A method for preparing polyamide hollow fiber membrane by thermally induced phase separation
By adding polystyrene nanoparticles to the polyamide film and using thermoform phase separation technology to regulate the porosity and phase change rate of the film, the problem of low separation accuracy of traditional polyamide films is solved, and efficient organic solvent separation application is achieved .
Patent Information
- Application Number
- CN202311731584.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-15
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-12-15
AI Technical Summary
Traditional polyamide films have a problem of low separation accuracy during solution forming and cannot meet the needs of high-precision separation applications in the petroleum and chemical industries.
By adding late-dissolvable polystyrene nanoparticles with adjustable pore size, the porosity of the polyamide is regulated, and the phase change rate inside and outside the membrane surface is precisely regulated by using thermo-induced phase separation technology to obtain a separation cortex with high separation accuracy.
It realizes the efficient separation application of polyamide hollow fiber membrane in organic solvent systems, and improves the separation accuracy and solvent resistance of the membrane.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of membrane technology, and in particular relates to a method for preparing a polyamide hollow fiber membrane by thermally induced phase separation. Background Art
[0002] The petrochemical and pharmaceutical industries are one of the pillar industries of the national economy. In these industries, the separation and purification of materials, drug purification and refining, solvent recovery and other processes mainly use traditional distillation, rectification, crystallization and other methods, which consume a lot of energy and are costly, usually accounting for 40-70% of the total investment and energy costs (Nature, 532 (2016) 435-437; Nat.Mater., 16 (2017) 276-279). Membrane separation technology is a new technology that does not involve phase change and can use simple physical screening to separate substances with high precision. It has made a significant contribution to water resource recycling and seawater desalination. It is a general trend to apply membrane separation technology to the separation and purification of materials in organic solvent systems, reduce energy consumption and achieve sustainable development. However, unlike the application in water systems, when used in organic solvents, membrane materials must not only have high permeation separation characteristics, but also strong solvent resistance. Polyamide (PA) is a polymer material with excellent performance, which has the characteristics of high toughness, high strength, low friction coefficient, excellent impact resistance, good chemical stability (resistance to seawater, solvents, oils), etc. However, due to the high heat resistance and solvent resistance of this type of polymer, it is difficult to process it into a film by solution molding. At present, all polyamide films are prepared by melt injection molding. However, the film stretched after melt extrusion has a low separation accuracy and cannot adapt to the high-precision separation applications in the current petroleum, chemical industry, and pharmaceutical industry. Summary of the invention
[0003] In view of the above-mentioned problems existing in the prior art, the purpose of the present invention is to design a technical solution for a method for preparing a polyamide hollow fiber membrane by thermally induced phase separation, wherein the porosity of the polyamide is regulated by adding polystyrene nanoparticles with adjustable pore size that can be dissolved later, so that the membrane has high permeability; further, the phase change rate of the inner and outer surfaces of the membrane is precisely controlled to obtain a separation cortex with high separation accuracy, thereby making the membrane have good separation accuracy, so as to realize the efficient separation application of the membrane in an organic solvent system.
[0004] The method for preparing a polyamide hollow fiber membrane by thermally induced phase separation is characterized by comprising the following steps:
[0005] 1) Dissolving 20-40 parts of polyamide in 40-70 parts of diluent at 200-250° C., adding 10-20 parts of porogenic particles after the polyamide is uniformly dissolved, continuing to dissolve, and then degassing online to obtain a casting solution; the diluent is at least one of dimethyl sulfone, cyclopentane sulfone, maleic anhydride, 4-phenyl benzophenone, vinyl carbonate, propylene carbonate, tetramethyl sulfone, polyethylene glycol, and polyethylene glycol dimethyl ether; the porogenic particles are polystyrene particles cross-linked with divinylbenzene;
[0006] 2) Extruding the above-mentioned casting liquid and core liquid through a spinneret into a hollow fiber membrane embryo, passing through an air bath section, and then entering a cooling bath to undergo phase separation and solidification to obtain a hollow fiber membrane filament; the cooling bath is one of a mixture of 5-15 parts of polyethylene glycol and 85-95 parts of polypropylene glycol, a mixture of 15-25 parts of glycerol and 75-85 parts of 1-octanol, and a mixture of 25-35 parts of diethylene glycol and 65-75 parts of triethylene glycol;
[0007] 3) The obtained hollow fiber membrane is placed in water for cleaning, then placed in an extractant to wash out the diluent, and finally immersed in a solvent to clean the porogenic particles. After cleaning and drying, a polyamide hollow fiber membrane is obtained.
[0008] The method for preparing polyamide hollow fiber membrane by thermally induced phase separation is characterized in that in step 1), the dissolution temperature is 220-230°C, the polyamide is 25-35 parts, the diluent is 50-60 parts, and the porogenic particles are 14-16 parts.
[0009] The method for preparing a polyamide hollow fiber membrane by thermally induced phase separation is characterized in that in step 1), the polyamide is one of polyamide 6, polyamide 66, polyamide 10, and polyamide 1010, and has a molecular weight of 15,000-30,000, preferably 20,000-25,000.
[0010] The method for preparing a polyamide hollow fiber membrane by thermally induced phase separation is characterized in that in step 1): the porogenic particles are polystyrene particles cross-linked with divinylbenzene, and the content of divinylbenzene is 5-15% of the polystyrene particles, preferably 8-12%; the particle size of the particles is 50-200 nanometers, preferably 80-150 nanometers; the dissolution time of the porogenic particles is 20 minutes to 2 hours, preferably 40 minutes to 1.5 hours, and more preferably 1 hour to 1.2 hours.
[0011] The method for preparing polyamide hollow fiber membrane by thermally induced phase separation is characterized in that in step 2), the inner hole diameter of the spinneret is 0.8-1.2 mm, the extrusion diameter of the polyamide liquid is 1.6-2.0 mm, and the size of the slit is controlled to be no less than 0.4 mm.
[0012] The method for preparing a polyamide hollow fiber membrane by thermally induced phase separation is characterized in that in step 2), the extrusion core liquid is at least one of polyethylene glycol 200, polyethylene glycol 300, polyethylene glycol 400, and polyethylene glycol 600.
[0013] The method for preparing a polyamide hollow fiber membrane by thermally induced phase separation is characterized in that in step 2): the cooling bath is one of a mixture of 10 parts of polyethylene glycol and 90 parts of polypropylene glycol, a mixture of 20 parts of glycerol and 80 parts of 1-octanol, and a mixture of 30 parts of diethylene glycol and 70 parts of triethylene glycol; the temperature of the cooling bath is -10-10°C, preferably -5-5°C, and more preferably -2-2°C.
[0014] The method for preparing a polyamide hollow fiber membrane by thermally induced phase separation is characterized in that in step 2), the length of the air bath section is 2-20 cm, preferably 5-15 cm, and more preferably 8-10 cm.
[0015] The method for preparing a polyamide hollow fiber membrane by thermally induced phase separation is characterized in that in step 3), the extractant is at least one of ethanol, ethyl acetate and methanol at 50°C-60°C, and the temperature is preferably 54°C-56°C.
[0016] The method for preparing polyamide hollow fiber membrane by thermally induced phase separation is characterized in that in step 3), the porogenic particle cleaning solvent is at least one of toluene, xylene, chloroform, styrene, carbon tetrachloride, and methyl ethyl ketone.
[0017] The thermally induced phase separation method described in the present invention is used to prepare a polyamide hollow fiber membrane. By selecting a suitable diluent to dissolve the polyamide at high temperature to solve its dissolution problem, a casting solution is obtained, which has film-forming properties. The polymers, additives, solvents, and diluents used in the present invention are optimized according to the Hansen interaction theory, focusing on the compatibility of these materials with to prevent the occurrence of defects. In addition, the parameter limits such as the amount of addition, molecular weight, concentration, and type of each component set in the present invention are based on the thermodynamic stability of the polyamide solution as a consideration. Thermodynamic stability is a prerequisite for the preparation of high-performance hollow fiber membranes.
[0018] The present invention utilizes a high-temperature dissolution method of a thermotropic phase to first dissolve it into a uniform solution to achieve extrusion molding. The present invention utilizes divinylbenzene cross-linked polystyrene nanoparticles to regulate the porosity of the polyamide membrane body, solves the problem that traditional inorganic particles are difficult to clean for regulating the porosity of the polyamide membrane, and has significant innovation. As is well known, polyamide materials have excellent solvent resistance and poor acid and alkali resistance. Traditional inorganic nanoparticles, such as silicon dioxide, titanium dioxide, calcium carbonate, etc., need to be cleaned with inorganic acids to obtain a higher porosity. Therefore, they are difficult to use to regulate the porosity of the polyamide membrane. In addition, traditional non-cross-linked organic nanoparticles, such as polystyrene particles prepared by traditional emulsion polymerization, are easily dissolved at high temperatures and are difficult to exert their pore-forming effect. Cross-linked organic nanoparticles, such as cross-linked polyimide particles, are difficult to dissolve, cannot be washed out, and cannot obtain sufficient porosity. The present invention uses divinylbenzene cross-linked polystyrene particles as porogens, and the cross-linking bonds are broken after being treated at high temperature for a certain period of time, so that they can be washed out with a solvent to obtain a rich pore structure. This high temperature treatment time is achieved in the present invention by controlling the dissolution time of the particles in the casting solution. Moreover, according to the different amounts of divinylbenzene used, different dissolution times can be adjusted to adjust the degree of cross-linking bond breaking, thereby adjusting their cleaning effect, obtaining a polyamide membrane with high porosity, and realizing the control of the bulk porosity of the polyamide membrane by nanoparticles.
[0019] The present invention further regulates the pore size of the membrane surface by changing the internal and external cooling baths to give the membrane high separation accuracy. The internal and external cooling baths used in the present invention are solutions or solvents that interact strongly with polyamide but weakly with diluents. In the process of preparing hollow fiber membranes by thermally induced phase separation, in order to achieve the separation accuracy of the membrane, the regulation of the pore structure of the cortex is extremely important. The pore structure is closely related to the concentration of the polymer on the surface. Under normal circumstances, the internal and external cooling baths use solutions or solvents that interact strongly with the diluent but weakly with the polymer, inducing the diluent to enrich on the surface during the molding process to reduce the concentration of the polymer on the surface, so that the pore structure of the cortex of the polymer hollow fiber membrane is in a loose macroporous state and cannot have fine-level separation characteristics. The present invention uses reverse thinking, according to the solubility parameter theory, and uses solutions that interact differently with polyamide and diluents as internal and external cooling baths, respectively, to achieve different degrees of enrichment of the polymer on the internal and external surfaces, so as to regulate the internal and external surface pore structure of the polyamide hollow fiber membrane, thereby achieving its high-precision separation. DETAILED DESCRIPTION
[0020] The present invention is described clearly and completely below in conjunction with specific embodiments. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example 1
[0021] 1) At 200°C, 20 parts of polyamide 6 with a molecular weight of 16,000 were dissolved in 70 parts of dimethyl sulfone. After the polyamide was evenly dissolved, 10 parts of 50 nanometer polystyrene nanoparticles with a divinylbenzene content of 5% were added. The mixture was continued for 2 hours, and then degassing was performed online to obtain a casting solution.
[0022] 2) Using a spinneret with an inner hole diameter of 0.8 mm, an extrusion diameter of 1.6 mm, and a slit size of 0.4 mm, the polyamide 6 casting solution and polyethylene glycol 200 obtained above were extruded into hollow fiber membrane embryos, which passed through a 2 cm air section and entered a mixture of 10% polyethylene glycol and 90% polypropylene glycol at -10°C to induce phase separation and solidify into a hollow fiber membrane filament;
[0023] 3) The obtained polyamide hollow fiber membrane is placed in water for cleaning, and then placed in 60°C ethanol to wash out the diluent, and finally immersed in toluene to clean the porogenic particles. After cleaning and drying, a polyamide hollow fiber membrane product is obtained. Example 2
[0024] 1) At 250°C, 40 parts of polyamide 66 with a molecular weight of 30,000 were dissolved in 40 parts of 4-phenylbenzophenone. After the polyamide was evenly dissolved, 20 parts of 200 nanometer polystyrene nanoparticles with a divinylbenzene content of 15% were added. The mixture was continued for 20 minutes, and then degassing was performed online to obtain a casting solution.
[0025] 2) Using a spinneret with an inner hole diameter of 1.2 mm, an extrusion diameter of 2.0 mm, and a slit size of 0.4 mm, the polyamide 66 casting solution and polyethylene glycol 600 obtained above were extruded into hollow fiber membrane embryos, which passed through an air section of 10 cm and entered a mixture of 30% diethylene glycol and 70% triethylene glycol at 10° C. to induce phase separation and solidify into a hollow fiber membrane filament;
[0026] 3) The obtained polyamide hollow fiber membrane is placed in water for cleaning, and then placed in 50°C ethyl acetate to wash out the diluent, and finally immersed in styrene to clean the porogenic particles. After cleaning and drying, a polyamide hollow fiber membrane product is obtained. Example 3
[0027] 1) At 230°C, 30 parts of polyamide 55 with a molecular weight of 25,000 were dissolved in 55 parts of tetramethyl sulfone. After the polyamide 10 was evenly dissolved, 15 parts of 100 nm polystyrene nanoparticles with a divinylbenzene content of 10% were added. The mixture was continued for 1 hour, and then degassing was performed online to obtain a casting solution.
[0028] 2) Using a spinneret with an inner hole diameter of 0.8 mm, an extrusion diameter of 1.8 mm, and a slit size of 0.5 mm, the polyamide 10 casting solution and polyethylene glycol 400 obtained above were extruded into hollow fiber membrane embryos, which passed through a 20 cm air section and entered a mixture of 20% glycerol and 80% 1-octanol at 0° C. to induce phase separation and solidify into a hollow fiber membrane filament;
[0029] 3) The obtained polyamide hollow fiber membrane is placed in water for cleaning, then placed in 55°C methanol to wash out the diluent, and finally immersed in chloroform to clean the porogenic particles. After cleaning and drying, a polyamide hollow fiber membrane product is obtained. Example 4
[0030] 1) At 215°C, 25 parts of polyamide 1010 with a molecular weight of 20,000 were dissolved in 67 parts of polyethylene glycol dimethyl ether. After the polyamide was evenly dissolved, 8 parts of polystyrene nanoparticles with a size of 80 nanometers and a divinylbenzene content of 8% were added. The mixture was continued for 1.5 hours, and then degassing was performed online to obtain a casting solution.
[0031] 2) Using a spinneret with an inner hole diameter of 1.0 mm, an extrusion diameter of 2.0 mm, and a slit size of 0.5 mm, the polyamide 1010 casting solution and polyethylene glycol 600 obtained above were extruded into hollow fiber membrane embryos, which passed through an air section of 10 cm and entered a mixture of 30% diethylene glycol and 70% triethylene glycol at 5° C. to induce phase separation and solidify into a hollow fiber membrane fiber;
[0032] 3) The obtained polyamide hollow fiber membrane is placed in water for cleaning, and then placed in 60°C ethanol to wash out the diluent, and finally immersed in xylene to clean the porogenic particles. After cleaning and drying, a polyamide hollow fiber membrane product is obtained. Example 5
[0033] 1) At 20°C, 20 parts of polyamide 6 with a molecular weight of 30,000 were dissolved in 60 parts of dimethyl sulfone. After the polyamide was evenly dissolved, 20 parts of polystyrene nanoparticles with a size of 200 nanometers and a divinylbenzene content of 15% were added. The mixture was continued for 2 hours, and then degassing was performed online to obtain a casting solution.
[0034] 2) Using a spinneret with an inner hole diameter of 0.8 mm, an extrusion diameter of 2.0 mm, and a slit size of 0.6 mm, the polyamide 6 casting solution and polyethylene glycol 300 obtained above were extruded into hollow fiber membrane embryos, which passed through an air section of 10 cm and entered a mixture of 30% diethylene glycol and 70% triethylene glycol at 10° C. to induce phase separation and solidify into a hollow fiber membrane filament;
[0035] 3) The obtained polyamide hollow fiber membrane is placed in water for cleaning, and then placed in 50°C methanol to wash out the diluent, and finally immersed in xylene to clean the porogenic particles. After cleaning and drying, a polyamide hollow fiber membrane product is obtained. Example 6
[0036] 1) At 250°C, 40 parts of polyamide 66 with a molecular weight of 30,000 were dissolved in 40 parts of a mixed diluent of dimethyl sulfone and cyclopentane. After the polyamide was evenly dissolved, 20 parts of polystyrene nanoparticles with a 50 nm divinylbenzene content of 10% were added. The mixture was continued for 20 hours, and then degassing was performed online to obtain a casting solution.
[0037] 2) Using a spinneret with an inner hole diameter of 0.8 mm, an extrusion diameter of 1.6 mm, and a slit size of 0.4 mm, the polyamide 66 casting solution and polyethylene glycol 300 obtained above were extruded into hollow fiber membrane embryos, which passed through a 2 cm air section and entered a mixture of 20% glycerol and 80% 1-octanol at -5°C to induce phase separation and solidify into a hollow fiber membrane filament;
[0038] 3) The obtained polyamide hollow fiber membrane is placed in water for cleaning, and then placed in 60°C ethanol to wash out the diluent, and finally immersed in styrene to clean the porogenic particles. After cleaning and drying, a polyamide hollow fiber membrane product is obtained.
[0039] The beneficial effects of the present invention are further demonstrated by corresponding test data below: Tables 1-3 are performance test tables of polyamide hollow fiber membranes prepared in the examples of the present invention.
[0040] Table 1 Performance of polyamide hollow fiber membranes according to Example 1
[0041] Polyamide hollow fiber membrane index Cut-off pore size 30-60 nm Ethanol flux 600 LMH@bar Porosity 60-80% Organic solvent resistance Ethanol, dimethylformamide, N-methylpyrrolidone, methanol, acetone, acetonitrile, alkanes, etc. Tensile Strength 8 N Elongation at break 200%
[0042] Table 2 Performance of polyamide hollow fiber membranes of Example 2
[0043] Polyamide hollow fiber membrane index Cut-off pore size 100-200 nm Porosity 50-60% Acetonitrile flux 1500 LMH@bar Organic solvent resistance Ethanol, dimethyl sulfoxide, acetone, acetonitrile, alkanes, etc. Tensile Strength 13 N Elongation at break 220%
[0044] Table 3 Performance of polyamide hollow fiber membranes of Example 3
[0045] Polyamide hollow fiber membrane index Cut-off pore size 80-120 nm Porosity 55-65% Acetone flux 900 LMH@bar Organic solvent resistance Ethanol, dimethyl sulfoxide, N-methylpyrrolidone, dimethylformamide, dimethylacetamide, acetonitrile, alkanes, etc. Tensile Strength 10 N Elongation at break 190%
[0046] Table 4 Performance of polyamide hollow fiber membranes of Example 4
[0047] Polyamide hollow fiber membrane index Cut-off pore size 60-100 nm Porosity 65-75% Dimethylformamide flux 700 LMH@bar Organic solvent resistance Ethanol, dimethyl sulfoxide, N-methylpyrrolidone, dimethylformamide, dimethylacetamide, acetonitrile, alkanes, etc. Tensile Strength 9 N Elongation at break 200%
[0048] Table 5 Performance of polyamide hollow fiber membranes of Example 5
[0049] Polyamide hollow fiber membrane index Cut-off pore size 100-200 nm Porosity 70-80% Dimethylacetamide flux 800 LMH@bar Organic solvent resistance Ethanol, dimethyl sulfoxide, N-methylpyrrolidone, dimethylformamide, dimethylacetamide, acetonitrile, alkanes, etc. Tensile Strength 8.2 N Elongation at break 205%
[0050] Table 6 Performance of polyamide hollow fiber membranes of Example 6
[0051] Polyamide hollow fiber membrane index Cut-off pore size 40-80 nm Porosity 60-70% Methanol flux 800 LMH@bar Organic solvent resistance Ethanol, dimethyl sulfoxide, N-methylpyrrolidone, dimethylformamide, dimethylacetamide, acetonitrile, alkanes, etc. Tensile Strength 11 N Elongation at break 210%
[0052] Tables 1-3 show that by measuring the solvent permeation flux, selectivity, and tensile strength of the polyamide hollow fiber membrane, it can be seen that the comprehensive performance of the hollow fiber membranes prepared in Examples 1, 2, and 6 of the present invention is relatively excellent, among which the solvent permeation flux of Example 2 is the best at 1500LMH@bar; the best pore size of the retention performance of Example 1 is 30-60 nanometers. The polyamide hollow fiber membranes prepared in Examples 3-5 of the present invention also have the performance described in the present invention.
[0053] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing polyamide hollow fiber membrane by thermally induced phase separation, Features The following steps are involved: 1) Dissolving 20-40 parts of polyamide in 40-70 parts of diluent at 200-250° C., adding 10-20 parts of porogenic particles after the polyamide is uniformly dissolved, continuing to dissolve, and then degassing online to obtain a casting solution; the diluent is at least one of dimethyl sulfone, cyclopentane sulfone, maleic anhydride, 4-phenylbenzophenone, vinyl carbonate, propylene carbonate, tetramethyl sulfone, polyethylene glycol, and polyethylene glycol dimethyl ether; the porogenic particles are polystyrene particles cross-linked with divinylbenzene, the content of divinylbenzene is 5-15% of the polystyrene particles, the particle size of the particles is 50-200 nanometers, and the dissolution time of the porogenic particles is 20 minutes to 2 hours; 2) Extruding the above-mentioned casting liquid and core liquid through a spinneret into a hollow fiber membrane embryo, passing through an air bath section, and then entering a cooling bath to undergo phase separation and solidification to obtain a hollow fiber membrane filament; the cooling bath is one of a mixture of 5-15 parts of polyethylene glycol and 85-95 parts of polypropylene glycol, a mixture of 15-25 parts of glycerol and 75-85 parts of 1-octanol, and a mixture of 25-35 parts of diethylene glycol and 65-75 parts of triethylene glycol; 3) The obtained hollow fiber membrane is placed in water for cleaning, and then placed in an extractant to wash out the diluent, wherein the extractant is at least one of ethanol, ethyl acetate, and methanol at 50°C-60°C, and finally the porogenic particles are cleaned by immersion in a solvent, wherein the porogenic particle cleaning solvent is at least one of toluene, xylene, chloroform, styrene, carbon tetrachloride, and methyl ethyl ketone. After cleaning and drying, a polyamide hollow fiber membrane is obtained.
2. A method for preparing a polyamide hollow fiber membrane by thermally induced phase separation as claimed in claim 1, Features In step 1), the dissolving temperature is 220-230° C., 25-35 parts of polyamide, 50-60 parts of diluent, and 14-16 parts of porogenic particles.
3. A method for preparing a polyamide hollow fiber membrane by thermally induced phase separation as claimed in claim 1, Features In step 1), the polyamide is one of polyamide 6, polyamide 66, polyamide 10 and polyamide 1010, and has a molecular weight of 15,000 to 30,000.
4. A method for preparing a polyamide hollow fiber membrane by thermally induced phase separation as claimed in claim 1, Features In step 1), the content of divinylbenzene is 8-12% of the polystyrene particles; the particle size of the particles is 80-150 nanometers; and the dissolution time of the porogenic particles is 40 minutes to 1.5 hours.
5. The method for preparing a polyamide hollow fiber membrane by thermally induced phase separation according to claim 1, Features In step 2), the inner hole diameter of the spinneret is 0.8-1.2 mm, the extrusion diameter of the polyamide liquid is 1.6-2.0 mm, and the size of the slit is controlled to be no less than 0.4 mm.
6. A method for preparing a polyamide hollow fiber membrane by thermally induced phase separation as claimed in claim 1, Features In step 2), the extrusion core liquid is at least one of polyethylene glycol 200, polyethylene glycol 300, polyethylene glycol 400, and polyethylene glycol 600.
7. A method for preparing a polyamide hollow fiber membrane by thermally induced phase separation as claimed in claim 1, Features In step 2), the cooling bath is one of a mixture of 10 parts of polyethylene glycol and 90 parts of polypropylene glycol, a mixture of 20 parts of glycerol and 80 parts of 1-octanol, and a mixture of 30 parts of diethylene glycol and 70 parts of triethylene glycol; the temperature of the cooling bath is -10-10°C.
8. A method for preparing a polyamide hollow fiber membrane by thermally induced phase separation as claimed in claim 1, Features In step 2), the air bath section has a length of 2-20 cm.
9. A method for preparing a polyamide hollow fiber membrane by thermally induced phase separation as claimed in claim 1, Features In step 3), the temperature of the extractant is 54°C-56°C.
Citation Information
Patent Citations
Method for preparing reinforced hollow fiber membrane of braided tube by using low-temperature thermal-induced phase separation method
CN102500246A
Method for preparing hollow fiber nanofiltration membrane by using thermally induced phase separation / interface cross linking synchronization method
CN102824859A
Porous polyamide hollow fiber membrane having very small pore diameter, and method for producing same
CN104640619A
Preparation method of enhanced polyvinylidene fluoride hollow fiber film of weaving pipe
CN107008163A
Nanofiltration membrane and preparation method thereof
CN116194195A