LED epitaxial structure with stress release layer and growth method thereof
Through the cyclic growth and high-temperature treatment of the InGaN/pause layer/GaN SL structure, a multi-layer stacked Pits layer is formed, which solves the problem of poor lattice quality and dislocation in the stress release layer structure of the LED epitaxial wafer, and improves the luminous efficiency and current diffusion. Effect.
Patent Information
- Application Number
- CN202311844706.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-29
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-12-29
AI Technical Summary
The stress relief layer structure of existing LED epitaxial wafers has structural defects such as poor lattice quality, dislocations, and pores during the growth process, resulting in low luminous efficiency, and the Pits layer grown at low temperature is difficult to effectively annihilate the dislocations derived from the bottom layer, affecting MQW The lattice quality of the layer and the current spreading effect.
Using the InGaN/pause layer/GaN SL structure, the InGaN layer is baked at high temperature to cause In atoms to precipitate or escape to form vacancy Pits, blocking dislocations derived from the bottom layer, and through cyclic growth to generate multi-layer superimposed Pits layers to improve the quality of the upper lattice and current spreading effects.
It effectively improves the luminous efficiency and anti-static ability of LED, improves the polarization effect, reduces the compressive stress of the MQW layer, and improves the lattice quality and current passing ability.
Smart Images

Figure CN117650210B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of LED chips, and in particular relates to an LED epitaxial structure with a stress release layer and a growth method thereof. Background Art
[0002] White light LEDs have replaced traditional lighting and become the preferred method for general indoor and outdoor lighting. How to improve the luminous efficiency of light-emitting diodes (LEDs) has become an important issue that needs to be addressed. Due to the properties of the material itself, mismatch stress in the epitaxial layer will introduce structural defects such as dislocations, stacking faults, and pores, which will deteriorate the crystal quality and reduce the luminous efficiency. How to improve the quality of epitaxial structure crystals has become an important issue in improving the luminous efficiency of LEDs.
[0003] In the prior art, stress release layers are used in LED epitaxial wafers to prevent dislocations derived from the bottom layer and reduce compressive stress by doping Al / In. However, the In / Al and GaN lattice are highly compatible, and the polarization effect becomes larger, which reduces the lattice quality of the MQW layer grown on it and affects the luminous efficiency. Secondly, the traditional stress release layer forms Pits (voids) by growing GaN at low temperature, so that the stress disappears at the pits, and the defects are merged into the pits. However, the pits generated at low temperature will continue to grow, and cannot effectively annihilate the dislocations derived from the bottom layer, and even derive to the MQW light-emitting layer, affecting the lattice quality of the MQW layer and reducing the luminous efficiency. Thirdly, the low-temperature growth of GaN opens the pits layer, and the lattice quality of the grown GaN layer is poor, and the generated V-shaped pits are not easy to fill, and the thickness of the pits is high, which is not conducive to the passage of large currents. Therefore, we urgently need to optimize the existing LED epitaxial wafer stress release layer structure and preparation method, and obtain a structure with relatively good lattice quality, few defects and small stress before growing the MQW light-emitting layer, improve the current diffusion effect, and facilitate the passage of large currents, thereby improving the light efficiency. Summary of the invention
[0004] In view of the deficiencies in the background technology, the present invention provides an LED epitaxial structure with a stress release layer, in which an InGaN / pause layer / GaN SL structure (cyclic growth structure) is grown in the stress release layer, and the InGaN layer is baked at a high temperature using the pause layer to cause In to precipitate or escape to form vacant pits, further blocking dislocations derived from the bottom layer. The structure grows cyclically to generate multi-layer superimposed pits, which is beneficial to stress release and improves the quality of the upper lattice. The structure also has a good current diffusion effect and is beneficial to the passage of large currents, thereby improving the light efficiency.
[0005] To achieve the above purpose, the technical solution of the present invention is as follows:
[0006] An LED epitaxial structure with a stress release layer, characterized in that it includes a substrate, and a buffer layer, a UGaN layer, an NGaN layer, a stress release layer, an MQW layer, an EBL layer and a P layer grown sequentially on the substrate, wherein the stress release layer is a periodic composite layer composed of repeated overlapping InGaN layers, pause layers and GaN cap layers grown sequentially from bottom to top.
[0007] Preferably, the number of repeated overlapping cycles of the stress release layer is 3-10.
[0008] Preferably, the stop layer comprises a first stop layer and a second stop layer, the first stop layer is grown under conditions without NH3, and the second stop layer is grown under conditions with NH3.
[0009] Preferably, the substrate is a PSS substrate plated with AlN, the buffer layer has a thickness of 180-220 Å, the UGaN layer has a thickness of 3-4 μm, and the NGaN layer has a thickness of 1-2 μm.
[0010] Preferably, the thickness of the InGaN layer in the stress release layer is 10-50 Å, and the thickness of the GaN capping layer is 100-400 Å.
[0011] A method for growing an LED epitaxial structure with a stress release layer is used to manufacture the above-mentioned LED epitaxial structure with a stress release layer. The specific method includes providing a substrate, and sequentially growing a buffer layer, a UGaN layer, an NGaN layer, a stress release layer, an MQW layer, an EBL layer and a P layer on the surface of the substrate. It is characterized in that the growth method of the stress release layer is to periodically grow an InGaN layer, a first pause layer, a second pause layer and a GaN cap layer in sequence.
[0012] Preferably, the growth conditions of the InGaN layer in the stress release layer are: N2: 120-150SLM, H2: 0SLM, NH3: 150-120SLM, pressure P=200Torr; rotation speed: 600Rmp; Temp=750-780°.
[0013] Preferably, the growth conditions of the first pause layer in the stress release layer are: N2: 0-150SLM, H2: 120-270SLM (N2 / NH3=0 is a pure H2 environment), NH3: 0SLM, pressure P=200Torr, rotation speed: 600Rmp; Temp= 900-1200°, no Mo source is introduced, and the time is 30-120s;
[0014] Preferably, the growth conditions of the second pause layer in the stress release layer are: N2: 120-150SLM, H2: 0SLM, NH3: 150-120 SLM, pressure P=200Torr, rotation speed: 600Rmp; Temp=900-1200° without Mo source introduction, time is 10-50s.
[0015] Preferably, the growth conditions of the GaN cap layer in the stress release layer are: N2: 120-150 SLM, H2: 0SLM, NH3: 150-120SLM, pressure P=200Torr; rotation speed: 600Rmp; Temp=900-1200°, and TMG / TEGa is introduced to grow a GaN stacking layer with a thickness of 100~400A.
[0016] Compared with the prior art, the present invention has the following beneficial effects:
[0017] (1) The present invention uses high temperature to cause In to precipitate or escape to form vacancies, thereby further blocking dislocations derived from the bottom layer;
[0018] (2) In the present invention, due to high temperature, In precipitates or escapes to generate vacancies Pits, which greatly improves the polarization effect, reduces the compressive stress of the MQW layer grown thereon, improves the lattice quality, and is beneficial to current expansion, thereby improving the luminescence efficiency;
[0019] (3) In the stress release layer of the present invention, InGaN / pause layer / GaN grow cyclically to generate a multi-layer superimposed Pits layer with good current diffusion effect and conducive to the passage of large current, thereby improving the light efficiency and anti-static ability. In addition, a single layer of Pits has a small opening and few derived dislocations, which has a positive effect on the lattice quality of the subsequently grown MQW layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Other features, objectives and advantages of the present invention will become more apparent from a reading of the detailed description of non-limiting embodiments made with reference to the following accompanying drawings.
[0021] Figure 1 This is a schematic diagram of an LED epitaxial structure with a stress release layer according to the present invention;
[0022] Figure 2 Schematic diagram of the vacancy Pits generation process of the stress release layer of the present invention using the InGaN / pause layer / GaN SL structure.
[0023] In the figure: 1. substrate, 2. buffer layer, 3. UGaN layer, 4. NGaN layer, 5. stress release layer, 501. InGaN layer, 502. first stop layer, 503. second stop layer, 504. GaN cap layer, 6. MQW layer, 7. EBL layer, 8. P layer. DETAILED DESCRIPTION
[0024] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0025] Example
[0026] An LED epitaxial structure with a stress release layer comprises a substrate, and a buffer layer, a UGaN layer, a NGaN layer, a stress release layer, an MQW layer, an EBL layer and a P layer grown sequentially on the substrate, wherein the stress release layer is a periodic composite layer composed of repeated overlapping of an InGaN layer, a pause layer and a GaN cap layer grown sequentially from bottom to top, and the number of repeated overlapping periods of the stress release layer is 3-10, wherein the pause layer comprises a first pause layer and a second pause layer, wherein the growth conditions of the first pause layer do not contain NH3, and the growth conditions of the second pause layer contain NH3.
[0027] A method for growing an LED epitaxial structure with a stress release layer, which is used to make the LED epitaxial structure with the stress release layer, comprises providing a PSS substrate plated with AlN, and sequentially growing a buffer layer with a thickness of 180-220A, a UGaN layer with a thickness of 3-4μm, and a NGaN layer with a thickness of 1-2μm (doped with SI) on the surface of the substrate. N-type GaN layer, concentration is 2E19), stress release layer, MQW layer, EBL layer and P layer. The methods of growing buffer layer, UGaN layer, NGaN layer, MQW layer, EBL layer and P layer are all existing conventional technologies and will not be repeated here. In this embodiment, the growth method of the stress release layer is to periodically grow an InGaN layer with a thickness of 10-50A, a first pause layer, a second pause layer and a GaN cap layer with a thickness of 100-400A in sequence; the structure (InGaN / pause layer / GaN) is periodically cycled 3-10 times to finally form a multi-level three-dimensional structure of the Pits layer to release stress, which is beneficial to current diffusion, improving light efficiency and stress release.
[0028] The growth conditions of the InGaN layer in the stress release layer are: N2: 120-150SLM, H2: 0SLM, NH3: 150-120SLM, pressure P = 200Torr; rotation speed: 600Rmp; Temp = 750-780°, the InGaN (highly doped In) layer releases stress and annihilates dislocations;
[0029] The growth conditions of the first pause layer in the stress release layer are: N2: 0-150SLM, H2: 120-270SLM (N2 / NH3=0 is pure H2 environment), NH3: 0SLM, pressure P=200Torr, rotation speed: 600Rmp; Temp= 900-1200°, no Mo source is introduced, the time is 30-120s, there is no NH3 in the first pause layer, and the GaN (InGaN) decomposition equilibrium is broken under the condition of no NH3 (the original reaction is TEGa+NH3+TMIn to generate InGaN+others, NH3 is a reactant, and the reduction will make the reversible equilibrium proceed like the left side; and at high temperature, TEGa / TMIn decomposes into atoms, so that the surface In atoms gather and precipitate (which will block the Pits mouth and annihilate dislocations), and the InGaN on the right is decomposed, and In escapes to form holes to release stress and annihilate dislocations), so that In atoms precipitate or escape to form Pits (holes), release stress, and annihilate dislocations;
[0030] The growth conditions of the second pause layer in the stress release layer are: N2: 120-150SLM, H2: 0SLM, NH3: 150-120SLM, pressure P = 200Torr, rotation speed: 600Rmp; Temp = 900-1200° without Mo source introduction, time is 10-50s, and the second pause layer obtains a steep and flat interface through atomic rearrangement.
[0031] The growth conditions of the GaN cap layer in the stress release layer are: N2: 120-150 SLM, H2: 0SLM, NH3: 150-120SLM, pressure P=200Torr; rotation speed: 600Rmp; Temp=900-1200°, TMG / TEGa is introduced to grow a GaN crystal layer with a thickness of 100~400A, and the GaN cap layer forms bonds with the remaining GaN after In precipitation or escape, thereby annihilating unnecessary dislocations.
[0032] The following is a detailed description of the process of generating vacancies Pits in the stress release layer (such as Figure 2 shown):
[0033] (1) The first layer of the stress release layer is an InGaN layer. Due to the different lattice constants, dislocations will occur between the InGaN layer and the GaN layer below it, such as Figure 2 A dislocation is formed at A in the middle;
[0034] (2) The high-temperature pause layer on the InGaN layer causes part of the In in the InGaN layer to escape or precipitate, leaving GaN, reducing the polarization effect at A;
[0035] (3) A GaN capping layer is grown at high temperature on the pause layer, and GaN forms a bond at position A, thereby eliminating the dislocation at position A.
[0036] (4) When an InGaN layer is grown on top, some dislocations are filled by the InGaN layer, causing the dislocations to disappear or change direction;
[0037] (5) In this cyclic growth, vacancy pits appear due to the escape or precipitation of In atoms. The polarization effect around the precipitated In atoms reduces the annihilation of some dislocations, and ultimately reduces the dislocations derived from the MQW layer, improving the lattice quality of the MQW layer. The vacancy pits formed are three-dimensional, which is more conducive to current expansion and improves the luminescence efficiency.
[0038] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention.
Claims
1. An LED epitaxial structure with a stress release layer, characterized in that: The invention comprises a substrate, and a buffer layer, a UGaN layer, a NGaN layer, a stress release layer, a MQW layer, an EBL layer and a P layer which are sequentially grown on the substrate. The stress release layer is a periodic composite layer composed of repeated overlapping InGaN layers, pause layers and GaN cap layers which are sequentially grown from bottom to top. The pause layers comprise a first pause layer and a second pause layer. The growth conditions of the first pause layer do not contain NH3, and the growth conditions of the second pause layer contain NH3.
2. The LED epitaxial structure with a stress release layer according to claim 1, characterized in that: The number of repeated overlapping cycles of the stress release layer is 3-10.
3. The LED epitaxial structure with a stress release layer according to claim 1, characterized in that: The substrate is a PSS substrate plated with AlN, the buffer layer has a thickness of 180-220 Å, the UGaN layer has a thickness of 3-4 μm, and the NGaN layer has a thickness of 1-2 μm.
4. The LED epitaxial structure with a stress release layer according to claim 1, characterized in that: The thickness of the InGaN layer in the stress release layer is 10-50A, and the thickness of the GaN cap layer is 100-400A.
5. A method for growing an LED epitaxial structure with a stress release layer, for manufacturing the LED epitaxial structure with a stress release layer according to any one of claims 1 to 4, the method comprising providing a substrate, and sequentially growing a buffer layer, a UGaN layer, a NGaN layer, a stress release layer, a MQW layer, an EBL layer and a P layer on the surface of the substrate, characterized in that: The stress release layer is grown by periodically and sequentially growing an InGaN layer, a first pause layer, a second pause layer and a GaN cap layer.
6. A method for growing an LED epitaxial structure with a stress release layer as claimed in claim 5, characterized in that: The growth conditions of the InGaN layer in the stress release layer are: N2: 120-150SLM, H2: 0SLM, NH3: 150-120SLM, pressure P=200Torr; Speed: 600Rmp; Temp=750-780°.
7. A method for growing an LED epitaxial structure with a stress release layer as claimed in claim 5, characterized in that: The growth conditions of the first pause layer in the stress release layer are: N2: 0-150SLM, H2: 120-270SLM, NH3: 0SLM, pressure P=200Torr, rotation speed: 600Rmp; Temp = 900-1200°, no Mo source input, time is 30-120s.
8. The method for growing an LED epitaxial structure with a stress release layer according to claim 5, characterized in that: The growth conditions of the second pause layer in the stress release layer are: N2: 120-150 SLM, H2: 0 SLM, NH3: 150-120 SLM, pressure P=200 Torr, rotation speed: 600 Rmp; Temp = 900-1200°, no Mo source input, time is 10-50s.
9. The method for growing an LED epitaxial structure with a stress release layer according to claim 5, characterized in that: The growth conditions of the GaN cap layer in the stress release layer are: N2: 120-150 SLM, H2: 0 SLM, NH3: 150-120 SLM, pressure P = 200 Torr; Speed: 600Rmp; Temp=900-1200°, TMG / TEGa is introduced to grow a GaN stacking layer with a thickness of 100~400A.
Citation Information
Patent Citations
GaN-based light-emitting diode epitaxial structure and preparation method thereof
CN104051586A
Novel GaN-based LED epitaxial layer structure and preparation method thereof
CN109888071A
LED epitaxial structure and preparation method thereof
CN114551663A
Epitaxy Technique for Reducing Threading Dislocations in Stressed Semiconductor Compounds
US20130193480A1