A PHBV microsphere, its preparation method and application

The preparation of PHBV microbeads using green solvents and solvent exchange methods solves the problems of toxic solvents and high-temperature melting methods in traditional methods, and realizes the production of environmentally friendly, controllable particle size and smooth surface microbeads, which are suitable for cosmetics and cleaning products.

CN117624652BActive Publication Date: 2026-11-17WENZHOU INST UNIV OF CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311342207.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-17
Publication Date
2026-11-17
Estimated Expiration
2043-10-17

AI Technical Summary

Technical Problem

Existing methods for preparing PHBV microbeads rely on toxic and harmful solvents, and the high-temperature melting method carries the risk of thermal degradation, making it difficult to achieve large-scale commercial production and environmentally friendly production.

Method used

PHBV microspheres were prepared using green solvents such as isosorbide dimethyl ether, propylene carbonate, divalent esters, dimethyl adipate, methyl lactate, and dipropylene glycol methyl ether, combined with a solvent exchange method. Spherical microspheres were formed by utilizing surface tension and shear force.

Benefits of technology

PHBV microbeads with controllable particle size and smooth surface were prepared, exhibiting good biodegradability and skin cleansing ability, suitable for large-scale production and stable under aseptic conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117624652B_ABST
    Figure CN117624652B_ABST
Patent Text Reader

Abstract

This invention relates to the field of material preparation technology, and particularly to a PHBV microsphere, its preparation method, and its application. The preparation method of the PHBV microsphere includes the following steps: dissolving poly(3-hydroxybutyrate-co-3-hydroxyvalerate) in a green solvent to obtain a poly(3-hydroxybutyrate-co-3-hydroxyvalerate) solution; adding the poly(3-hydroxybutyrate-co-3-hydroxyvalerate) solution to a polysorbate-80 aqueous solution and stirring continuously, obtaining a solidified PHBV microsphere initial product after solvent exchange; filtering and washing the solidified PHBV microsphere initial product, and freeze-drying to obtain the PHBV microspheres; wherein the green solvent includes one or more of isosorbide dimethyl ether, propylene carbonate, divalent esters, dimethyl adipate, methyl lactate, and dipropylene glycol methyl ether. This invention uses a green solvent to dissolve PHBV and utilizes a solvent exchange method to prepare PHBV microspheres with controllable particle size. The entire preparation method is green and simple, thus promising for large-scale production of PHBV microspheres.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of materials preparation technology, and in particular to a PHBV microsphere, its preparation method and application. Background Technology

[0002] Plastic microbeads, belonging to primary microplastics, are mainly used in personal care products or cosmetics for mechanical exfoliation, such as toothpaste, facial cleansers, and scrubs. Traditional plastic microbeads are made of materials such as polypropylene and polyethylene (PE), which are non-biodegradable. Their small size makes them prone to adsorbing toxins, posing a threat to the ecological environment and even human health once released into the aquatic environment. Therefore, in recent years, many countries have issued "plastic restriction orders" for cosmetic production. China, in its "Guidance Catalogue for Industrial Structure Adjustment" (2019), also requires that the production of daily chemical products containing plastic microbeads be prohibited by December 31, 2020, and their sale by December 31, 2022. This forces the cosmetics industry to seek sustainable and biodegradable alternatives to microbeads.

[0003] Several biodegradable materials could be potential alternatives to traditional microbeads: natural hard materials such as walnut shells and rice seeds; natural polymers such as cellulose, chitin, lignin, alginate, and starch; and bio-based synthetic polymers such as polycaprolactone and polylactic acid. However, natural hard materials are rigid and have sharp edges when mechanically ground, which can easily damage the skin during washing; some natural polymers require expensive ionic liquids to dissolve, making them costly and difficult to handle and recycle; and the bio-based polymer polylactic acid is non-degradable in seawater. Therefore, developing polymer microbeads with suitable mechanical properties and marine degradability remains challenging.

[0004] Poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (PHBV) is a bio-based polyester with the chemical structure shown in formula (1). It is produced by microorganisms under non-equilibrium conditions and can ultimately be completely degraded by microorganisms into carbon dioxide, water, and biomass. The biomass then enters the microorganisms to provide them with nutrients, thus forming a closed-loop cycle from "cradle to cradle." PHBV is not only biocompatible and can degrade in soil, compost, and activated sludge, but it can also degrade in seawater, making it a viable alternative to traditional plastic microbeads. For example, Chloé Volant et al. prepared PHBV microbeads and studied their marine degradation compared to polylactic acid. Cheng et al. investigated the marine degradation of commercially available PHBV microbeads through a two-step experiment.

[0005] Equation (1): .

[0006] However, most traditional commercial methods for preparing PHBV microspheres employ emulsification / solvent evaporation, which uses toxic organic solvents, posing potential threats to the environment and human health. For example, Chloé Volante et al. prepared PHBV microspheres via an emulsification process: PHBV (3 mol% HV) was dissolved in chloroform reflux at 50 °C for 24 h to obtain a 50 g / L PHBV solution. The PHBV solution was then slowly added to a 2% (w / v) aqueous solution of polyvinyl alcohol, mechanically stirred at 4000 rpm for 15 min, and continuously magnetically stirred for 24 hours to slowly evaporate the organic solvent. The resulting microspheres were then separated using a sieve, washed with deionized water, and finally lyophilized to collect the microspheres. Yousof Farrage et al., in addition to using the emulsification / solvent evaporation method, also prepared PHBV microspheres via nanoprecipitation: PHBV (12 mol% HV, Mn 2.4 × 10⁻⁶) was dissolved in chloroform under ultrasonic and heating conditions at 40 °C. 5 PHBV solutions with a concentration of 0.1–1% w / v were prepared by dissolving PHBV in dichloromethane or chloroform. Then, PHBV / dichloromethane and PHBV / trichloromethane solutions were added dropwise to methanol or methanol-water solutions containing sodium dodecyl sulfate surfactant, respectively, and formed microspheres under ultrasonic or mechanical stirring at room temperature. The organic solvent was then evaporated, the microspheres were washed several times with water, collected, and lyophilized. PHBV (12 mol% HV, Mn 2.4 × 10⁻⁶) was heated to 85 °C and then added to the solution. 5 PHBV / DMF solution with a concentration of 0.1–2% w / v was prepared by dissolving it in dimethylformamide (DMF). The PHBV / DMF solution was then added dropwise to water or sodium chloride solution and subjected to ultrasonic or mechanical stirring at room temperature to form microbeads. The microbeads were washed several times with water, collected, and lyophilized for characterization.

[0007] As an alternative, Choietal prepared poly(3-hydroxybutyrate-co-4-hydroxybutyrate), P3HB-4HB microbeads for skin exfoliation using a solvent-free melt electrospray method. The preparation process was as follows: First, 3g of P3HB-4HB particles were loaded into a heated metal syringe connected to an oil circulator. The melting temperature was adjusted to 170-230°C, and the P3HB-4HB particles were stored in the metal syringe at the specified temperature for 30 minutes to ensure melting. Subsequently, the metal syringe was vertically mounted on an injection pump, and a high-voltage generator was connected to needles of various sizes (17-23G) mounted on the metal syringe. The applied voltage was adjusted within the range of 0-6 kV. A coagulation bath containing distilled water (i.e., the non-solvent form of P3HB-4HB) was used at room temperature, with the distance between the needle and the coagulation bath set to 15 cm. The prepared microbeads had a smoother surface and adsorbed less organic contaminants than commercial microbeads.

[0008] However, the high temperatures required for melting polymers can lead to polymer thermal degradation and alterations in their chemical and physical properties. Furthermore, the relatively complex design and operation, along with the lack of large-scale commercial industrial equipment, pose challenges to melt electrospraying. Therefore, seeking environmentally friendly solvents and simple production methods is crucial for achieving sustainable PHBV microsphere manufacturing. Summary of the Invention

[0009] The present invention aims to overcome the problems and deficiencies existing in the prior art by providing a PHBV microsphere and its preparation method to overcome the above-mentioned deficiencies.

[0010] To achieve the above-mentioned objectives, the present invention is implemented through the following technical solution: On one hand, the present invention provides a method for preparing PHBV microspheres, comprising the following steps: (1) Dissolve poly(3-hydroxybutyrate-co-3-hydroxyvalerate) in a green solvent to obtain a poly(3-hydroxybutyrate-co-3-hydroxyvalerate) solution; (2) The poly(3-hydroxybutyrate-co-3-hydroxyvalerate) solution was added to the polysorbate-80 aqueous solution and stirred continuously. After solvent exchange, the cured PHBV microbeads were obtained. (3) The cured PHBV microbeads are filtered and washed, and then freeze-dried to obtain the PHBV microbeads; The green solvent includes one or more of isosorbide dimethyl ether, propylene carbonate, divalent ester, dimethyl adipate, methyl lactate, and dipropylene glycol methyl ether.

[0011] Most current methods for producing poly(3-hydroxybutyrate-co-3-hydroxyvalerate) microspheres (PHBV microspheres) rely on emulsification techniques using large amounts of toxic and harmful organic solvents. This invention, on a green scale, uses one or more green solvents such as isosorbide dimethyl ether, propylene carbonate, divalent esters, dimethyl adipate, methyl lactate, and dipropylene glycol methyl ether as good solvents, and polysorbate-80 aqueous solution as an antisolvent, to rapidly prepare PHBV microspheres with controllable particle size using a solvent exchange method. Among these, isosorbide dimethyl ether, propylene carbonate, divalent esters, dimethyl adipate, methyl lactate, and dipropylene glycol methyl ether are commonly used in organic reactions, and no research has yet been proposed in the existing technology regarding the use of these green solvents to prepare PHBV microspheres.

[0012] Solvent exchange method: When the polymer solution is added dropwise to the antisolvent, the polymer solution immediately breaks into spherical droplets due to the combined effects of surface tension and shear force. Upon initial contact with the aqueous solution, the outer surface of the polymer droplets quickly becomes supersaturated due to the rapid diffusion of the green solvent and water, forming initially solidified microbeads. As the solvent and water continue to diffuse within the droplets, solidified microbeads eventually form.

[0013] By controlling process parameters such as polymer solution concentration, stirring speed, and surfactant concentration, PHBV microbeads of different sizes can be prepared. The prepared microbeads are spherical with smooth surfaces (their morphology is more regular and their surface smoother than microbeads prepared by melt spraying). The smooth surface not only results in less adsorption of organic pollutants but also makes them gentler and more comfortable when used for skin exfoliation. Cleansers containing the PHBV microbeads of this invention have better skin cleansing efficiency compared to commercially available cleansers without microbeads, cleansers containing irregularly shaped PE particles, and cleansers containing microcrystalline cellulose (MCC) particles. Because the invention for preparing PHBV microbeads is green and simple, and can achieve concentrations up to 15 wt%, large-scale production is expected. Furthermore, the PHBV microbeads prepared in this invention can degrade in the presence of microorganisms but remain stable in the absence of microorganisms.

[0014] Preferably, the poly(3-hydroxybutyrate-co-3-hydroxyvalerate) contains 18-28 mol of hydroxyvalerate.

[0015] Polyhydroxybutyrate (PHB) has poor toughness. Introducing hydroxyvalerate (HV) reduces the structural regularity of PHB, affecting both its crystal structure and crystallization rate. Increased HV content leads to decreased crystallinity and melting temperature, while higher HV content results in faster degradation. Since HV content affects the physical properties, thermal properties, and biodegradability of PHBV, the selection of HV content was experimentally controlled according to specific application requirements. Ultimately, this invention determined that PHBV microspheres prepared with an HV content of 18–28 mol% yielded the best quality.

[0016] Preferably, the temperature of the poly(3-hydroxybutyrate-co-3-hydroxyvalerate) solution is greater than or equal to 80 °C.

[0017] The inventors discovered in experiments that poly(3-hydroxybutyrate-co-3-hydroxyvalerate) is difficult to dissolve below 80 ℃, and the prepared solution is prone to solidification and lacks fluidity. Therefore, the temperature of poly(3-hydroxybutyrate-co-3-hydroxyvalerate) solution should be greater than or equal to 80 ℃.

[0018] Preferably, the concentration of the poly(3-hydroxybutyrate-co-3-hydroxyvalerate) solution is 5-15% by weight.

[0019] The concentration of poly(3-hydroxybutyrate-co-3-hydroxyvalerate) solution has a certain influence on the particle size and morphology of the prepared PHBV microspheres. By controlling the concentration of poly(3-hydroxybutyrate-co-3-hydroxyvalerate) solution, PHBV microspheres of different sizes can be obtained. Among them, the PHBV microspheres prepared when the concentration of poly(3-hydroxybutyrate-co-3-hydroxyvalerate) solution is 5~15% have better quality.

[0020] Preferably, the temperature of the polysorbate-80 aqueous solution is 40~80 °C.

[0021] In experiments, this invention found that higher temperatures in the polysorbate-80 aqueous solution resulted in better morphology, greater dispersion, and smaller particle size of the formed PHBV microspheres. This may be related to the surface tension of the polysorbate-80 aqueous solution; as temperature increases, the surface tension decreases, which is more conducive to the formation and stability of PHBV microspheres. Therefore, this invention uses a polysorbate-80 aqueous solution temperature of 40-80°C. Similarly, at a constant temperature, appropriately increasing the surfactant concentration results in more stable PHBV microspheres with smaller particle sizes.

[0022] Preferably, the concentration of the polysorbate-80 aqueous solution is 0.2-4% by weight.

[0023] Preferably, the stirring speed in step (2) is 300~1200 rpm.

[0024] Preferably, the size of the PHBV microspheres is 48~365 μm.

[0025] Secondly, the present invention provides PHBV microspheres, which are prepared by the preparation method described above.

[0026] Thirdly, the present invention provides the application of PHBV microspheres prepared by the above-described preparation method or the above-described PHBV microspheres in daily chemical products.

[0027] This application has the following beneficial effects: (1) This invention uses a green solvent to dissolve PHBV and uses a solvent exchange method to prepare PHBV microbeads with controllable particle size. The entire preparation method is green and simple. Even when the PHBV concentration is as high as 15 wt%, high-quality PHBV microbeads can be obtained, which is expected to realize large-scale production of PHBV microbeads. (2) The PHBV microbeads prepared in this invention can degrade in the presence of microorganisms, but remain stable in the absence of microorganisms, that is, they have a stable shelf life under sterile conditions and are eco-friendly. (3) The PHBV microbeads prepared in this invention have a smooth surface and a regular spherical shape. Compared with commercial MCC and PE particles, the PHBV microbeads in this invention exhibit excellent cleansing ability for the skin. Attached Figure Description

[0028] Figure 1 The images show the microscopic images and size distribution of the PHBV microbeads in Example 1.

[0029] Figure 2 The images show the microscope images and size distribution of the PHBV microbeads in Example 2.

[0030] Figure 3 The images show the microscopic images and size distribution of the PHBV microbeads in Example 3.

[0031] Figure 4 The images show the microscope images and size distribution of the PHBV microbeads in Example 4.

[0032] Figure 5 The images show the microscope images and size distribution of the PHBV microbeads in Example 5.

[0033] Figure 6 The images show the microscope images and size distribution of the PHBV microbeads in Example 6.

[0034] Figure 7 The images show the microscope images and size distribution of the PHBV microbeads in Example 7.

[0035] Figure 8 The images show the microscope images and size distribution of the PHBV microbeads in Example 8.

[0036] Figure 9 The images show the microscope images and size distribution of the PHBV microbeads in Example 9.

[0037] Figure 10 Microscopic images and size distribution of PHBV microbeads in Example 10.

[0038] Figure 11 The images show the microscopic images and size distribution of the PHBV microbeads in Example 11.

[0039] Figure 12 The images show the microscope images and size distribution of the PHBV microbeads in Example 12.

[0040] Figure 13 The images show the microscope images and size distribution of the PHBV microbeads in Example 13.

[0041] Figure 14 The image shows a microscope image and size distribution of the PHBV microbeads in Example 14.

[0042] Figure 15 The image shows a microscope image and size distribution of the PHBV microbeads in Example 15.

[0043] Figure 16 The image shows a microscope image and size distribution of the PHBV microbeads in Example 16.

[0044] Figure 17 The image shows a microscope image and size distribution of the PHBV microbeads in Example 17.

[0045] Figure 18 This is a microscope image of the PHBV microbeads in Example 18.

[0046] Figure 19 This is a microscope image of the PHBV microbeads in Example 19.

[0047] Figure 20 This is a microscope image of the PHBV microbeads in Example 20.

[0048] Figure 21 This is a SEM image of the PHBV microbeads in Example 1.

[0049] Figure 22 This is a SEM image of the PHBV microbeads in Example 21.

[0050] Figure 23 This is a SEM image of the PHBV microbeads in Example 22.

[0051] Figure 24 The cleaning efficiency of detergents containing microbeads, PHBV microbeads, MCC particles, and PE particles on skin dirt was compared.

[0052] Figure 25 SEM images of PHBV microbeads after degradation in activated sludge aqueous solution (a) and seawater (b). Detailed Implementation

[0053] The present invention will be further described below with reference to the accompanying drawings and specific embodiments. Those skilled in the art will be able to implement the present invention based on these descriptions. Furthermore, the embodiments of the present invention described below are generally only some, not all, of the embodiments of the present invention. Therefore, all other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort should fall within the scope of protection of the present invention.

[0054] Example 1: Preparation of PHBV microbeads 0.12 g of PHBV was dissolved in 0.88 g of isosorbide dimethyl ether at 80 °C to obtain a 5 wt% PHBV solution. The hot PHBV solution was then added dropwise at a rate of 10 s / drop to 25 g of 1 wt% polysorbate-80 aqueous solution at 80 °C, while continuously stirring at 500 rpm. PHBV microspheres formed instantly upon the addition of the antisolvent to the polymer solution. Subsequently, the good solvent inside the microspheres exchanged with the external antisolvent, and the PHBV microspheres gradually solidified. The solidified microspheres were filtered through a filter screen, washed several times with deionized water, and finally freeze-dried to collect the microspheres. All microspheres were spherical with a size of approximately 82 μm. Their microscopic images and size distribution are shown in the figure below. Figure 1 As shown, the SEM image is as follows Figure 21 As shown.

[0055] Example 2: Preparation of PHBV microbeads The difference between this embodiment and Example 1 is that the PHBV solution concentration is 9 wt%. The microbeads are all spherical, with a size of approximately 111 μm, and their microscopic images and size distribution are as follows. Figure 2 As shown.

[0056] Example 3: Preparation of PHBV microbeads The difference between this embodiment and Example 1 is that the PHBV solution concentration is 12 wt%. The microbeads are all spherical, with a size of approximately 142 μm, and their microscopic images and size distribution are as follows. Figure 3 As shown.

[0057] Example 4: Preparation of PHBV microbeads The difference between this embodiment and Example 1 is that the PHBV solution concentration is 15 wt%. The microbeads are all spherical, with a size of approximately 365 μm, and their microscopic images and size distribution are as follows. Figure 4 As shown.

[0058] Example 5: Preparation of PHBV microbeads The difference between this embodiment and Example 1 is that the PHBV solution concentration is 12 wt% and the stirring speed is 300 rpm. The microspheres are all spherical, with a size of approximately 258 μm, and their microscopic images and size distribution are as follows. Figure 5 As shown.

[0059] Example 6 Preparation of PHBV microbeads The difference between this embodiment and Example 5 is that the stirring speed is 500 rpm. The microspheres are all spherical, with a size of approximately 122 μm, and their microscopic images and size distribution are as follows. Figure 6 As shown.

[0060] Example 7 Preparation of PHBV microbeads The difference between this embodiment and Example 5 is that the stirring speed is 900 rpm. The microspheres are all spherical, with a size of approximately 69 μm, and their microscopic images and size distribution are as follows. Figure 7 As shown.

[0061] Example 8: Preparation of PHBV microbeads The difference between this embodiment and Example 5 is that the stirring speed is 1200 rpm. The microspheres are all spherical, with a size of approximately 48 μm, and their microscopic images and size distribution are as follows. Figure 8 As shown.

[0062] Example 9 Preparation of PHBV microbeads The difference between this embodiment and Example 1 is that the PHBV solution concentration is 12 wt% and the polysorbate-80 aqueous solution concentration is 0.2 wt%. The microbeads are all spherical, with a size of approximately 217 μm, and their microscopic images and size distribution are as follows. Figure 9 As shown.

[0063] Example 10 Preparation of PHBV microbeads The difference between this example and Example 9 is that the concentration of the polysorbate-80 aqueous solution is 0.5 wt%. The microbeads are all spherical, with a size of approximately 181 μm, and their microscopic images and size distribution are as follows. Figure 10 As shown.

[0064] Example 11 Preparation of PHBV microbeads The difference between this example and Example 9 is that the concentration of the polysorbate-80 aqueous solution is 2 wt%. The microspheres are all spherical, with a size of approximately 140 μm, and their microscopic images and size distribution are as follows. Figure 11 As shown.

[0065] Example 12 Preparation of PHBV microbeads The difference between this example and Example 9 is that the concentration of the polysorbate-80 aqueous solution is 4 wt%. The microspheres are all spherical, with a size of approximately 85 μm, and their microscopic images and size distribution are as follows. Figure 12 As shown.

[0066] Example 13 Preparation of PHBV microbeads The difference between this embodiment and Example 1 is that 0.12 g of PHBV was dissolved in 0.88 g of propylene carbonate at 80 °C to obtain a 12 wt% PHBV solution. The microbeads are all spherical, with a size of approximately 70 μm, and their microscopic images and size distribution are as follows. Figure 13 As shown.

[0067] Example 14 Preparation of PHBV microbeads The difference between this embodiment and Example 1 is that 0.12 g of PHBV was dissolved in 0.88 g of divalent ester (DBE) at 80 °C to obtain a 12 wt% PHBV solution. The microbeads are all spherical, with a size of approximately 97 μm, and their microscopic images and size distribution are as follows. Figure 14 As shown.

[0068] Example 15 Preparation of PHBV microbeads The difference between this embodiment and Example 1 is that 0.12 g of PHBV was dissolved in 0.88 g of dimethyl adipate at 80 °C to obtain a 12 wt% PHBV solution. The microbeads are all spherical, with a size of approximately 114 μm, and their microscopic images and size distribution are as follows. Figure 15 As shown.

[0069] Example 16 Preparation of PHBV microbeads The difference between this embodiment and Example 1 is that 0.12 g of PHBV was dissolved in 0.88 g of methyl lactate at 80 °C to obtain a 12 wt% PHBV solution. The microbeads are all spherical, with a size of approximately 113 μm, and their microscopic images and size distribution are as follows. Figure 16 As shown.

[0070] Example 17 Preparation of PHBV microbeads The difference between this embodiment and Example 1 is that 0.12 g of PHBV was dissolved in 0.88 g of dipropylene glycol methyl ester at 80 °C to obtain a 12 wt% PHBV solution. The microbeads were all spherical, with a size of approximately 112 μm, and their microscopic images and size distribution are shown below. Figure 17 As shown, it does not dissolve as well as other solvents and produces lumpy aggregates.

[0071] Example 18 Preparation of PHBV microbeads The difference between this embodiment and Example 1 is that the temperature of the polysorbate-80 aqueous solution is 40 °C. The microbeads are all spherical, and their microscopic images are as follows. Figure 18 As shown.

[0072] Example 19 Preparation of PHBV microbeads The difference between this embodiment and Example 1 is that the temperature of the polysorbate-80 aqueous solution is 50 °C. The microbeads are all spherical, and their microscopic images are as follows. Figure 19 As shown.

[0073] Example 20: Preparation of PHBV microbeads The difference between this embodiment and Example 1 is that the temperature of the polysorbate-80 aqueous solution is 60 °C. The microbeads are all spherical, and their microscopic images are as follows. Figure 20 As shown.

[0074] Comparative Example 1 The SEM image of the MCC microbeads used in the product is as follows: Figure 22 As shown.

[0075] Comparative Example 2 The SEM image of the PE microbeads used in the product is as follows: Figure 23 As shown.

[0076] [Performance Testing] 1. The cleaning efficiency of detergents without microbeads, detergents containing PHBV microbeads, detergents containing MCC particles, and detergents containing PE particles on skin dirt was tested. Since the inner forearm is flat and hairless, it was chosen as the test substrate. The detergent consisted of 30 mg of microbeads and 4 mL of commercial liquid soap without microbeads. Results are as follows: Figure 24As shown in the figure. In this test, the exfoliating product containing PHBV microbeads showed excellent cleaning efficiency, requiring approximately 94 seconds to completely remove contaminants, while commercial soaps without microbeads (164 seconds), commercial MCC particles (105 seconds), and PE particles (115 seconds) had slower cleaning efficiency.

[0077] 2. Test the degradation performance of PHBV microspheres in aquatic media containing microorganisms such as activated sludge and seawater, such as... Figure 25 The images shown are SEM images of PHBV microbeads after degradation in activated sludge aqueous solution (a) and seawater (b), respectively, after 150 days with or without microorganisms (control). 50X and 2.5KX represent magnification.

[0078] Scanning electron microscopy revealed that PHBV microbeads became porous and rough on the surface after 150 days of degradation in activated sludge and seawater, while those in culture medium remained smooth. This indicates that the degradation of PHBV microbeads in a microbial-free aqueous medium is negligible, implying a stable shelf life under sterile conditions. In summary, the results demonstrate that PHBV microbeads degrade in the presence of microorganisms but remain stable in the absence of microorganisms.

Claims

1. A method for preparing PHBV microbeads, characterized by, Includes the following steps: (1) Dissolve poly(3-hydroxybutyrate-co-3-hydroxyvalerate) in a green solvent to obtain a poly(3-hydroxybutyrate-co-3-hydroxyvalerate) solution; (2) The poly(3-hydroxybutyrate-co-3-hydroxyvalerate) solution was added to the polysorbate-80 aqueous solution and stirred continuously. After solvent exchange, the cured PHBV microbeads were obtained. (3) The cured PHBV microbeads are filtered and washed, and then freeze-dried to obtain the PHBV microbeads; The green solvent includes one or more of isosorbide dimethyl ether, propylene carbonate, divalent ester, dimethyl adipate, and methyl lactate. The temperature of the poly(3-hydroxybutyrate-co-3-hydroxyvalerate) solution is greater than or equal to 80°C, and the temperature of the polysorbate-80 aqueous solution is 40~80°C.

2. The method for preparing PHBV microspheres as described in claim 1, characterized in that, The hydroxyvalerate content of the poly(3-hydroxybutyrate-co-3-hydroxyvalerate) is 18~28 mol%.

3. In the method for preparing PHBV microbeads as described in claim 1 or 2, the concentration of the poly(3-hydroxybutyrate-co-3-hydroxyvalerate) solution is 5-15% by weight.

4. In the method for preparing PHBV microbeads as described in claim 1, the concentration of the polysorbate-80 aqueous solution is 0.2-4% by weight.

5. The method for preparing PHBV microspheres as described in claim 1, characterized in that, The stirring speed in step (2) is 300~1200 rpm.

6. The method for preparing PHBV microbeads according to claim 1 or 5, wherein, The size of the PHBV microspheres is 48~365 μm.