A method for forming diffusion-linked structures
The diffusion bonding molding method solves the problems of long process cycle and low precision in aerospace plate-body hybrid structural components, and achieves efficient and precise integral molding, which is suitable for the production of plate-body hybrid structural components in the aerospace field.
Patent Information
- Application Number
- CN202410031644.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-09
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-01-09
AI Technical Summary
Existing technologies suffer from long process cycles and low precision when manufacturing complex plate-body hybrid structural components in high-end fields such as aerospace. In particular, the welding of hybrid cylindrical and protrusion structural components leads to error accumulation and low production efficiency.
The diffusion bonding molding method involves disassembling the molded part into a semi-cylindrical section and peripheral bosses, pre-forming and bonding by hot pressing, bonding by diffusion under high temperature and high pressure using a specific mold, and applying pressure with high pressure inert gas to achieve the overall molding of the cylindrical shape and the bosses.
It achieves efficient, one-time integral molding, reduces processes, saves materials, shortens the production cycle, improves product precision and production efficiency, and is suitable for mass production.
Smart Images

Figure CN117680942B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of materials engineering technology, and in particular relates to a method for forming diffusion bonding. Background Technology
[0002] Currently, there is an increasing demand for complex plate-body hybrid structural components in high-end fields such as aerospace. For the preparation of plate-body hybrid structural parts that combine cylinders and protrusions, the cylinder section and protrusions are usually formed by welding. This requires a large number of forming molds, inspection molds, welding fixtures, assembly jigs, and post-weld heat treatment tooling. During the final assembly process, the accumulation of part errors will cause the final product to have low precision. The entire process cycle is long, which seriously restricts product delivery.
[0003] There is an urgent need to develop a high-efficiency, high-precision integral molding method for plate-and-plate hybrid structural components to meet the needs of the high-end equipment manufacturing industry. Summary of the Invention
[0004] Based on the above analysis, the embodiments of the present invention aim to provide a diffusion bonding molding method to solve the problems of long cycle and low precision in existing plate hybrid structure molding methods.
[0005] The objective of this invention is mainly achieved through the following technical solutions: A method for forming diffusion-linked bonds includes the following steps: Step S1: Disassemble the plate-body hybrid structure of the molded part to obtain a semi-cylindrical section and peripheral bosses; Step S2: Cut the semi-cylindrical section to obtain a rectangular steel plate; cut the peripheral bosses to obtain the block blank; Step S3: Pre-form the rectangular steel plate by hot pressing to obtain a semi-cylindrical section; Step S4: The semi-cylindrical section and the boss are integrally diffused together to obtain a hybrid structure diffused connector; Step S5: Weld the two semi-cylindrical sections together to complete the final shaping.
[0006] Further, in step S2, the semi-cylindrical section is cut to obtain a rectangular steel plate, including: After extending both sides of the semi-cylindrical section by 50mm, it is unfolded to obtain a rectangular blanking size.
[0007] Furthermore, in step S3, the rectangular steel plate is pre-formed by hot pressing, and then formed using an upper mold and a first lower mold.
[0008] Furthermore, in step S3, the rectangular steel plate is pre-formed by hot pressing, and the forming conditions used are as follows: The molding temperature is 750℃, the molding pressure is 30t, and the holding time is 15min.
[0009] Furthermore, in step S4, the semi-cylindrical section and the boss are integrally diffused and connected, and formed using an upper mold and a second lower mold.
[0010] Furthermore, in step S4, the semi-cylindrical section and the boss are integrally connected by a diffusion structure, specifically including: Step S4.1: Inspect, clean, and insulate the mold; Step S4.2: Molding and furnace loading; Step S4.3: Diffusion molding.
[0011] Furthermore, in step S4.3, diffusion molding involves filling the mold with high-pressure inert gas and applying gas pressure to the part to be molded.
[0012] Furthermore, the process of filling with high-pressure inert gas and applying gas pressure to the part to be molded specifically involves: Air is pumped through the air inlet in the upper mold, through the hollowed-out part of the first conformal steel plate, into the second conformal steel plate. The diffusion pressure is then transmitted through the second conformal steel plate to the outer surface of the semi-cylindrical section and the junction of the small and large protrusions.
[0013] Furthermore, the molding conditions used in step S3.4.3 for diffusion bonding molding are as follows: The diffusion temperature is 930℃, the vacuum degree is 1×10-5Pa, the pressurization tonnage of the thermoforming machine is 50t, the diffusion gas pressure is 2MPa, the diffusion time is 2h, and the diffusion is carried out by a staged heating and pressurization method.
[0014] Furthermore, a diffusion bonding molding die is used to perform diffusion bonding molding of the plate-body hybrid structure.
[0015] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects: (1) The diffusion connection molding method provided by the present invention adopts a body hybrid structure diffusion connection molding mold, which can form a cylindrical and bump hybrid structure molded part in one step with high quality, reducing the number of processes, saving materials, shortening the production cycle and reducing production costs.
[0016] (2) The diffusion bonding molding method provided by the present invention has high molding efficiency and is conducive to the mass production of products.
[0017] In this invention, the above-described technical solutions can be combined with each other to achieve more preferred combinations. Other features and advantages of this invention will be set forth in the following description, and some advantages may become apparent from the description or be learned by practicing the invention. The objects and other advantages of this invention can be realized and obtained from what is particularly pointed out in the description and drawings. Attached Figure Description
[0018] The accompanying drawings are for illustrative purposes only and are not intended to limit the invention. Throughout the drawings, the same reference numerals denote the same parts.
[0019] Figure 1 This is a flowchart of the diffusion bonding forming method in specific embodiment 1; Figure 2 This is a schematic diagram of the overall assembly structure of the diffusion connection molding die for the plate hybrid structure in specific embodiment 2; Figure 3 This is a schematic diagram of the upper mold structure of the diffusion connection molding die for the plate-body hybrid structure in specific embodiment 2; Figure 4 This is a schematic diagram of the installation structure of the first conformal steel plate and the second conformal steel plate in the upper mold of the diffusion connection forming mold of the plate body hybrid structure in specific embodiment 2. Figure 5 (a) is a schematic diagram of the structure of the first conformal steel plate of the diffusion connection forming mold of the plate body hybrid structure in specific embodiment 2; Figure 5 (b) is a schematic diagram of the second conformal steel plate of the diffusion connection forming mold for the plate hybrid structure in specific embodiment 2; Figure 6 This is a schematic diagram of the lower mold structure of the diffusion connection molding die for the plate-body hybrid structure in specific embodiment 2; Figure 7 This is a schematic diagram of the structure of the molded part according to the diffusion bonding molding method of specific embodiment 1; Figure 8 This is an exploded view of the molded part according to the diffusion bonding molding method of specific embodiment 1; Figure 9 This is an exploded view of the small bumps in the diffusion connection molding method of specific embodiment 1; Figure 10 A schematic diagram of the large bump in the diffusion connection molding method of specific embodiment 1; Figure 11 This is a schematic diagram of the semi-cylindrical segment forming method of diffusion connection in specific embodiment 1; Figure 12 This is a schematic diagram of the diffusion bonding molding method of the specific embodiment 1.
[0020] Figure label: 1-Upper mold, 101-Upper mold body, 1011-Inflation hole, 1012-Upper mold pressure plate groove, 1013-Upper mold temperature measuring hole, 1014-Upper mold positioning groove, 102-First conformal steel plate, 103-Second conformal steel plate, 104-Lifting lug, 2-Lower mold, 2-1-First lower mold, 2-2-Second lower mold, 201-Lower mold body, 2011-Lower mold temperature measuring hole, 201 2-Lower mold positioning groove, 2013-Lower mold pressure plate groove, 2014-Groove, 202-Limiting block, 203-Limiting stop block, 2031-Positioning pin hole, 3-Formed part, 301-Semi-cylindrical section, 3011-10mm thick semi-cylindrical section, 3012-6mm thick semi-cylindrical section, 3013-12mm thick semi-cylindrical section, 302-Small protrusion, 303-Large protrusion. Detailed Implementation
[0021] The preferred embodiments of the present invention will now be described in detail with reference to the accompanying drawings, which constitute a part of the present invention and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not intended to limit the scope of the present invention.
[0022] Example 1 This invention discloses a method for forming diffusion-linked structures, such as... Figure 1 As shown, the following is adopted Figures 2-6 The plate-body hybrid structure shown is formed by diffusion connection molding.
[0023] like Figure 7 As shown, the molded part 3 is made of TA15 titanium alloy and has external dimensions of Φ600mm×250mm. The main body of the cylinder consists of three sections: a 12mm thick cylinder 3011, an 8mm thick cylinder 3012, and a 14mm thick cylinder 3013, which are joined together. Small solid protrusions 302 of various shapes are distributed around the inner perimeter, and two large trapezoidal protrusions 303 are symmetrically distributed at the bottom of the inner side.
[0024] The diffusion bonding forming method provided by the present invention includes the following steps: Step S1: Disassemble the plate-body hybrid structure of the molded part 3 to obtain the semi-cylindrical section 301 and the peripheral boss; Step S2: Cutting the semi-cylindrical section 301 and the surrounding bosses to obtain a rectangular steel plate and a boss blank; Step S3: Pre-form the rectangular steel plate by hot pressing to obtain the semi-cylindrical section 301; Step S4: The semi-cylindrical section 301 and the boss are integrally diffused together to obtain a hybrid structure diffused connector; Step S5: After diffusion is completed, remove the workpiece and weld the two semi-cylindrical sections 301 into a whole to complete the final forming.
[0025] In step S1, based on the structure of the molded part 3, the three cylindrical segments of different thicknesses are disassembled into six semi-cylindrical segments, namely two cylindrical segments 3011 with a thickness of 12mm and a cross-section of 8mm, two cylindrical segments 3012 with a cross-section of 8mm and two cylindrical segments 3013 with a cross-section of 14mm; the peripheral bosses are disassembled into small protrusions 302 of various shapes and two large protrusions 303.
[0026] Step S2 also includes the following steps: Step S2.1: Cut the semi-cylindrical section 301; Step S2.2: Cut the small boss 302 into blanks; Step S2.3: Cut the large boss 303 into shape.
[0027] like Figure 8 As shown, in step S2.1, the two sides of the semi-cylindrical section 301 are increased by 50mm and then unfolded to obtain a rectangular blank size of 12mm. 1000 mm 101 mm, 8 mm 1100 mm 220 mm and 14 mm 1000 mm 81 mm.
[0028] like Figure 9 As shown, in step S2.2, the small protrusions 302 in the model are numbered, and the material is cut and shaped. The cutting method is not limited to wire cutting and milling.
[0029] like Figure 10 As shown, in step S2.3, the large protrusion 303 is blanked and its shape is machined. The blanking method is not limited to wire cutting and milling.
[0030] All blanked parts must have their surrounding burrs removed after blanking.
[0031] like Figure 11 As shown, in step S3, the rectangular steel plate is pre-formed by hot pressing using the upper mold 1 and the first lower mold 2-1, specifically including the following steps: When hot-pressing and preforming rectangular steel plates, the mold and blanking parts need to be processed. This includes: Step S3.1: Weld the first conformal steel plate 102 and the second conformal steel plate 103 to the upper mold 1, and check the airtightness; Step S3.2: Fix and position the upper mold 1 and the first lower mold 2-1; Step S3.3: Apply a uniform Ti1# coating to the surface of the rectangular blank for heat protection; Step S3.4: Hot pressing.
[0032] The molding conditions adopted were: molding temperature of 750℃, molding pressure of 30t, and holding time of 15min.
[0033] In order not to affect the diffusion quality, after the hot pressing preforming of the semi-cylindrical section 301 is completed, the diffusion surfaces of the semi-cylindrical section 301, the small protrusion 302 and the large protrusion 303 are polished, and the whole is subjected to alkaline pickling.
[0034] The semi-cylindrical section 301 is already a whole consisting of three arc points fixed together. Its overlapping parts are prone to inadequate pickling, which affects the diffusion quality. Extend the pickling time of the semi-cylindrical section 301 by 1 hour. After pickling, rinse the overlapping parts with running water, and then place it in a constant temperature oven to dry completely before use.
[0035] In step S4, the semicircular arc segment 301 and the boss are connected by a diffusion connection, including the following steps: Step S4.1: Inspect, clean, and insulate the mold; Step S4.2: Molding and furnace loading; Step S4.3: Diffusion molding.
[0036] In diffusion bonding molding, the molds used are upper mold 1 and second lower mold 2-2.
[0037] In step S4.1, it should be noted that before diffusion bonding, the mold needs to be inspected, cleaned, and kept warm, including: Step S4.1.1: Check the airtightness of the air bag formed by the first conformal steel plate 102 and the second conformal steel plate 103 of the upper mold 1 and the forming surface of the upper mold 1 multiple times to ensure the normal progress of diffusion connection.
[0038] Step S4.1.2: In order not to affect the diffusion quality, the forming surfaces of the upper mold 1 and the second lower mold 2-2 need to be polished and cleaned with a high-pressure air gun, and then boron nitride is sprayed onto their surfaces as a lubricant.
[0039] Step S4.1.3: Further, after cleaning the mold, place the upper mold 1 in a box furnace at 600℃ for 3 hours to allow it to fully expand. During the heat preservation, evacuate the inside of the air bag to retract the expanded part and facilitate mold closing.
[0040] Step S4.2 includes the following steps: Step S4.2.1: Mold assembly; Step S4.2.2: Mold closing; Step S4.2.3: Put it into the furnace.
[0041] In step S4.2.1, the workpiece to be formed is loaded into the mold, such as... Figure 12As shown, the second lower mold 2-2 is fixed to the platform via the lower mold positioning groove 2013, and the positioning pin is installed in the positioning pin hole 2031. The small protrusion 302 and the large protrusion 303 are placed in the groove 2014 of the forming surface of the second lower mold 2-2, and the pre-formed semi-cylindrical section 301 is then placed over the forming surface of the second lower mold 2-2. During the installation process, care should be taken to protect the diffusion surface to prevent contamination that could affect the diffusion quality.
[0042] In step S4.2.2, the heated upper mold 1 is hoisted and manually aligned with the second lower mold 2-2. During the descent, the upper mold pressure plate groove 1014 is aligned with the lower mold pressure plate groove 2012, and the upper mold 1 is positioned using the positioning pins in the positioning pin holes 2031 of the second lower mold 2-2, allowing the upper mold 1 to fall onto the second lower mold 2-2. During the mold closing process, the upper mold 1 may get stuck. If the clearance is small, it can be pressed down using a press. If the clearance is too large, it must be reheated and kept warm to prevent the seal of the second conformal steel plate 103 from being broken.
[0043] Furthermore, after mold closing, check the airbag's seal again. Inflate the air passage and check if the airbag is intact.
[0044] Thermocouples are inserted into the upper mold temperature measuring hole 1013 and the lower mold temperature measuring hole 2011 respectively to monitor the temperature uniformity of the upper mold 1 and the second lower mold 2-2.
[0045] In step S4.2.3, after placing the mold into the vacuum hot press, connect the air line. Note that the air line should not be too long or too close to the heating belt to prevent overheating and cracking. At the same time, the air line can be appropriately lengthened to prevent air leakage under the combined action of high temperature and high pressure.
[0046] After the material is placed in the furnace, apply a 10t mold closing pressure and evacuate the vacuum furnace. It is important to note that the vacuum level should be reduced to 10t before proceeding. -1 After the pressure drops below 0.1 MPa, check the airtightness of the mold again by introducing air pressure of 0.1~0.2 MPa and confirm that the air bag is intact.
[0047] In step S4.3, the part to be molded undergoes diffusion bonding molding. High-pressure inert gas is injected into the mold, and gas pressure is applied to the part to be molded to perform diffusion bonding molding. It should be noted that the diffusion molding conditions used are: The diffusion temperature is 930℃ and the vacuum degree is 1×10⁻⁶. -5 Pa, the pressurization tonnage of the thermoforming machine is 50t, the diffusion pressure is 2MPa, and the diffusion time is 2h.
[0048] Based on the structure of the semi-cylindrical section and the protrusion, and the characteristics of the area to be diffused, the diffusion connection molding pressurization method adopted is as follows: Heat to 920℃ and hold for 120 minutes to ensure thorough heating of the mold and parts. After completion, maintain the temperature and pressure for 60 minutes, then pressurize the air bag at a rate of 0.5 MPa / 10 minutes, hold for 10 minutes, and repeat the process until the air pressure reaches 1.5 MPa, holding for 180 minutes; increase the air pressure to 2 MPa within 10 minutes, holding for 180 minutes; increase the air pressure to 2.5 MPa within 10 minutes, holding for 60 minutes. After completion, remove the pressure and cool down.
[0049] During diffusion molding, air is injected into the second conformal steel plate 103 through the air inlet 1011 in the upper mold 1, passing through the hollow portion of the first conformal steel plate 102. The second conformal steel plate 103 transmits the diffusion pressure to the junction of the outer surface of the semi-cylindrical section 301 with the small protrusion 302 and the large protrusion 303. Under the action of diffusion pressure, the outer surface of the semi-cylindrical section 301 is tightly bonded to the protrusions embedded in the lower mold 2, and the overlapping portion of the semi-cylindrical section 301 is also tightly bonded, ensuring that the pressure at the diffusion interface meets the diffusion requirements. Under the action of high temperature and high pressure, diffusion connection is achieved.
[0050] Example 2 A specific embodiment of the present invention, such as Figure 2 As shown, a diffusion bonding molding die for Example 1 is disclosed, comprising an upper die 1 and a lower die 2.
[0051] After the upper mold 1 and the lower mold 2 are closed, they form a cuboid. The upper mold 1 is the upper mold for applying gas pressure, mainly used for the pre-forming of the semi-cylindrical section and the final forming of the molded part through gas pressure diffusion connection.
[0052] like Figure 3 As shown, the upper mold 1 includes an upper mold body 101, a first conformal steel plate 102, a second conformal steel plate 103, and a lifting lug 104.
[0053] like Figure 4 As shown, an air inlet 1011 is provided on the semi-circular forming surface of the upper mold body 101 of the upper mold 1, which is used to apply gas pressure to the first conformal steel plate 102 and the second conformal steel plate 103, and indirectly apply gas pressure to the small protrusion 311 and the large protrusion 312 of the semi-circular section, thereby promoting the diffusion connection forming of the product.
[0054] like Figure 5 As shown in (a), it should be noted that the first conformal steel plate 102 is a conformal steel plate with a hollowed-out shape, with the hollowed-out shape in the middle corresponding to the part of the groove 2014 of the lower mold 2. The air inlet 1011 is located in the hollowed-out part.
[0055] like Figure 5As shown in (b), the second conformal steel plate 103 is a conformal steel plate under gas pressure. One side is in contact with the first conformal steel plate 102, and the other side is in direct contact with the outer surface of the semi-cylindrical section 301 of the forming part 3. It is used to pressurize the forming part 3 so that the inner surface of the semi-cylindrical section 301 and the protrusion to be diffused fit tightly together for diffusion forming.
[0056] The first conformal steel plate 102 and the second conformal steel plate 103 are welded and fixed to the semi-circular forming surface of the upper mold body 101. The first conformal steel plate 102 and the second conformal steel plate 103 form an air bag with the forming surface of the upper mold body 101. After the sealing is completed, the air tightness of the air bag needs to be tested to ensure the reliability of the seal.
[0057] The upper part of the upper mold body 101 is provided with an upper mold pressure plate groove 1014, and the lower part is provided with an upper mold positioning groove 1012, which are used for positioning the upper mold 1 and fixing the upper mold 1 to the first lower mold 2-1 or the second lower mold 2-2. Temperature measuring holes 1013 are provided at different parts of the upper mold 1 for inserting thermocouples to monitor the temperature uniformity of the upper mold 1.
[0058] The upper part of the upper mold 1 is provided with a lifting lug 104 for lifting and transferring the upper mold 1.
[0059] The lower mold 2 includes a first lower mold 2-1 and a second lower mold 2-2 with identical structures. The first lower mold 2-1 is used for hot-pressing pre-forming of the semi-cylindrical section 301, and the second lower mold 2-2 is used for diffusion-connection forming. Figure 6 As shown, the lower mold 2 includes a lower mold body 201, a limiting block 202, and a limiting stop block 203.
[0060] The lower mold body 201 includes an upwardly convex semi-circular forming surface. The upwardly convex semi-circular forming surface of the lower mold 2 matches the downwardly concave semi-circular forming surface of the upper mold 1.
[0061] The lower part of the lower mold body 201 is provided with a lower mold positioning groove 2012 and a lower mold pressure plate groove 2013 for positioning the lower mold 2 and fixing the lower mold 2 to the platform. Temperature measuring holes 2011 are provided at different parts of the lower mold 2 for inserting thermocouples to monitor the temperature uniformity of the lower mold 2.
[0062] The surface of the lower mold body 201 has a groove 2014, the shape of which matches the profile of the small protrusion 302 and the large protrusion 303 to be diffused.
[0063] A limiting block 202 is provided at the semi-circular termination position of the lower mold 2. After the limiting block 202 is pulled out from both sides, the protrusion with the largest demolding angle can be successfully demolded after diffusion.
[0064] A limit stop 203 is provided at the part of the lower mold body 201 that connects to the upper mold 1. The limit stop 203 has a positioning pin hole 2031, into which a positioning pin can be inserted for positioning the sheet metal and limiting the upper mold 1.
[0065] In practical use, firstly, the first conformal steel plate 102 and the second conformal steel plate 103 are welded to the forming surface of the upper mold body 101, and the airtightness is checked; secondly, the lower mold 2 is fixed to the platform through the lower mold positioning groove 2012; then, the parts to be formed are placed on the forming surface of the lower mold 2 in sequence, the hook of the lifting device is suspended from the lifting lug 104 of the upper mold 1, and lifted above the lower mold 2, so that the upper mold pressure plate groove 1014 is aligned with the lower mold pressure plate groove 2012, and the upper mold 1 is positioned through the positioning pin hole 2031 of the limiting block 203; finally, the mold is closed.
[0066] Thermocouples are inserted into the upper mold temperature measuring hole 1013 and the lower mold temperature measuring hole 2011 respectively to monitor the temperature uniformity of the upper mold 1 and the lower mold 2.
[0067] During the pre-forming of the semi-cylindrical section 301, it is placed between the upper mold 1 and the first lower mold 2-1 and directly hot-pressed. During diffusion forming, small protrusions 302 and large protrusions 303 are placed in the groove 2014 of the lower mold 2. The pre-formed semi-cylindrical section 301 is then placed over the lower mold forming surface of the second lower mold 2-2. Air is injected into the second conformal steel plate 103 through the air inlet 1011 in the upper mold 1, passing through the hollow part of the first conformal steel plate 102. The diffusion pressure is then transmitted to the outer surface of the semi-cylindrical section 301 at the junction with the small protrusions 302 and large protrusions 303 via the second conformal steel plate 103. Under the action of diffusion pressure, the outer surface of the semi-cylindrical section 301 is tightly bonded to the protrusions embedded in the lower mold 2, and the overlapping part of the semi-cylindrical section 301 is also tightly bonded, ensuring that the pressure at the diffusion interface meets the diffusion requirements. Under the action of high temperature and high pressure, diffusion connection is achieved.
[0068] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.
Claims
1. A method of diffusion bonding forming, characterized by, Includes the following steps: Step S1: Disassemble the plate-body hybrid structure of the molded part (3) to obtain the semi-cylindrical section (301) and the peripheral boss; Step S2: The semi-cylindrical section (301) is cut to obtain a rectangular steel plate; the peripheral boss is cut to obtain a block blank, and the block blank is processed to obtain the peripheral boss; Step S3: Hot press the rectangular steel plate to preform it into a semi-cylindrical section (301). In step S3, the rectangular steel plate is pre-formed by hot pressing, and the upper mold (1) and the first lower mold (2-1) are used for forming. Step S4: The semi-cylindrical section (301) and the peripheral boss are diffused together to obtain a hybrid structure diffused connector; in step S4, the semi-cylindrical section (301) and the peripheral boss are diffused together and formed using the upper mold (1) and the second lower mold (2-2); The upper mold (1) includes an upper mold body (101), a first conformal steel plate (102), and a second conformal steel plate (103); an air inlet (1011) is provided on the semi-circular forming surface of the upper mold body (101); the first conformal steel plate (102) is a conformal steel plate with a hollow shape, and the hollow shape in the middle corresponds to the part of the groove (2014) provided on the arc surface of the second lower mold (2-2); the groove (2014) is used to place the peripheral boss; the second conformal steel plate (103) is a conformal steel plate with applied gas pressure, one side of which is in contact with the first conformal steel plate (102), and the other side is in direct contact with the outer surface of the semi-cylindrical section (301); The diffusion connection in step S4 includes filling the upper mold (1) with high-pressure inert gas and applying gas pressure to the part to be formed; through the air inlet (1011) in the upper mold (1) through the hollow part of the first conformal steel plate (102) to inflate the second conformal steel plate (103), and through the second conformal steel plate (103) to transmit the diffusion pressure to the outer surface of the semi-cylindrical section (301) and the junction of the peripheral boss; Step S5: Weld the two semi-cylindrical sections (301) into a whole to complete the final forming.
2. The method for forming diffusion bonding according to claim 1, characterized in that, In step S2, the semi-cylindrical section is cut to obtain a rectangular steel plate, including: After extending the two sides of the semi-cylindrical section (301) by 50mm, it is unfolded to obtain a rectangular blanking size.
3. The method for forming diffusion bonding according to claim 1, characterized in that, In step S3, the rectangular steel plate is pre-formed by hot pressing, and the forming conditions used are as follows: The molding temperature is 750℃, the molding pressure is 30t, and the holding time is 15min.
4. The molding method for diffusion bonding according to claim 1, characterized in that, In step S4, the semi-cylindrical section (301) and the surrounding bosses are connected in a diffusion manner, specifically including: Step S4.1: Inspect, clean and keep the upper mold (1) and the second lower mold (2-2) warm; Step S4.2: Molding and furnace loading; Step S4.3: Diffusion molding.
Citation Information
Patent Citations
Forming method of variable cross-section cylindrical part with internally-attached boss
CN117324741A
Plate body mixed structure assembling diffusion connection forming die
CN117943461A