-HCS / SA-Ca / Ag0.5) loaded with silver nanoparticles.

[0111] Comparative Example 1

[0112] A method for preparing a hydrogel membrane without nanomaterial loading includes the following steps:

[0113] S1. Chitosan and sodium alginate are mixed to prepare a hydrogel membrane, specifically including:

[0114] S11. The detailed synthesis route is as follows: First, add 3g of chitosan to 300mL of 1% w / v acetic acid solution to prepare a 1% w / v chitosan solution; then stir the chitosan solution until completely dissolved; then add 12g of hydroxyethyl acrylate to the 1% w / v chitosan solution and stir continuously for 48h in a water bath at 60℃ to allow chitosan and hydroxyethyl acrylate to undergo a Michael addition reaction to obtain a reaction solution; then adjust the pH of the reaction solution to 7 with 10% w / v sodium hydroxide solution; then add the reaction solution dropwise to acetone to precipitate water-soluble chitosan; dry the precipitated water-soluble chitosan at 60℃, collect the water-soluble chitosan and grind it into powder to obtain water-soluble chitosan;

[0115] S12. Dissolve 1g of the water-soluble chitosan obtained in S11 in distilled water and stir continuously at 70℃ to obtain a 1% w / v water-soluble chitosan solution; then mix the obtained water-soluble chitosan solution with sodium alginate at a mass ratio of 1:3 to obtain a mixed solution; stir the mixed solution continuously overnight until the sodium alginate is completely dissolved; let the mixture of water-soluble chitosan and sodium alginate stand for 12h to defoam, then transfer it to a glass petri dish and dry it at 40℃ for 12h to obtain a chitosan / sodium alginate hydrogel membrane;

[0116] S2. Immerse the hydrogel membrane in a calcium salt solution to obtain a calcium crosslinked hydrogel membrane, specifically including:

[0117] The chitosan / sodium alginate hydrogel membrane prepared in S12 was immersed in 0.25M CaCl2 solution for 30 minutes, then washed several times with distilled water, and then dried in an oven at 40℃ to obtain a calcium crosslinked water-soluble chitosan / sodium alginate (HCS / SA-Ca) unloaded nanomaterial hydrogel membrane.

[0118] Detection and Analysis

[0119] 1) Infrared spectroscopy analysis

[0120] Infrared spectroscopy analysis was performed on the chitosan (CS), sodium alginate (SA), and the prepared water-soluble chitosan (HCS) from Example 1. The results are as follows: Figure 1 As shown in Figure A.

[0121] from Figure 1 As observed in A, for chitosan (CS), 3421 cm -1 The absorption peak at 2919 cm⁻¹ is attributed to the broad peak resulting from the overlap of the OH stretching vibration absorption peak and the NH stretching vibration absorption peak; -1 1653cm -1 and 1383cm -1 1322cm -1 The absorption peaks at these locations correspond to the stretching vibration of CH in the CS backbone, the C=O stretching vibration of the amide (amide I band), the CO stretching vibration of the primary alcohol group (-CH2-OH), and the NH bending vibration of the amide, respectively.

[0122] For sodium alginate (SA), 1595cm -1 and 1351cm -1 The absorption peak at that point is attributed to the C=O asymmetric stretching vibration and the C=O symmetric stretching vibration of -COO-.

[0123] Compared to chitosan (CS), water-soluble chitosan (HCS) has a lower concentration at 1726 cm⁻¹. -1 A new absorption peak for the C=O asymmetric stretching vibration of the ester bond in hydroxyethyl acrylate appeared at 1408 cm⁻¹. -1 A new absorption peak for the CO stretching vibration of the secondary alcohol group (-CH2-CH2-OH) in hydroxyethyl acrylate was observed, thus proving the successful modification of water-soluble chitosan (HCS).

[0124] The HCS / SA hydrogel membrane and composite hydrogel membrane (TA8-HCS / SA-Ca / Ag0.5) prepared in Example 1 using tannic acid (TA) and S12, and the membranes in Example 5 (TA6-HCS / SA-Ca / Ag0.5) and Example 6 were used.

[0125] The composite hydrogel membranes prepared in Example 7 (TA7-HCS / SA-Ca / Ag0.5) and Example 8 (TA10-HCS / SA-Ca / Ag0.5), as well as the calcium-crosslinked water-soluble chitosan / sodium alginate (HCS / SA-Ca) unsupported nanomaterial hydrogel membrane prepared in Example 1, were analyzed by infrared spectroscopy. The results are as follows: Figure 1 As shown in B.

[0126] from Figure 1 Observations in B show that for the HCS / SA hydrogel membrane, 1625 cm⁻¹ -1 1401cm-1 and 1317cm -1 The characteristic peaks at these locations correspond to the asymmetric stretching vibration of C=O in the carboxylic acid group, the symmetric stretching vibration of C=O, and the bending vibration of NH in the amide group, respectively.

[0127] For the composite hydrogel membranes prepared in Examples 1 (TA8-HCS / SA-Ca / Ag0.5), 5 (TA6-HCS / SA-Ca / Ag0.5), 6 (TA7-HCS / SA-Ca / Ag0.5), and 7 (TA10-HCS / SA-Ca / Ag0.5), due to the interaction of TA and Ca... 2+ Under alkaline conditions, coordination bonds are formed, leading to a decrease in the degree of crosslinking. The characteristic peak of the asymmetric stretching vibration belonging to C=O decreases from 1617 cm⁻¹. -1 Moved to 1628cm -1 As the pH of the TA solution decreases, the asymmetric stretching vibration frequency of C=O in the TA-HCS / SA-Ca / Ag membrane decreases. This phenomenon may be due to the lower pH of the TA solution increasing the degree of protonation and hydrogen bonding in the hydrogel. TA at 1718 cm⁻¹... -1 1612cm -1 and 1203cm -1 The characteristic peaks at these locations are attributed to the stretching vibrations of C=O, C=C, and Ph-O, respectively. In Examples 1 (TA8-HCS / SA-Ca / Ag0.5), 5 (TA6-HCS / SA-Ca / Ag0.5), 6 (TA7-HCS / SA-Ca / Ag0.5), and 7...

[0128] In the composite hydrogel membranes prepared by (TA10-HCS / SA-Ca / Ag0.5), some peaks belonging to TA were observed, which proved that TA was successfully introduced into these hydrogel membranes.

[0129] 2) XRD analysis

[0130] X-ray diffraction analysis was performed on the hydrogel films prepared in Examples 1 to 7, as well as in Control Example 1. The results are as follows: Figure 2 As shown.

[0131] from Figure 2Analysis revealed that the composite hydrogel films prepared in Examples 2 (TA8-HCS / SA-Ca / Ag1), 3 (TA8-HCS / SA-Ca / Ag5), and 4 (TA8-HCS / SA-Ca / Ag10) exhibited four distinct absorption peaks at 2θ = 38.40°, 44.62°, 64.94°, and 76.86°. These peaks belong to face-centered cubic AgNPs with crystal plane indices of (111), (200), (220), and (311), respectively. Furthermore, the crystallinity of the AgNPs increased with the crystallinity of Ag... + As the concentration decreased, the absorption peaks decreased. In Example 1 (TA8-HCS / SA-Ca / Ag0.5), the composite hydrogel membrane showed two absorption peaks at 2θ = 38.40° and 44.62°. However, no obvious peaks were detected in the composite hydrogel membranes prepared in Example 6 (TA7-HCS / SA-Ca / Ag0.5) and Example 5 (TA6-HCS / SA-Ca / Ag0.5), possibly because the amount of AgNPs formed was too small to detect their absorption peaks.

[0132] 3) SEM analysis

[0133] The HCS / SA hydrogel membrane and the composite hydrogel membrane TA8-HCS / SA-Ca / Ag0.5 prepared in Example 1 were analyzed by scanning electron microscopy to further observe the microstructure of the un-silver-loaded and silver-loaded hydrogel membranes. The results are as follows: Figure 3 As shown in Figure A.

[0134] from Figure 3 Analysis A shows that the surface of the HCS / SA hydrogel membrane has a dense structure, and the surface of the composite hydrogel membrane TA8-HCS / SA-Ca / Ag0.5 hydrogel membrane contains nearly spherical nanoparticles. Combined with X-ray diffraction analysis results, these spherical nanoparticles can be identified as AgNPs.

[0135] 4) EDS analysis

[0136] The composite hydrogel membrane TA8-HCS / SA-Ca / Ag0.5 prepared in Example 1 was subjected to EDS surface scanning analysis to observe the elemental distribution of the composite hydrogel membrane TA8-HCS / SA-Ca / Ag0.5. The results are as follows: Figure 3 As shown in B.

[0137] from Figure 3Analysis in section B revealed the presence of carbon, oxygen, calcium, and silver elements on the surface of the TA8-HCS / SA-Ca / Ag0.5 nanoparticle-loaded composite hydrogel membrane. The absorbance band at approximately 3 keV confirmed the presence of silver nanoparticles on the TA8-HCS / SA-Ca / Ag0.5 composite hydrogel membrane. The uniform distribution of calcium elements indicates a good degree of cross-linking between the hydrogel and calcium ions.

[0138] 4) Stability and swelling analysis

[0139] The good swelling and stability of hydrogels can absorb wound secretions, creating a suitable microenvironment for wound healing. Therefore, the gel content of the calcium cross-linked water-soluble chitosan / sodium alginate (HCS / SA-Ca) hydrogel membrane and composite hydrogel membrane (TA8-HCS / SA-Ca / Ag0.5) prepared in Example 1, as well as the composite hydrogel membranes prepared in Examples 5 (TA6-HCS / SA-Ca / Ag0.5), 6 (TA7-HCS / SA-Ca / Ag0.5), and 7 (TA10-HCS / SA-Ca / Ag0.5) were tested, and the results are as follows. Figure 4 As shown in Figure A.

[0140] from Figure 4 Analysis in section A shows that the gel content of both the calcium-crosslinked water-soluble chitosan / sodium alginate gel membrane and the composite hydrogel membrane is above 90%. However, from... Figure 4 Analysis A shows that the pH value of the tannic acid solution affects the gel content of the composite hydrogel membrane. The gel content of the composite hydrogel membrane (TA-HCS / SA-Ca / Ag) decreases with increasing pH. When the pH value of the tannic acid solution is below 8, the gel content of the composite hydrogel membrane (TA-HCS / SA-Ca / Ag) remains above 90%, thus demonstrating the good stability of these composite hydrogel membranes. When the pH value of the tannic acid solution reaches 10, the gel content begins to decrease significantly, which may be due to the formation of a complex between tannic acid and calcium ions, leading to a decrease in the degree of cross-linking of the hydrogel.

[0141] The calcium-crosslinked water-soluble chitosan / sodium alginate (HCS / SA-Ca) hydrogel membrane and composite hydrogel membrane (TA8-HCS / SA-Ca / Ag0.5) prepared in Example 1, as well as the composite hydrogel membranes prepared in Examples 5 (TA6-HCS / SA-Ca / Ag0.5), 6 (TA7-HCS / SA-Ca / Ag0.5), and 7 (TA10-HCS / SA-Ca / Ag0.5), were subjected to swelling tests by immersion in phosphate-buffered saline (PBS). The results are as follows: Figure 4 As shown in B and 4C.

[0142] from Figure 4Comprehensive analysis of B and 4C indicates that the calcium-crosslinked water-soluble chitosan / sodium alginate (HCS / SA-Ca) hydrogel membrane fractured and deformed after being immersed in PBS solution (pH 7.4) at 37°C for 24 hours, while Example 1...

[0143] The composite hydrogel membrane in (TA8-HCS / SA-Ca / Ag0.5) remained relatively stable after immersion in PBS (37℃, pH 7.4) for 72 h. Furthermore, it was found that the swelling degree of the composite hydrogel membrane (TA-HCS / SA-Ca / Ag) could be adjusted by regulating the pH of the tannic acid solution, and the swelling degree tended to increase with increasing pH of the tannic acid solution. The swelling ratio of the calcium-crosslinked water-soluble chitosan / sodium alginate (HCS / SA-Ca) hydrogel membrane was 631.01±8.81%. The swelling ratio of the composite hydrogel membrane in Example 5 (TA6-HCS / SA-Ca / Ag0.5) was 530.33±13.02%. The swelling ratio of the composite hydrogel membrane in Example 6 (TA7-HCS / SA-Ca / Ag0.5) was 388.89±23.99%. The swelling ratio of the composite hydrogel membrane in Example 1 (TA8-HCS / SA-Ca / Ag0.5) was 536.00±16.89%. The swelling ratio of the composite hydrogel membrane in Example 7 (TA10-HCS / SA-Ca / Ag0.5) was 648.69±12.10%. The equilibrium swelling time of calcium-crosslinked water-soluble chitosan / sodium alginate (HCS / SA-Ca) hydrogel membrane was 24 h, and the equilibrium swelling time was extended to 72 h after loading AgNPs in tannic acid solution.

[0144] 5) Mechanical property analysis

[0145] The composite hydrogel films prepared in Examples 1 (TA8-HCS / SA-Ca / Ag0.5), 5 (TA6-HCS / SA-Ca / Ag0.5), 6 (TA7-HCS / SA-Ca / Ag0.5), and 7 (TA10-HCS / SA-Ca / Ag0.5), as well as the calcium-crosslinked water-soluble chitosan / sodium alginate (HCS / SA-Ca) unloaded nanomaterial hydrogel film prepared in Example 1, were tested for mechanical properties such as bending characteristics, tensile strength, elongation at break, and Young's modulus using a universal tensile testing machine. The results are as follows: Figure 5 As shown in A, 5B and 5C.

[0146] from Figure 5Analysis revealed that, compared to the calcium-crosslinked water-soluble chitosan / sodium alginate (HCS / SA-Ca) hydrogel membrane, the composite hydrogel membrane loaded with silver nanoparticles of this invention exhibits better flexibility. Furthermore, the AgNP-loaded HCS / SA-Ca hydrogel membrane becomes more flexible with increasing pH of the tannic acid solution. Compared to the calcium-crosslinked water-soluble chitosan / sodium alginate (HCS / SA-Ca) hydrogel membrane, the tensile strength and Young's modulus of the AgNP-loaded HCS / SA-Ca hydrogel membrane tend to decrease, which is attributed to the decrease in AgNPs. + The introduction of tannic acid reduced the crosslinking degree of the HCS / SA-Ca hydrogel membrane. However, the elongation at break of the AgNP-loaded HCS / SA-Ca hydrogel membrane increased significantly, exhibiting better extensibility. This characteristic demonstrates that the AgNP-loaded HCS / SA-Ca hydrogel membrane is more suitable for skin contact and body movement. Furthermore, the effect of loading AgNPs onto tannic acid solutions at different pH values ​​on the mechanical properties of the hydrogel membrane was investigated. When the pH of the TA solution was 6–10, the tensile strength of the AgNPs / SA-Ca hydrogel membrane decreased from 8078.5±594 kPa to 1131.6±62 kPa, the Young's modulus decreased from 2859.3±25 kPa to 22.36±1.25 kPa, and the elongation at break increased from 6.256±1.25% to 56.857±1.62%. These results may be due to pH regulating the phenolic hydroxyl groups in tannic acid molecules, affecting the hydrogen bonding effect within the HCS / SA-Ca hydrogel network. Generally, the tensile strength of human skin ranges from 1 to 32 MPa, and the elongation at break is approximately 17% to 27%. Comparing the mechanical properties of HCS / SA-Ca hydrogel membranes loaded with AgNPs in tannic acid solutions at different pH values, it was found that the composite hydrogel membrane prepared in Example 1 (TA8-HCS / SA-Ca / Ag0.5) is more suitable as a wound dressing.

[0147] 6) Hemolysis analysis

[0148] The hemolysis rate of the composite hydrogel membranes prepared in Examples 1 (TA8-HCS / SA-Ca / Ag0.5), 5 (TA6-HCS / SA-Ca / Ag0.5), 6 (TA7-HCS / SA-Ca / Ag0.5), and 7 (TA10-HCS / SA-Ca / Ag0.5) was analyzed compared with the calcium-crosslinked water-soluble chitosan / sodium alginate (HCS / SA-Ca) unloaded nanomaterial hydrogel membrane prepared in Control Example 1. The results are as follows: Figure 6 As shown.

[0149] from Figure 6Analysis revealed that the hemolysis rate of the hydrogel membrane was measured to assess its blood compatibility. After incubating rabbit blood for 1 hour with extracts of HCS / SA-Ca, TA6-HCS / SA-Ca / Ag0.5, TA7-HCS / SA-Ca / Ag0.5, TA8-HCS / SA-Ca / Ag0.5, and TA10-HCS / SA-Ca / Ag0.5 hydrogel membranes, the solution colors of the hydrogel membrane test group and the negative control group (PBS buffer) remained essentially unchanged. Conversely, the solution color of the positive control group (water) turned blood red. Furthermore, the hemolysis rate of the hydrogel membrane test group was calculated. Figure 6 As shown in the lower section. From Figure 6 The analysis in the lower part of the paper shows that the hemolysis rate of the chitosan / sodium alginate hydrogel membrane loaded with silver nanoparticles increases with the increase of the pH of the tannic acid soaking solution. The hemolysis rate of each experimental group is below 5%, which meets the hemolysis safety requirements.

[0150] 7) Antibacterial activity analysis

[0151] Antibacterial hydrogels possess the ability to rapidly kill bacteria and absorb wound exudate, making them suitable for treating wound infections. The antibacterial activity of the composite hydrogel membranes prepared in Examples 1 (TA8-HCS / SA-Ca / Ag0.5), 2 (TA8-HCS / SA-Ca / Ag1), 3 (TA8-HCS / SA-Ca / Ag5), and 4 (TA8-HCS / SA-Ca / Ag10) against *Escherichia coli*, *Pseudomonas aeruginosa*, and *Staphylococcus aureus* was tested using the inhibition zone method. The results are as follows: Figure 7 As shown in Table 2, the antibacterial activity of silver-loaded hydrogel membranes soaked in AgNO3 solutions of different concentrations against Escherichia coli, Pseudomonas aeruginosa, and Staphylococcus aureus was further investigated. The diameter of the inhibition zone was measured with a ruler.

[0152] from Figure 7 Observation revealed a distinct inhibition zone around the AgNP-loaded TA-HCS / SA-Ca / Ag0.5 hydrogel membrane of the present invention. The results indicate that the loading of AgNPs significantly enhances the antibacterial activity of the HCS / SA-Ca hydrogel membrane.

[0153] Analysis of Table 1 shows that the concentration of AgNO3 solution has a significant impact on the antibacterial effect of the hydrogel membrane loaded with AgNPs. Figure 7 As can be seen from Table 1, the composite hydrogel membrane prepared in Example 1 (TA8-HCS / SA-Ca / Ag0.5) has the best antibacterial effect against the three bacteria.

[0154] Table 1. Diameter of the antibacterial zone of silver-loaded hydrogel membranes prepared by immersion in AgNO3 solution of different concentrations.

[0155]

[0156] In summary, the study found that the pH value of the TA solution used for in-situ reduction of AgNPs has a significant impact on the antibacterial effect of calcium-crosslinked water-soluble chitosan / sodium alginate (HCS / SA-Ca) hydrogel membranes. Example 5

[0157] The composite hydrogel membranes prepared in Example 1 (TA6-HCS / SA-Ca / Ag0.5) and Example 6 (TA7-HCS / SA-Ca / Ag0.5) showed antibacterial activity against S. aureus. Examples 1 (TA8-HCS / SA-Ca / Ag0.5) and Example 7...

[0158] The composite hydrogel membrane prepared with (TA10-HCS / SA-Ca / Ag0.5) exhibited antibacterial activity against all three bacteria. Furthermore, the composite hydrogel membrane prepared in Example 1 (TA8-HCS / SA-Ca / Ag0.5) showed the strongest antibacterial activity against all three bacteria, with inhibition zone diameters of 25.4–26.1 mm against *E. coli*, 31.5–33.0 mm against *S. aureus*, and 22.3–23.1 mm against *P. aeruginosa*. Comparison of the antibacterial effects of the same hydrogel membrane against the three bacteria revealed that the AgNP-loaded hydrogel membrane exhibited the strongest growth inhibition against *S. aureus*. Human wounds are frequently infected with Gram-positive bacteria, with *S. aureus* infection being the most common. Therefore, AgNP-loaded hydrogel membranes show potential application value in the treatment of wound infections.

[0159] The above embodiments are merely preferred embodiments provided to fully illustrate the present invention, and the scope of protection of the present invention is not limited thereto. Equivalent substitutions or modifications made by those skilled in the art based on the present invention are all within the scope of protection of the present invention.

Claims

1. A method for preparing a composite hydrogel loaded with nanometer antibacterial material, characterized in that, Includes the following steps: S1. Chitosan and sodium alginate are mixed to prepare a chitosan / sodium alginate composite hydrogel membrane; S2. The chitosan / sodium alginate composite hydrogel membrane prepared in S1 is immersed in a calcium salt solution to obtain a calcium crosslinked chitosan / sodium alginate hydrogel membrane. S3. The calcium-crosslinked chitosan / sodium alginate hydrogel membrane prepared in S2 is immersed in a silver salt solution once, and then immersed in a solution of traditional Chinese medicine active components containing polyphenol groups a second time to obtain a composite hydrogel loaded with nano-antibacterial materials. The concentration of silver salt in the silver salt solution is 0.5~10mM; the active ingredient solution of traditional Chinese medicine contains 2~100 ortho- and tho-diphenol hydroxyl groups; The active ingredient solution of traditional Chinese medicine is selected from at least one of tannic acid solution, curcumin solution and chlorogenic acid solution; The concentration of the active ingredient in the solution of traditional Chinese medicine is 0.05M~0.1M; And / or the pH value of the solution of the active components of the traditional Chinese medicine is between 6 and 10.

2. The method of claim 1, wherein the nanomaterial- loaded composite hydrogel is prepared by mixing the nanomaterial and the polymer solution. In S1, the chitosan is water-soluble chitosan; And / or in S2, the calcium salt is selected from calcium chloride; And / or in S3, the silver salt is selected as silver nitrate.

3. The method of claim 2, wherein the nanomaterial- loaded composite hydrogel is prepared by mixing the nanomaterial and the polymer solution. The method for preparing the water-soluble chitosan is as follows: chitosan is dissolved in acetic acid solution, then hydroxyethyl acrylate is added, and the mixture is continuously stirred at 50℃~70℃ to obtain a reaction solution; the pH value of the reaction solution is adjusted to neutral, acetone is added, and the mixture is dried to obtain water-soluble chitosan.

4. The method of claim 1, wherein the nanomaterial- loaded composite hydrogel is prepared by mixing the nanomaterial and the polymer solution. S1 specifically includes: mixing and stirring chitosan aqueous solution with sodium alginate until sodium alginate is completely dissolved, allowing it to stand, drying it, and obtaining a hydrogel membrane.

5. The method of claim 4, wherein the nanomaterial- loaded composite hydrogel is prepared by mixing the nanomaterial and the polymer solution. The chitosan aqueous solution contains 1-5% chitosan by mass concentration. And / or the mass ratio of the chitosan aqueous solution to sodium alginate is 1:3 to 1:

5.

6. The method for preparing the composite hydrogel loaded with nano-antibacterial materials according to claim 1, characterized in that, In step S2, the concentration of calcium salt in the calcium salt solution is 0.25M~0.5M; And / or the soaking time in the calcium salt solution is 30 min to 2 h.

7. A composite hydrogel loaded with nano-antibacterial materials prepared by the preparation method according to any one of claims 1 to 6.

8. The use of the nanometer antibacterial material loaded composite hydrogel prepared by the preparation method of any one of claims 1 to 6, characterized in that, Application of the composite hydrogel loaded with nano-antibacterial materials in the preparation of antibacterial dressings.

Citation Information

Patent Citations

  • Method for reducing and preparing functionalized nano-silver based on polyphenol

    CN103302306A

  • Bionic alginate composite antimicrobial dressing and preparation method thereof

    CN103908693A