A composite copper foil with enhanced adhesion between copper foil and substrate
By introducing a zinc oxide layer loaded with precious metal nanoparticles into the composite copper foil, the problems of expensive production equipment and insufficient bonding force of the composite copper foil are solved, the bonding force between the copper foil and the polymer layer is improved, and the process flow is simplified. And improve the safety of lithium batteries.
Patent Information
- Application Number
- CN202311716258.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-13
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-12-13
AI Technical Summary
The existing composite copper foil production process equipment is expensive, the production efficiency is low, and the bonding force between the copper foil and the substrate is low, which limits the large-scale production of composite copper foil.
A zinc oxide layer loaded with precious metal nanoparticles is introduced between the polymer layer and the copper foil layer. The zinc oxide nanolayer is prepared by spraying and heat treatment, and the precious metal nanoparticles are reduced on it to improve the polymerization of the copper foil and the polymer. The bonding force of material layers.
It effectively improves the bonding force between the copper foil and the polymer layer, reduces the cost of zinc oxide, simplifies the process, reduces the dendrite formation of lithium ions during the charge and discharge process, and improves the safety of lithium batteries.
Smart Images

Figure CN117691121B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal films and relates to a composite copper foil with enhanced adhesion between the copper foil and a substrate. Background Art
[0002] Lithium battery copper foil is developing towards thinness, high density, high tensile strength and high elongation. Composite copper foil is made of insulating polymer materials such as PET (polyethylene terephthalate), PP (polypropylene), etc. as the base material, and copper foil layers covering the upper and lower surfaces. Compared with electrolytic copper foil, the weight is reduced by 50-60%, the energy density is increased by 5-10%, and the price sensitivity of raw copper is lower. The cost of raw copper can be reduced by 35-50%. More importantly, the circuit-breaking effect of the polymer film in the composite copper foil can significantly improve the safety of the battery. In addition, the flexibility of the composite copper foil can absorb the stress when the battery expands, thereby increasing the life of the lithium battery.
[0003] The current production process of composite copper foil mainly includes a one-step water electroplating, a two-step process of magnetron sputtering priming and water electroplating thickening, and a magnetron one-step process. Chinese invention patent application CN115700295A provides a continuous preparation process for PET composite copper foil, which uses PET as a carrier, deposits a uniform thin copper layer on the surface by magnetron sputtering, and then increases the thickness of the PET composite copper foil by pulse electroplating. The Cu-PET-Cu base composite structure is adopted, and the preparation process is stable and controllable, with a thickness of more than 10μm. However, the process is complex, the equipment is expensive, the production efficiency is low, and the bonding force between the copper foil and the base film is low, which is not conducive to the large-scale production of composite copper foil.
[0004] Chinese invention patent CN1088006C discloses a metal body with a vapor deposition treatment layer and an adhesion promotion layer, that is, a metal foil such as copper foil, on the surface of which a layer of metal oxide or metal nitride is vapor deposited, which can improve the bonding strength of the foil to a non-conductive substrate. These metal foils can be used to manufacture batteries, EMI / RFI protective linings, printed circuit boards and other products.
[0005] Chinese invention patent application CN116770246A discloses a method for enhancing the adhesion of composite copper foil and a composite copper foil. The method uses magnetron sputtering to plate a partial oxidized metal film layer on the surface of a substrate. The method can effectively improve the adhesion between the film layer and the substrate (adhesion reaches 5B), improve the coating efficiency, and complete the preparation of a composite copper foil with a single-sided film thickness of 1-2μm at one time. However, the partial oxidized metal film layer prepared by the method needs to be controlled by specific processes such as oxygen permeation to keep the element and the oxide within a certain ratio range, which is relatively complicated.
[0006] Chinese invention patent application CN113036153A discloses a copper-based current collector that induces preferential lateral deposition of lithium metal anodes, and its preparation method and application, a zinc oxide layer and a copper nanosheet array that are in situ grown or ex situ modified on the surface of copper foil, and a zinc oxide layer that is flattened on the surface of the copper-based foil, which can reduce the parallel charge density and prevent the vertical deposition and growth of lithium metal on the current collector. Lithium metal is induced to preferentially deposit in the lateral direction, and the generation of lithium dendrites is inhibited, thereby improving the safety and cycle life of lithium metal batteries.
[0007] Although metal oxides have complex processes in the preparation of composite copper foil, they play an important role in improving the adhesion between copper foil and substrate. Zinc oxide nanomaterials have been widely studied and applied in transparent conductive electrodes of nano-optoelectronic devices, flat panel displays and solar cells due to their excellent optoelectronic properties. In addition, ZnO-modified copper foil can induce lithium ion deposition, thereby improving the life of lithium batteries. Therefore, further research is needed to improve zinc oxide itself and the process of introducing zinc oxide into composite copper foil to improve the comprehensive performance of composite copper foil. Summary of the invention
[0008] The present invention aims to solve the problem of complicated process and expensive equipment for the process of using magnetron sputtering to prime and then electroplating to thicken the copper foil, and provides a composite copper foil with enhanced adhesion to the substrate. The composite copper foil introduces a zinc oxide layer loaded with precious metal nanoparticles between the polymer layer and the copper foil layer, which can effectively improve the binding force between the copper foil and the polymer, reduce the formation of dendrites of lithium ions during the charging and discharging process, and improve the safety of lithium batteries.
[0009] The technical solution of the present invention is as follows:
[0010] A composite copper foil for enhancing the adhesion between the copper foil and a substrate, the composite copper foil comprising a high molecular polymer layer, a zinc oxide nanolayer loaded with precious metal particles and a copper foil layer; the zinc oxide nanolayer loaded with precious metal particles is located on both sides of the high molecular polymer layer, and the surface of the zinc oxide nanolayer loaded with precious metal particles away from the high molecular polymer layer is the copper foil layer.
[0011] Furthermore, the method for preparing the zinc oxide nanolayer loaded with precious metal particles is as follows:
[0012] (1) spraying an alcohol solution of zinc salt on a polymer layer to form a sol of zinc salt, and then heat-treating the polymer layer to obtain a zinc oxide nanoparticle-loaded polymer layer;
[0013] (2) Immersing the high molecular polymer layer loaded with zinc oxide nanoparticles in a polyol solution containing a noble metal salt and a stabilizer to reduce the noble metal ions into noble metal nanoparticles.
[0014] Furthermore, the molar ratio of the noble metal salt to the zinc salt is 1:0.25-1.2.
[0015] Furthermore, the alcohol solution of zinc salt consists of zinc salt, nitrogen-containing ligand and ethanol.
[0016] Furthermore, the zinc salt is selected from at least one of ZnSO4·7H2O, ZnCl2, Zn(NO3)2·6H2O and Zn(OAC)2·2H2O; preferably Zn(OAC)2·2H2O.
[0017] Furthermore, the nitrogen-containing ligand is selected from at least one of triethanolamine, diethanolamine, ethanolamine, tripropanolamine and dipropanolamine; preferably ethanolamine.
[0018] Furthermore, the zinc ion concentration in the alcohol solution of the zinc salt is 10-200 mM, preferably 20-50 mM; the concentration of the nitrogen-containing ligand is 10-100 mM, preferably 30-50 mM.
[0019] Furthermore, the noble metal salt is selected from at least one of Pd, Ag, Ru, Pt, Ir and Au salts; specifically, at least one of nitrates, chlorides and acetates of noble metals; preferably AgNO3 or PdCl2.
[0020] Furthermore, the polymer in the polymer layer is selected from at least one of polyimide, polyethylene terephthalate and polyphenylene sulfide.
[0021] In some embodiments of the present invention, the preparation method of the composite copper foil is as follows:
[0022] (1) Preparation of zinc oxide nanolayer: spraying an alcohol solution of zinc salt on a polymer base film, and subjecting the film to heat treatment to obtain a composite film 1;
[0023] (2) Loading precious metal nanoparticles: immersing the composite membrane 1 in a polyol solution containing precious metal salts and stabilizers to reduce the precious metal ions to precious metal nanoparticles, and washing to obtain the composite membrane 2;
[0024] (3) Chemical copper plating: The composite film 2 is immersed in an alkaline chemical copper plating solution for copper plating to obtain a composite copper foil.
[0025] Furthermore, the stabilizer is a surfactant or a high molecular polymer, selected from at least one of cetyltrimethylammonium bromide (CTAB), polyacrylamide (PAM) and polyvinylpyrrolidone (PVP); preferably polyvinylpyrrolidone (PVP).
[0026] Furthermore, the polyol is selected from at least one of ethylene glycol, 1,4-butanediol, 1,5-pentanediol, glycerol and di(ethylene glycol); preferably ethylene glycol.
[0027] Furthermore, the reduction temperature is 110-180° C. and the reduction time is 40 min-16 h.
[0028] Furthermore, the alkaline chemical copper plating solution comprises copper sulfate, a reducing agent and a complexing agent.
[0029] Furthermore, the reducing agent is a dual reducing agent system consisting of dimethylaminoborane (DMAB) and sodium hypophosphite (SHP).
[0030] Furthermore, the complexing agent is disodium ethylenediaminetetraacetate (EDTA-2Na).
[0031] Furthermore, the alkaline chemical copper plating solution contains Cu 2+ The concentration is 5-20 g / L, the concentration of sodium hypophosphite (SHP) is 5-100 g / L, the concentration of dimethylaminoborane (DMAB) is 0.05-5 g / L; the concentration of disodium ethylenediaminetetraacetate (EDTA-2Na) is 10-30 g / L.
[0032] Furthermore, the pH value of the alkaline chemical copper plating solution is 8-10.
[0033] Furthermore, the copper plating temperature is 20-100° C., preferably 60-80° C., and the copper plating time is 1 min-2 h, preferably 3 min-1 h.
[0034] Furthermore, the polymer layer has a thickness of 4-6 μm.
[0035] Furthermore, the zinc oxide nanolayer has a thickness of 50-200 nm.
[0036] Compared with the prior art, the present invention has the following beneficial effects:
[0037] (1) The composite copper foil of the present invention introduces zinc oxide between the polymer layer and the copper foil layer to effectively improve the bonding force between the copper foil and the polymer; and the use of zinc oxide is low in cost and has a wide source;
[0038] (2) The present invention further introduces precious metal nanoparticles on the zinc oxide layer, which facilitates the subsequent chemical copper plating and avoids the steps of substrate roughening, immersion in precious metal solution, tin sensitization and activation;
[0039] (3) The zinc oxide layer adopts the process of spraying and heating treatment, which avoids the use of expensive equipment such as laser pulse deposition and magnetron sputtering, making it easier to achieve large-scale preparation;
[0040] (4) The presence of the zinc oxide layer or the zinc oxide layer loaded with precious metal nanoparticles in the composite copper foil of the present invention can reduce the formation of dendrites of lithium ions during the charging and discharging process and improve the safety of lithium batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 It is a schematic diagram of the structure of the composite copper foil of the present invention. DETAILED DESCRIPTION
[0042] The following non-limiting examples can enable those skilled in the art to more fully understand the present invention, but do not limit the present invention in any way. The following content is merely an exemplary description of the scope of the present invention, and those skilled in the art can make various changes and modifications to the present invention based on the disclosed content, which should also fall within the scope of the present invention.
[0043] Example 1
[0044] A composite copper foil (structure such as Figure 1 As shown), comprising a polymer layer, a zinc oxide nanolayer containing palladium nanoparticles located on both sides of the polymer layer, and a copper foil layer located on the surface of the zinc oxide nanolayer containing palladium nanoparticles away from the polymer layer (wherein the polymer layer is polyethylene terephthalate PET, with a thickness of 5 μm);
[0045] The preparation process of composite copper foil is as follows:
[0046] (1) Preparation of zinc oxide nanolayer: 0.2195 g of Zn(OAC)2·2H2O was placed in 100 mL of ethanol and stirred to dissolve to prepare a 10 mM zinc acetate alcohol solution; 0.1832 g of ethanolamine was added to make the concentration 30 mM; stirring was continued for 1 h to mix the solution evenly; a layer of zinc acetate sol was formed on the PET film by spraying, and heat-treated at 200°C for 1 h to obtain a PET film with a zinc oxide nanolayer on the surface (i.e., ZnO-PET-ZnO film);
[0047] (2) Loading precious metal nanoparticles: 1 g of palladium chloride was dissolved in 4 mL of concentrated hydrochloric acid, and the volume was fixed to 100 mL with deionized water to prepare a palladium chloride precursor solution; then 200 mL of ethylene glycol solution was preheated to 120° C., stirred and heated for 2 h, 5 mL of the prepared palladium chloride precursor solution was slowly injected, and PVP-K30 was added so that PVP-K30 / Pd (mass ratio) = 1.5 to obtain an ethylene glycol solution of palladium chloride; the ZnO-PET-ZnO film was immersed in the solution, and heated at 150° C. for 2 h to obtain a ZnO-PET-ZnO film loaded with precious metal palladium nanoparticles (i.e., Pd-ZnO-PET-ZnO-Pd film);
[0048] (3) Chemical copper plating: before copper plating, the Pd-ZnO-PET-ZnO-Pd film was cleaned with ethanol for 3-4 times; 1.566 g of copper sulfate pentahydrate, 0.2 g of DMAB, 5 g of SHP and 2 g of EDTA-2Na were added to 100 mL of deionized water, and stirred to fully dissolve to obtain an alkaline chemical copper plating solution; the Pd-ZnO-PET-ZnO-Pd film was immersed in the alkaline chemical copper plating solution, and copper was plated at 80° C. for 1 hour to obtain a composite copper foil;
[0049] (4) Anti-oxidation treatment: The composite copper foil was immersed in an anti-oxidation liquid (a mixture of 1 g / L benzotriazole and 1 g / L benzoic acid) for 5 seconds, and the liquid was squeezed out by a water-collecting roller, dried by hot air at 100°C, and rolled up.
[0050] Example 2
[0051] A composite copper foil, comprising a high molecular polymer layer, a zinc oxide nanolayer containing silver nanoparticles located on both sides of the high molecular polymer layer, and a copper foil layer located on the surface of the zinc oxide nanolayer containing silver nanoparticles away from the high molecular polymer layer (wherein the high molecular polymer layer is polyimide PI with a thickness of 5 μm);
[0052] The preparation process of composite copper foil is as follows:
[0053] (1) Preparation of zinc oxide nanolayer: 0.2876 g of ZnSO4·7H2O was placed in 100 mL of ethanol and stirred to dissolve to prepare a 10 mM zinc acetate alcohol solution; 0.3053 g of ethanolamine was added to make the concentration 50 mM; stirring was continued for 1 h to mix the solution evenly; a layer of zinc acetate sol was formed on the PI film by spraying, and heat-treated at 300°C for 2 h to obtain a PI film with a zinc oxide nanolayer on the surface (i.e., ZnO-PI-ZnO film);
[0054] (2) Loading precious metal nanoparticles: 2.5 g of silver nitrate was dissolved in 4 mL of concentrated hydrochloric acid, and the volume was fixed to 100 mL with deionized water to prepare a silver nitrate precursor solution; then 200 mL of ethylene glycol solution was preheated to 120° C., stirred and heated for 2 h, 5 mL of the prepared silver nitrate precursor solution was slowly injected, and PVP-K30 was added so that PVP-K30 / Pd (mass ratio) = 1.5 to obtain an ethylene glycol solution of silver nitrate; the ZnO-PI-ZnO film was immersed in the solution, and heated at 150° C. for 2 h to obtain a ZnO-PI-ZnO film loaded with precious metal silver nanoparticles (i.e., Ag-ZnO-PI-ZnO-Ag film);
[0055] (3) Chemical copper plating: before copper plating, the Ag-ZnO-PI-ZnO-Ag film was cleaned with ethanol for 3-4 times; 1.566 g of copper sulfate pentahydrate, 0.2 g of DMAB, 5 g of SHP and 2 g of EDTA-2Na were added to 100 mL of deionized water, and stirred to fully dissolve to obtain an alkaline chemical copper plating solution; the Ag-ZnO-PI-ZnO-Ag film was immersed in the alkaline chemical copper plating solution, and copper was plated at 80° C. for 1 h to obtain a composite copper foil;
[0056] (4) Anti-oxidation treatment: The composite copper foil was immersed in an anti-oxidation liquid (a mixture of 1 g / L benzotriazole and 1 g / L benzoic acid) for 5 seconds, and the liquid was squeezed out by a water-collecting roller, dried by hot air at 100°C, and rolled up.
[0057] Example 3
[0058] A composite copper foil, comprising a polymer layer, a zinc oxide nanolayer containing palladium nanoparticles located on both sides of the polymer layer, and a copper foil layer located on the surface of the zinc oxide nanolayer containing palladium nanoparticles away from the polymer layer (wherein the polymer layer is polyethylene terephthalate (PET) with a thickness of 4.5 μm);
[0059] The preparation process of composite copper foil is as follows:
[0060] (1) Preparation of zinc oxide nanolayer: 2.195 g of Zn(OAC)2·2H2O was placed in 100 mL of ethanol and stirred to dissolve to prepare a 100 mM zinc acetate alcohol solution; 0.3154 g of diethanolamine was added to make the concentration 30 mM; the solution was stirred for 1 h to mix the solution evenly; a layer of zinc acetate sol was formed on the PET film by spraying, and the film was heat treated at 200°C for 2 h to obtain a PET film with a zinc oxide nanolayer on the surface (i.e., ZnO-PET-ZnO film);
[0061] (2) Loading precious metal nanoparticles: 1 g of palladium chloride was dissolved in 4 mL of concentrated hydrochloric acid, and the volume was fixed to 100 mL with deionized water to prepare a palladium chloride precursor solution; then 200 mL of ethylene glycol solution was preheated to 120° C., stirred and heated for 2 h, and 20 mL of the prepared palladium chloride precursor solution was slowly injected, and PVP-K30 was added so that PVP-K30 / Pd (mass ratio) = 1.5 to obtain an ethylene glycol solution of palladium chloride; the ZnO-PET-ZnO film was immersed in the solution, and heated at 150° C. for 2 h to obtain a ZnO-PET-ZnO film loaded with precious metal palladium nanoparticles (i.e., Pd-ZnO-PET-ZnO-Pd film);
[0062] (3) Chemical copper plating: before copper plating, the Pd-ZnO-PET-ZnO-Pd film was cleaned with ethanol for 3-4 times; 1.566 g of copper sulfate pentahydrate, 0.2 g of DMAB, 5 g of SHP and 2 g of EDTA-2Na were added to 100 mL of deionized water, and stirred to fully dissolve to obtain an alkaline chemical copper plating solution; the Pd-ZnO-PET-ZnO-Pd film was immersed in the alkaline chemical copper plating solution, and copper was plated at 80° C. for 1 hour to obtain a composite copper foil;
[0063] (4) Anti-oxidation treatment: The composite copper foil was immersed in an anti-oxidation liquid (a mixture of 1 g / L benzotriazole and 1 g / L benzoic acid) for 5 seconds, and the liquid was squeezed out by a water-collecting roller, dried by hot air at 100°C, and rolled up.
[0064] Example 4
[0065] A composite copper foil, comprising a polymer layer, a zinc oxide nanolayer located on both sides of the polymer layer, and a copper foil layer located on the surface of the zinc oxide nanolayer away from the polymer layer (wherein the polymer layer is polyethylene terephthalate (PET) with a thickness of 6 μm);
[0066] The preparation process of composite copper foil is as follows:
[0067] (1) Preparation of zinc oxide nanolayer: 0.6815 g ZnCl2 was placed in 100 mL ethanol, and the mixture was stirred to dissolve to prepare a 50 mM zinc acetate alcohol solution; 0.1832 g ethanolamine was added to make the concentration 30 mM; the mixture was stirred for 1 h to mix the solution evenly; a layer of zinc acetate sol was formed on the PET film by spraying, and the film was heat treated at 300°C for 2 h to obtain a PET film having a zinc oxide nanolayer on the surface (i.e., ZnO-PET-ZnO film);
[0068] (2) Loading precious metal nanoparticles: 1 g of palladium chloride was dissolved in 4 mL of concentrated hydrochloric acid, and the volume was fixed to 100 mL with deionized water to prepare a palladium chloride precursor solution; then 200 mL of ethylene glycol solution was preheated to 120° C., stirred and heated for 2 h, 10 mL of the prepared palladium chloride precursor solution was slowly injected, and PAM was added so that PAM / Pd (mass ratio) = 1.5 to obtain an ethylene glycol solution of palladium chloride; the ZnO-PET-ZnO film was immersed in the solution, and heated at 150° C. for 2 h to obtain a ZnO-PET-ZnO film loaded with precious metal palladium nanoparticles (i.e., Pd-ZnO-PET-ZnO-Pd film);
[0069] (3) Chemical copper plating: before copper plating, the Pd-ZnO-PET-ZnO-Pd film was cleaned with ethanol for 3-4 times; 1.566 g of copper sulfate pentahydrate, 0.2 g of DMAB, 5 g of SHP and 2 g of EDTA-2Na were added to 100 mL of deionized water, and stirred to fully dissolve to obtain an alkaline chemical copper plating solution; the Pd-ZnO-PET-ZnO-Pd film was immersed in the alkaline chemical copper plating solution, and copper was plated at 80° C. for 1 hour to obtain a composite copper foil;
[0070] (4) Anti-oxidation treatment: The composite copper foil was immersed in an anti-oxidation liquid (a mixture of 1 g / L benzotriazole and 1 g / L benzoic acid) for 5 seconds, and the liquid was squeezed out by a water-collecting roller, dried by hot air at 100°C, and rolled up.
[0071] Comparative Example 1
[0072] Compared with Example 1, the only difference is that: no zinc oxide layer is included;
[0073] (1) Roughening: prepare an alkaline roughening solution of 30 g / L KOH + 20 g / L KMnO4, treat at 70 °C for 10 min, and etch nanopores on the surface of the base film;
[0074] (2) Neutralization: 3g / 100L acetic acid aqueous solution, soak for 5min;
[0075] (3) Sensitization: soak in stannous chloride solution, SnCl2 15g / L, add 4mL concentrated hydrochloric acid, soak for 5min at room temperature;
[0076] (4) Pd loading: 0.125 g of PdCl2 was dissolved in 5 mL of concentrated hydrochloric acid, and the volume was made up to 250 mL with deionized water. The treated base film was immersed in the solution for 5 min.
[0077] Comparative Example 2
[0078] Compared with Example 1, the only difference is that the zinc oxide layer does not carry precious metal nanoparticles.
[0079] Comparative Example 3
[0080] Compared with Example 1, the only difference is that: the zinc oxide nanolayer containing palladium nanoparticles is replaced by a zinc oxide nanolayer containing copper nanoparticles;
[0081] The specific operation of step (2) loading copper nanoparticles is as follows:
[0082] 2.9914 g of copper nitrate trihydrate (Cu 2+Concentration 0.02M), 92g glycerol (concentration 1M), 0.3g PVP-K30 (PVP = K30 / Cu = 1:5 mass ratio) and 4g NaOH are mixed, heated to 140°C with stirring, and maintained for 17min to obtain.
[0083] The other steps are the same as in Example 1.
[0084] Comparative Example 4
[0085] Compared with Example 1, the only difference is that 4 mL of the prepared palladium chloride precursor solution is injected.
[0086] Comparative Example 5
[0087] Compared with Example 1, the only difference is that 25 mL of the prepared palladium chloride precursor solution is injected.
[0088] Comparative Example 6
[0089] Compared with Example 1, the only difference is that 4.829 g of Zn(OAC)2·2H2O is put into 100 mL of ethanol to obtain a 220 mM zinc acetate alcohol solution.
[0090] Comparative Example 7
[0091] Compared with Example 1, the only difference is that 0.1098 g of Zn(OAC)2·2H2O is put into 100 mL of ethanol to obtain a 5 mM zinc acetate alcohol solution.
[0092] Composite copper foil performance test:
[0093] (1) The thickness of the copper foil layer of the composite copper foil prepared in the above-mentioned embodiment and comparative example was tested using a step profiler.
[0094] (2) The adhesion between the film layer and the substrate is tested by the 100-grid method. The bonding strength between the copper foil and the substrate is divided into 1-5B levels (as shown in Table 1) with reference to GB / T9286-2021 "Scratching test for paint and varnish films". The general process is: use a multi-blade cutting knife to make 6 parallel cuts on the surface of the material with a spacing of 2mm.
[0095] Table 1 Bonding strength between copper foil and substrate
[0096]
[0097]
[0098] The performance characterization results of the composite copper foil prepared in the comparative examples of each embodiment are shown in Table 2.
[0099] Table 2 Composite copper foil performance characterization results
[0100]
[0101] It can be seen from the above table that the composite copper foil with the zinc oxide layer has a significantly improved bonding force between the copper layer and the base film compared to the composite copper foil without the layer, which improves the processing performance of the composite copper foil; at the same time, it is helpful to improve the thickness uniformity of the copper foil layer obtained by chemical copper plating in the later stage; it can be seen from comparative examples 2 and 3 compared with Example 1 that the addition of precious metal particles improves the electrical conductivity and provides catalytic sites for chemical copper plating in the later stage. After replacing with non-precious metal copper, the conductivity is improved, but it is far less than the effect of loading precious metal particles, and it also has a certain impact on the thickness uniformity of the copper foil; the effect on the adhesion of the composite copper foil is the same; compared with Example 1, when the load of the precious metal is too high, the dispersion is uneven, resulting in a certain degree of decrease in adhesion and thickness uniformity. If it is too low, the copper plating efficiency will be low, and the ability to improve adhesion is insufficient, which cannot meet the needs of chemical copper plating in the later stage; compared with Example 1, if the zinc oxide layer is too thick and easy to fall off, it is not conducive to chemical copper plating in the later stage, resulting in a significant decrease in the thickness uniformity of the copper foil layer, and the oxide layer is too thin, and the adhesion of the composite copper foil cannot be better improved.
[0102] Finally, it should be noted that the above content is only used to illustrate the technical solution of the present invention, rather than to limit the scope of protection of the present invention. Simple modifications or equivalent substitutions of the technical solution of the present invention by ordinary technicians in this field do not deviate from the essence and scope of the technical solution of the present invention.
Claims
1. A composite copper foil for enhancing the adhesion between the copper foil and the substrate, characterized in that: The composite copper foil comprises a polymer layer, a zinc oxide nanolayer loaded with precious metal particles, and a copper foil layer; the zinc oxide nanolayer loaded with precious metal particles is located on both sides of the polymer layer, and the surface of the zinc oxide nanolayer loaded with precious metal particles away from the polymer layer is a copper foil layer; The method for preparing the zinc oxide nanolayer loaded with precious metal particles is as follows: (1) spraying an alcohol solution of zinc salt onto a polymer layer to form a sol of zinc salt, and then subjecting the layer to heat treatment to obtain a polymer layer loaded with zinc oxide nanoparticles; (2) immersing the polymer layer loaded with zinc oxide nanoparticles in a polyol solution containing a noble metal salt and a stabilizer to reduce the noble metal ions to noble metal nanoparticles; The molar ratio of the noble metal salt to the zinc salt is 1:0.25-1.2; The zinc salt is Zn(OAc)2·2H2O; the noble metal salt is palladium chloride; The zinc ion concentration in the alcohol solution of the zinc salt is 10-100 mM; the alcohol solution of the zinc salt comprises a zinc salt, a nitrogen-containing ligand and ethanol; The nitrogen-containing ligand is selected from at least one of triethanolamine, diethanolamine, ethanolamine, tripropanolamine and dipropanolamine.
2. The composite copper foil according to claim 1, characterized in that: The concentration of the nitrogen-containing ligand is 10-100 mM.
3. The composite copper foil according to claim 1, characterized in that: The stabilizer is selected from at least one of cetyltrimethylammonium bromide, polyacrylamide and polyvinylpyrrolidone.
4. The composite copper foil according to claim 1, characterized in that The high molecular polymer in the high molecular polymer layer is at least one selected from polyimide, polyterephthalate and polyphenylene sulfide.