A method for preparing mushroom-shaped monodisperse ZnO particles with downtransfer luminescence
By adding polyvinylpyrrolidone and Zn(AC)2·2H2O to benzyl alcohol solvent and combining it with elemental powder carrier, mushroom-shaped ZnO particles with uniform morphology and good dispersibility were prepared. This solved the problem of poor dispersion and morphological uniformity of ZnO particles in the prior art, and realized down-transfer luminescence performance, which is suitable for sensing and optical coatings.
Patent Information
- Application Number
- CN202311438555.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-01
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-11-01
AI Technical Summary
Existing technologies make it difficult to prepare monodisperse ZnO particles with uniform particle size. In particular, small-sized ZnO particles lack down-transfer luminescence properties, and ZnO particles synthesized by traditional methods have poor dispersion and morphological uniformity.
Mushroom-shaped monodisperse ZnO particles were prepared by controlling the reaction conditions using benzyl alcohol as a solvent and polyvinylpyrrolidone as an additive. Zn(AC)2·2H2O was used as the zinc source and elemental powder was used as the carrier. After the reaction, ZnO particles with down-transfer luminescence function were obtained by centrifugation and washing.
Mushroom-shaped ZnO particles with a diameter of approximately 1000 nm were prepared. These particles exhibited good dispersibility and morphological uniformity, and were able to absorb ultraviolet light and emit visible light, demonstrating downconversion luminescence properties. They are suitable for applications in sensing and optical coatings.
Smart Images

Figure CN117682548B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a method for preparing mushroom-shaped monodisperse ZnO particles with downtransfer luminescence, belonging to the field of inorganic nanomaterial preparation technology. Background Technology
[0002] The properties of semiconductor nanomaterials are closely related to their morphology and size. Therefore, the synthesis of morphology-controllable semiconductor nanostructures has become a focus of attention in the field of materials science.
[0003] ZnO is a typical semiconductor material. Its stable crystal structure at room temperature and pressure is hexagonal wurtzite. At room temperature, ZnO has a band gap of 3.37 eV and a high exciton binding energy of up to 60 meV, far exceeding other blue light-emitting semiconductors. It can be used to fabricate important optoelectronic devices such as short-wavelength lasers and light-emitting semiconductors. ZnO possesses excellent optical, electrical, ferromagnetic, and piezoelectric properties and is widely used in numerous fields. Currently, there are few reports on the synthesis of monodisperse ZnO particles with uniform particle size. Therefore, preparing monodisperse ZnO particles with a narrow particle size distribution remains a challenging task. Furthermore, small ZnO particles (within 10 nm) can absorb ultraviolet light and emit visible light due to their surface defects, while larger ZnO particles generally lack down-transfer luminescence properties. Summary of the Invention
[0004] To overcome the shortcomings of existing technologies, this invention provides a method for preparing mushroom-shaped monodisperse ZnO particles with downconversion luminescence. Benzyl alcohol is used as a solvent, polyvinylpyrrolidone (PVP) as an additive, Zn(AC)₂·2H₂O as a zinc source, and elemental powder as a carrier. The prepared ZnO particles have uniform morphology, good dispersibility, and can absorb light around 365 nm and emit visible light around 625 nm, exhibiting downconversion luminescence function.
[0005] The technical solution adopted by this invention to solve its technical problem is: A method for preparing mushroom-shaped monodisperse ZnO particles with downtransfer luminescence, the method comprising the following steps: S1. Add zinc acetate dihydrate (Zn(AC)2·2H2O) to benzyl alcohol solution, stir thoroughly, then add polyvinylpyrrolidone (PVP), and stir thoroughly again to obtain mixed solution A; S2. Add elemental powder as a carrier to the mixed solution A in step S1, and stir thoroughly to obtain mixture B; S3. Pour the stirred solution into a polytetrafluoroethylene liner, then seal the reaction vessel, place it in an oven for heating, and then allow it to cool naturally to room temperature. The reaction products are washed by centrifugation with deionized water and anhydrous ethanol to remove residual reaction liquid, and monodisperse ZnO particles of uniform size are obtained.
[0006] In the above-mentioned method for preparing mushroom-shaped monodisperse ZnO particles with downtransfer luminescence, in step S1, the volume of benzyl alcohol solution is 15-30 mL, the amount of zinc acetate dihydrate added is 0.2-0.8 mmol, and the amount of PVP added is 0.5-2.0 g.
[0007] In the above-mentioned method for preparing mushroom-shaped monodisperse ZnO particles with downtransfer luminescence, in step S1, the volume of benzyl alcohol solution is 15-20 mL, the amount of zinc acetate dihydrate added is 0.3-0.6 mmol, and the amount of PVP added is 0.6-1.8 g.
[0008] In the above-mentioned method for preparing mushroom-shaped monodisperse ZnO particles with down-transfer luminescence, the elemental powder in step S2 is elemental selenium.
[0009] In the above-mentioned method for preparing mushroom-shaped monodisperse ZnO particles with downward transfer luminescence, in step S3, the oven heating temperature is 120℃~180℃, and the heat preservation reaction time is 12~24h.
[0010] In the above-mentioned method for preparing mushroom-shaped monodisperse ZnO particles with downward transfer luminescence, in step S3, the oven heating temperature is 120℃~160℃, and the heat preservation reaction time is 12~18h.
[0011] The beneficial effects of this invention are: (1) This invention provides a new method for preparing monodisperse ZnO particles. This method is highly operable, has a simple apparatus, and is highly reproducible.
[0012] (2) Compared with traditional ZnO particles, the monodisperse mushroom-shaped ZnO particles prepared by the present invention have the advantages of large particle size (particle size ≈ 1000 nm), concentrated particle size distribution and good stability.
[0013] (3) The monodisperse mushroom-shaped ZnO particles prepared by this invention can absorb ultraviolet light and emit visible light, exhibiting downconversion luminescence properties. For small ZnO particles with a size of less than 10 nm, their surface defects can absorb ultraviolet light and emit visible light, while larger ZnO particle materials generally do not have downconversion luminescence properties. However, the mushroom-shaped ZnO particles with a size of approximately 1000 nm prepared by this invention can still absorb ultraviolet light of about 365 nm and emit visible light of about 625 nm, exhibiting downconversion luminescence function. These ZnO particles are expected to be applied in fields such as sensing, luminescence, and optical coatings. Attached Figure Description
[0014] Figure 1 (a)-(b) are scanning electron microscope images of mushroom-shaped monodisperse ZnO particles obtained in Example 1 of the present invention; Figure 2 The photoexcitation and photoemission spectra of mushroom-shaped ZnO particle powder obtained in Example 1 of this invention are shown. Figure 3 (a)-(b) are scanning electron microscope images of mushroom-shaped monodisperse ZnO particles obtained in Example 2 of the present invention; Figure 4 (a)-(b) are scanning electron microscope images of mushroom-shaped monodisperse ZnO particles obtained in Example 3 of the present invention; Figure 5 (a)-(d) are scanning electron microscope images of ZnO particles obtained in the comparative examples of this invention. Detailed Implementation
[0015] The mushroom-shaped ZnO nanoparticles prepared by the method of this invention have a size of approximately 1000 nm and exhibit down-transfer luminescence properties. In contrast, conventional inorganic materials typically exhibit luminescence due to their very small crystallite size; for example, quantum dots typically have a size of a few nanometers to tens of nanometers. This indicates that the mushroom-shaped ZnO nanoparticles prepared by this invention are composed of very small ZnO nanocrystals.
[0016] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention. Example 1
[0017] This embodiment provides a method for preparing mushroom-shaped monodisperse ZnO particles with down-transfer luminescence. In this embodiment, 0.2 mmol of selenium powder is added to the mixed solution in step S1, and the specific steps include the following: S1. Add 0.45 mmol of zinc acetate dihydrate (Zn(AC)2·2H2O) to 20 mL of benzyl alcohol solution, stir thoroughly, then add 1.2 g of polyvinylpyrrolidone (PVP), and stir thoroughly again to obtain mixed solution A; S2. Add 0.2 mmol of selenium powder as a carrier to the mixed solution A in step S1, and stir thoroughly to obtain mixture B; S3. Pour the stirred solution into a polytetrafluoroethylene liner, then seal the reaction vessel. React at 150°C for 12 hours, then allow it to cool naturally to room temperature. Wash the reaction product with deionized water and anhydrous ethanol by centrifugation to remove residual reaction liquid and obtain monodisperse ZnO particles of uniform size.
[0018] Figure 1 (a)-(b) are scanning electron microscope images of monodisperse mushroom-shaped ZnO particles obtained in Example 1 of the present invention. It can be seen that the mushroom-shaped ZnO particles have good monodispersity, uniform morphology, and uniform size of about 1000 nm.
[0019] Figure 2 The photoexcitation and photoemission spectra of mushroom-shaped ZnO particle powder obtained in Example 1 of this invention are shown. It can be seen that the mushroom-shaped ZnO particle powder can absorb ultraviolet light and emit visible light at approximately 625 nm, exhibiting downconversion luminescence properties. Example 2
[0020] This embodiment provides a method for preparing mushroom-shaped monodisperse ZnO particles with down-transfer luminescence. The specific steps are the same as in Example 1, except for the ratio of the added amounts. Specifically, the method includes the following steps: S1. Add 0.60 mmol of zinc acetate dihydrate (Zn(AC)2·2H2O) to 20 mL of benzyl alcohol solution, stir thoroughly, then add 1.8 g of polyvinylpyrrolidone (PVP), and stir thoroughly again to obtain mixed solution A; S2. Add 0.3 mmol of selenium powder as a carrier to the mixed solution A in step S1, and stir thoroughly to obtain mixture B; S3. Pour the stirred solution into a polytetrafluoroethylene liner, then seal the reaction vessel. React at 150°C for 12 hours, then allow it to cool naturally to room temperature. Wash the reaction product with deionized water and anhydrous ethanol by centrifugation to remove residual reaction liquid and obtain monodisperse ZnO particles of uniform size.
[0021] Figure 3 Images (a)-(b) are scanning electron microscope (SEM) images of monodisperse mushroom-shaped ZnO particles obtained in Example 2 of this invention. It can be seen that the mushroom-shaped ZnO particles exhibit good monodispersity, uniform morphology, and a uniform size of approximately 1000 nm. Compared to Example 1, the ZnO particles have a morphology closer to spherical. Example 3
[0022] This embodiment provides a method for preparing mushroom-shaped monodisperse ZnO particles with down-transfer luminescence. The specific steps are the same as in Example 1, except for the ratio of the added amounts. Specifically, the method includes the following steps: S1. Add 0.30 mmol of zinc acetate dihydrate (Zn(AC)2·2H2O) to 20 mL of benzyl alcohol solution, stir thoroughly, then add 0.6 g of polyvinylpyrrolidone (PVP), and stir thoroughly again to obtain mixed solution A; S2. Add 0.1 mmol of selenium powder as a carrier to the mixed solution A in step S1, and stir thoroughly to obtain mixture B; S3. Pour the stirred solution into a polytetrafluoroethylene liner, then seal the reaction vessel. React at 150°C for 12 hours, then allow it to cool naturally to room temperature. Wash the reaction product with deionized water and anhydrous ethanol by centrifugation to remove residual reaction liquid and obtain monodisperse ZnO particles of uniform size.
[0023] Figure 4 (a)-(b) are scanning electron microscope images of monodisperse mushroom-shaped ZnO particles obtained in Example 3 of the present invention. Comparative Example 1
[0024] In Comparative Example 1, only benzyl alcohol in Example 1 was replaced with ethylene glycol; all other conditions were the same as in Example 1. Scanning electron microscope images of the ZnO nanoparticles prepared in this way are shown below. Figure 5 As shown in Figure a, the ZnO particles are non-spherical and poorly dispersed. This is likely due to differences in the dispersibility of the reactants in the solvent. Comparative Example 2
[0025] In the preparation process of Comparative Example 2, the amounts of benzyl alcohol solution, zinc acetate dihydrate, and PVP added exceeded the limits specified in this invention. Other preparation conditions were the same as in Example 1, and the specific preparation steps were as follows: S1. Add 0.15 mmol of zinc acetate dihydrate (Zn(AC)2·2H2O) to 10 mL of benzyl alcohol solution, stir thoroughly, then add 0.3 g of polyvinylpyrrolidone (PVP), and stir thoroughly again to obtain mixed solution A; S2. Add 0.2 mmol of selenium powder as a carrier to the mixed solution A in step S1, and stir thoroughly to obtain mixture B; S3. Pour the stirred solution into a polytetrafluoroethylene liner, then seal the reaction vessel. React at 150°C for 12 hours, then allow it to cool naturally to room temperature. Wash the reaction products with deionized water and anhydrous ethanol by centrifugation to remove residual reaction liquid.
[0026] Scanning electron microscope images of the prepared ZnO nanoparticles are shown below. Figure 5 As shown in Figure b, the ZnO particles are flat and round with a central protrusion, exhibiting poor dispersibility. This may be due to a lower reactant content, leading to fewer collisions and hindering growth into larger spherical shapes. Comparative Example 3
[0027] In the preparation of ZnO particles in Comparative Example 3, the addition of the elemental support in step S2 of Example 1 was omitted, while other conditions remained the same as in Example 1. Scanning electron microscope images of the prepared ZnO nanoparticles are shown below. Figure 5 As shown in Figure c, the mushroom-shaped ZnO surface is rough, with many hexagonal particles. This may be because the elemental metal powder does not participate in the reaction but acts as a carrier, preventing the later-formed hexagonal ZnO particles from accumulating on the surface of the mushroom-shaped ZnO particles when the elemental metal is added. In contrast, Comparative Example 3, which did not add elemental metal powder, caused the later-formed particles to deposit on the surface of the mushroom-shaped ZnO particles. Comparative Example 4
[0028] In the preparation steps, PVP was not added in step S1, and other conditions were the same as in Example 1. Scanning electron microscope images of the prepared ZnO nanoparticles are shown below. Figure 5 As shown in Figure d, the synthesized nanoparticles vary in size and have irregular shapes. This is likely because the absence of a surfactant makes it difficult to disperse the reactants uniformly, resulting in the inconsistent shapes of the synthesized nanoparticles.
[0029] Scanning electron microscope images of ZnO nanoparticles obtained in Comparative Examples 1-4 show that the ZnO particles have poor overall dispersion and poor morphological uniformity.
Claims
1. A process for the preparation of mushroom-shaped monodispersed ZnO particles with down-conversion luminescence, characterized by: The method includes the following steps: S1. Add zinc acetate dihydrate Zn(AC)2·2H2O to benzyl alcohol solution, stir thoroughly, then add polyvinylpyrrolidone PVP, and stir thoroughly again to obtain mixed solution A. S2. Add elemental powder as a carrier to the mixed solution A in step S1, and stir thoroughly to obtain mixture B; S3. Pour the stirred solution into a polytetrafluoroethylene liner, then seal the reaction vessel, place it in an oven for heating, and then allow it to cool naturally to room temperature. The reaction products are washed by centrifugation with deionized water and anhydrous ethanol to remove residual reaction liquid and obtain monodisperse ZnO particles of uniform size. In step S1, the volume of benzyl alcohol solution is 15-30 mL, the amount of zinc acetate dihydrate added is 0.2-0.8 mmol, and the amount of PVP added is 0.5-2.0 g. The elemental powder in step S2 is elemental selenium. In step S3, the oven heating temperature is 120℃~180℃, and the heat preservation reaction time is 12~24h.
2. The method for preparing mushroom-shaped monodisperse ZnO particles with down-transfer luminescence according to claim 1, characterized in that: In step S1, the volume of benzyl alcohol solution is 15-20 mL, the amount of zinc acetate dihydrate added is 0.3-0.6 mmol, and the amount of PVP added is 0.6-1.8 g.
3. The method for preparing mushroom-shaped monodisperse ZnO particles with down-transfer luminescence according to claim 1, characterized in that: In step S3, the oven heating temperature is 120℃~160℃, and the heat preservation reaction time is 12~18h.
Citation Information
Patent Citations
Composition containing fine particles and process for producing the same
CN101031285A
Preparation method for Zno quantum dot
CN102206486A