Adhesive composition, adhesive layer and adhesive sheet

By designing adhesive compositions with low dielectric constant and dielectric loss, the problem of insufficient dielectric properties in the high-frequency band is solved, improving the antenna gain and water resistance of millimeter-wave antennas, suppressing radiation loss, and making them suitable for component bonding of millimeter-wave antennas.

CN117693571BActive Publication Date: 2026-11-17NITTO DENKO CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202280051064.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-07-21
Filing Date
2022-07-19
Publication Date
2026-11-17
Estimated Expiration
2042-07-19

AI Technical Summary

Technical Problem

Existing adhesives have high dielectric loss at high frequencies, which cannot meet the requirements of low dielectric constant and low dielectric loss for millimeter-wave antennas. They are also susceptible to moisture, which leads to reduced antenna gain and increased radiation loss.

Method used

An adhesive composition is provided, which has a dielectric constant of 2.0 to 5.0 at frequencies of 28 GHz and 60 GHz, a dielectric loss of 0.0001 to 0.05, a saturated moisture absorption rate of less than 2.8% at 65°C and 90% RH, and a dielectric loss change of less than 0.006, thereby suppressing radiation loss by controlling the dielectric properties and moisture absorption rate.

Benefits of technology

Achieving low dielectric constant and dielectric loss at high frequencies, reducing the influence of moisture, improving antenna gain, and stabilizing and suppressing radiation loss, this technology is suitable for component bonding in millimeter-wave antennas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117693571B_ABST
    Figure CN117693571B_ABST
Patent Text Reader

Abstract

This invention provides an adhesive composition and an adhesive sheet capable of forming an adhesive layer with low dielectric constant and dielectric loss at high frequencies, dielectric properties that are not easily affected by moisture, and suitable for bonding components of millimeter-wave antennas. The adhesive composition of the first aspect of this invention has a dielectric constant of 2.0 to 5.0 at a frequency of 28 GHz, a dielectric loss of 0.0001 to 0.05 at a frequency of 28 GHz, a saturated moisture absorption rate of less than 2.8% at 65°C and 90% RH, and a change in dielectric loss calculated by the following formula of less than 0.006. Change in dielectric loss = D fmax -D fmin .
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to adhesive compositions, adhesive layers, and adhesive sheets. More specifically, it relates to adhesive compositions, adhesive layers, and adhesive sheets suitable for bonding constituent components of millimeter-wave antennas. Background Technology

[0002] In recent years, the communication speed and capacity of portable communication devices such as smartphones have been developing year by year. As the next generation of ultra-high-speed data communication standard, the fifth generation (5G) is expected to achieve 100 times the ultra-high-speed / large-capacity communication, 1 / 10 the low latency, and more than 10 times the number of simultaneous connections compared with the fourth generation (4G).

[0003] To achieve the ultra-high speed / high capacity communication, low latency, and multiple simultaneous connections of 5G as described above, high-frequency electromagnetic waves with frequencies greater than 24 GHz, known as millimeter waves, are used, and the wavelength is shortened to the millimeter level, thus enabling the transmission of large amounts of data at once.

[0004] On the other hand, compared with the frequency band used by 4G, millimeter waves are more easily attenuated by resonance absorption by rain, oxygen in the air, and water molecules, have strong straight-line propagation, and are easy to reflect. Furthermore, the antennas used for millimeter wave communication (hereinafter sometimes referred to as "millimeter wave antennas") require higher antenna gain than those used in traditional 4G communication.

[0005] Patent Document 1 discloses a structure in which a cover member is stacked on a substrate on which an antenna element is provided, as a millimeter-wave antenna mounted on a portable communication device such as a smartphone, and the substrate and the cover member are bonded together using an adhesive.

[0006] As such an adhesive, for example, Patent Document 2 discloses an adhesive containing a polymer obtained by polymerizing a mixture of monomers including 2-ethylhexyl acrylate, a specific alkyl methacrylate, and a hydroxyl-containing monomer, which can form an adhesive layer with a dielectric constant of 3.5 or less at a frequency of 100 kHz.

[0007] In addition, Patent Document 3 discloses an adhesive layer containing a specific acrylic polymer, a vinyl monomer having a polyepoxide chain, a photopolymerization initiator, and a crosslinking agent, and having a relative permittivity of 3.5 or less at a frequency of 1 MHz.

[0008] Existing technical documents

[0009] Patent documents

[0010] Patent Document 1: Japanese Patent Application Publication No. 2019-186942

[0011] Patent Document 2: Japanese Patent Application Publication No. 2015-183178

[0012] Patent Document 3: Japanese Patent Application Publication No. 2020-007570 Summary of the Invention

[0013] The problem that the invention aims to solve

[0014] It is known that the dielectric loss of the raw materials used in the components of a millimeter-wave antenna reduces the amplitude of the millimeter wave. To avoid reducing antenna gain, low dielectric constant, and especially low dielectric loss, is required for millimeter waves at high frequencies. Similarly, the adhesives used to bond the components of the millimeter-wave antenna also require low dielectric constant and low dielectric loss at high frequencies. Furthermore, as mentioned above, water readily absorbs / blocks high-frequency millimeter waves; therefore, the dielectric properties must be resistant to the effects of moisture.

[0015] While the adhesive in Patent Document 2 has a low dielectric constant at low frequencies (100kHz), its dielectric loss at high frequencies is not low enough. Similarly, the adhesive layer in Patent Document 3 also has a low relative dielectric constant at low frequencies (1MHz), but its dielectric loss at high frequencies is not low enough. Furthermore, only the dielectric constant at low frequencies is described, and information on dielectric loss at high frequencies is not disclosed, thus failing to provide a solution to the problem addressed in this application.

[0016] This invention was conceived based on the above-described situation. The object of this invention is to provide an adhesive composition capable of forming an adhesive layer with low dielectric constant and dielectric loss at high frequencies, dielectric properties unaffected by moisture, and suitable for bonding components constituting millimeter-wave antennas. Another object of this invention is to provide an adhesive layer with low dielectric constant and dielectric loss at high frequencies, dielectric properties unaffected by moisture, and suitable for bonding components constituting millimeter-wave antennas. Furthermore, another object of this invention is to provide an adhesive sheet having an adhesive layer with low dielectric constant and dielectric loss at high frequencies, dielectric properties unaffected by moisture, and suitable for bonding components constituting millimeter-wave antennas.

[0017] means for solving problems

[0018] That is, the present invention provides an adhesive composition wherein the dielectric constant of the adhesive composition at a frequency of 28 GHz is 2.0 to 5.0, the dielectric loss of the adhesive composition at a frequency of 28 GHz is 0.0001 to 0.05, the saturated moisture absorption rate of the adhesive composition at 65°C and 90% RH is less than 2.8%, and the change in dielectric loss calculated by the following formula is less than 0.006.

[0019] Change in dielectric loss = D fmax -D fmin

[0020] D fmax The maximum dielectric loss was observed at a frequency of 28 GHz during the period when the adhesive composition was humidified to saturation at 65°C and 90% RH, and then the dielectric loss was tracked over time at 23°C ± 1°C and 52% ± 1% RH.

[0021] D fmin The minimum dielectric loss was observed at a frequency of 28 GHz during the period when the adhesive composition was humidified to saturation at 65°C and 90% RH, and then the dielectric loss was tracked over time at 23°C ± 1°C and 52% ± 1% RH.

[0022] In the above adhesive composition, the dielectric constant is 2.0 to 5.0 at a frequency of 28 GHz. This configuration can improve the antenna gain of the millimeter-wave antenna using the above adhesive composition to bond the constituent components.

[0023] In the above adhesive composition, the dielectric loss at a frequency of 28 GHz is 0.0001 to 0.05, and this configuration can improve the antenna gain of the millimeter-wave antenna using the above adhesive composition to bond the constituent components.

[0024] In the above adhesive composition, the saturated moisture absorption rate is less than 2.8% under the conditions of 65°C and 90%RH. Such a composition has excellent water resistance when used as an adhesive layer in millimeter-wave antennas and the like near room temperature, and can suppress the radiation loss of millimeter waves.

[0025] In the above adhesive composition, the change in dielectric loss at a frequency of 28 GHz is 0.006 or less. This configuration can control the change in dielectric loss caused by moisture absorption to a low level, thereby suppressing millimeter-wave radiation loss. That is, when the change in dielectric loss is 0.006 or less, an adhesive composition with excellent water resistance and the ability to suppress millimeter-wave radiation loss can be obtained.

[0026] In the above-described adhesive composition, the dielectric constant at a frequency of 60 GHz is preferably 2.0 to 5.0. This configuration is preferred from the viewpoint of improving the antenna gain of millimeter-wave antennas using the above-described adhesive composition to bond structural components.

[0027] The present invention also provides an adhesive composition, wherein the dielectric constant of the adhesive composition at a frequency of 60 GHz is 2.0 to 5.0, the dielectric loss of the adhesive composition at a frequency of 60 GHz is 0.0001 to 0.05, the saturated moisture absorption rate of the adhesive composition at 65°C and 90% RH is less than 2.8%, and the change in dielectric loss calculated by the following formula is less than 0.003.

[0028] Change in dielectric loss = D fmax -D fmin

[0029] D fmax The maximum dielectric loss was observed at a frequency of 60 GHz during the period when the adhesive composition was humidified to saturation at 65°C and 90% RH, and then tracked over time at 23°C ± 1°C and 52% ± 1% RH.

[0030] D fmin The minimum dielectric loss was observed at a frequency of 60 GHz during the period when the adhesive composition was humidified to saturation at 65°C and 90% RH, and then tracked over time at 23°C ± 1°C and 52% ± 1% RH.

[0031] In the above adhesive composition, the dielectric constant is 2.0 to 5.0 at a frequency of 60 GHz. This configuration can improve the antenna gain of the millimeter-wave antenna using the above adhesive composition to bond the constituent components.

[0032] In the above adhesive composition, the dielectric loss at a frequency of 60 GHz is 0.0001 to 0.05, and this configuration can improve the antenna gain of the millimeter-wave antenna using the above adhesive composition to bond the constituent components.

[0033] In the above adhesive composition, the saturated moisture absorption rate is less than 2.8% under the conditions of 65°C and 90%RH. Such a composition has excellent water resistance when used as an adhesive layer in millimeter-wave antennas and the like near room temperature, and can suppress the radiation loss of millimeter waves.

[0034] In the above adhesive composition, the change in dielectric loss at a frequency of 60 GHz is less than 0.003. This configuration can control the change in dielectric loss caused by moisture absorption to a low level, thereby suppressing millimeter-wave radiation loss. That is, when the change in dielectric loss is less than 0.003, an adhesive composition with excellent water resistance and the ability to suppress millimeter-wave radiation loss can be obtained.

[0035] Regarding the above adhesive composition, the total light transmittance of the adhesive layer with a thickness of 25 μm is preferably 85% or more.

[0036] Regarding the above adhesive composition, the haze measured for an adhesive layer with a thickness of 25 μm is preferably 1.0% or less.

[0037] The present invention also provides an adhesive layer, wherein the adhesive layer is formed from the above-described adhesive composition.

[0038] The present invention also provides an adhesive sheet, wherein the adhesive sheet has the above-described adhesive layer.

[0039] The present invention also provides a millimeter-wave antenna, the millimeter-wave antenna having at least a substrate and the aforementioned adhesive sheet, wherein the substrate has an antenna element on at least one side, and the adhesive sheet is attached to the side of the substrate having the antenna element.

[0040] Invention Effects

[0041] The adhesive composition and adhesive layer of the present invention exhibit low dielectric constant and dielectric loss in the high-frequency band of millimeter waves, enabling the suppression of millimeter wave radiation loss to a low level. Therefore, by using the adhesive sheet of the present invention to bond the constituent components of a millimeter-wave antenna, a millimeter-wave antenna exhibiting high antenna gain can be efficiently manufactured. Furthermore, the dielectric properties of the adhesive composition of the present invention are not easily affected by moisture. Therefore, millimeter-wave antennas using the adhesive sheet of the present invention are not easily affected by moisture, and millimeter-wave radiation loss can be stably suppressed to a low level. Attached Figure Description

[0042] Figure 1 A schematic diagram (cross-sectional view) illustrating one embodiment of the millimeter-wave antenna of the present invention.

[0043] Figure 2 A schematic diagram (cross-sectional view) illustrating one embodiment of the millimeter-wave antenna of the present invention.

[0044] Figure 3 A schematic diagram (cross-sectional view) illustrating one embodiment of the millimeter-wave antenna of the present invention.

[0045] Figure 4 This is a schematic diagram (sectional view) of the antenna stack used in the evaluation of transmit and receive characteristics. Figure 4 (a) is a side sectional view. Figure 4 (b) is the top projection. Detailed Implementation

[0046] [Adhesive Composition]

[0047] The adhesive composition of the first aspect of the present invention has a dielectric constant of 2.0 to 5.0 at a frequency of 28 GHz, a dielectric loss of 0.0001 to 0.05 at a frequency of 28 GHz, a saturated moisture absorption rate of 2.8% or less under the conditions of 65°C and 90% RH, and a change in dielectric loss of 0.006 or less calculated by the following formula.

[0048] Change in dielectric loss = D fmax -D fmin

[0049] D fmax The maximum dielectric loss was observed at a frequency of 28 GHz during the period when the adhesive composition was humidified to saturation at 65°C and 90% RH, and then the dielectric loss was tracked over time at 23°C ± 1°C and 52% ± 1% RH.

[0050] D fmin The minimum dielectric loss was observed at a frequency of 28 GHz during the period when the adhesive composition was humidified to saturation at 65°C and 90% RH, and then the dielectric loss was tracked over time at 23°C ± 1°C and 52% ± 1% RH.

[0051] The adhesive composition of the second aspect of the present invention has a dielectric constant of 2.0 to 5.0 at a frequency of 60 GHz, a dielectric loss of 0.0001 to 0.05 at a frequency of 60 GHz, a saturated moisture absorption rate of less than 2.8% under the conditions of 65°C and 90% RH, and a change in dielectric loss of less than 0.003 calculated by the following formula.

[0052] Change in dielectric loss = D fmax -D fmin

[0053] D fmax The maximum dielectric loss was observed at a frequency of 60 GHz during the period when the adhesive composition was humidified to saturation at 65°C and 90% RH, and then the dielectric loss was tracked over time at 23°C ± 1°C and 52% ± 1% RH.

[0054] D fmin The minimum dielectric loss was observed at a frequency of 60 GHz during the period when the adhesive composition was humidified to saturation at 65°C and 90% RH, and then the dielectric loss was tracked over time at 23°C ± 1°C and 52% ± 1% RH.

[0055] The adhesive composition of the present invention can have any form, such as solvent-based, emulsion-based, hot-melt-based, solvent-free (active energy ray curing type, such as monomer mixture, or monomer mixture and some of its polymers, etc.).

[0056] The adhesive composition of the present invention, as described above, can be solvent-based, that is, it can contain organic solvents.

[0057] As the aforementioned organic solvents, any organic compound used as a solvent is acceptable. Examples include: hydrocarbon solvents such as cyclohexane, hexane, heptane, and methylcyclohexane; aromatic solvents such as toluene and xylene; ester solvents such as butyl acetate, ethyl acetate, and methyl acetate; ketone solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; and alcohol solvents such as methanol, ethanol, propanol, butanol, and isopropanol. The aforementioned organic solvents can also be mixed solvents containing two or more organic solvents.

[0058] The adhesive composition of the first aspect of the present invention has a low dielectric constant at 28 GHz, which can suppress radiation loss of millimeter waves. The dielectric constant of the adhesive composition of the first aspect of the present invention at a frequency of 28 GHz is 5.0 or less, preferably 4.5 or less, more preferably 4.0 or less, further preferably 3.5 or less, even more preferably 3.4 or less, particularly preferably 3.3 or less, and most preferably 3.2 or less, 3.1 or less, 3.0 or less, or 2.9 or less. The lower limit value is not particularly limited and can be 2.0 or more, or 2.1 or more, or 2.2 or more. Furthermore, the adhesive composition of the second aspect preferably has a dielectric constant at a frequency of 28 GHz within the above-mentioned range.

[0059] In this specification, the dielectric constant is measured using the method described in the examples below. It should be noted that "relative dielectric constant" is the value obtained by dividing "dielectric constant" by "vacuum dielectric constant," which is 1. Therefore, in this specification, "dielectric constant" and "relative dielectric constant" are considered to have the same meaning. Furthermore, the adhesive composition of the first aspect of the present invention and the adhesive composition of the second aspect of the present invention are sometimes collectively referred to as "the adhesive composition of the present invention."

[0060] The adhesive composition of the first aspect of the present invention has a low dielectric loss at 28 GHz, which can suppress the radiation loss of millimeter waves. The dielectric loss of the adhesive composition of the first aspect of the present invention at a frequency of 28 GHz is 0.050 or less, preferably 0.045 or less, more preferably 0.040 or less, further preferably 0.035 or less, even more preferably 0.030 or less, particularly preferably 0.025 or less, and most preferably 0.020 or less. The lower limit value is 0.0001 or more, and may also be 0.0005 or more, or 0.0010 or more. Furthermore, the adhesive composition of the second aspect of the present invention preferably has a dielectric loss at a frequency of 28 GHz within the above-mentioned range.

[0061] The adhesive composition of the second aspect of the present invention has a low dielectric constant at 60 GHz, which can suppress radiation loss of millimeter waves. The dielectric constant of the adhesive composition of the second aspect of the present invention at a frequency of 60 GHz is 5.0 or less, preferably 4.5 or less, more preferably 4.0 or less, further preferably 3.5 or less, even more preferably 3.4 or less, particularly preferably 3.3 or less, and most preferably 3.2 or less, 3.1 or less, 3.0 or less, or 2.9 or less. The lower limit value is not particularly limited and can be 2.0 or more, or 2.1 or more, or 2.2 or more. Furthermore, the dielectric constant of the adhesive composition of the first aspect of the present invention is preferably within the above-mentioned range at a frequency of 60 GHz.

[0062] The adhesive composition of the second aspect of the present invention has a low dielectric loss at 60 GHz, which can suppress the radiation loss of millimeter waves. The dielectric loss of the adhesive composition of the second aspect of the present invention at a frequency of 60 GHz is 0.050 or less, preferably 0.045 or less, more preferably 0.040 or less, further preferably 0.035 or less, even more preferably 0.030 or less, particularly preferably 0.025 or less, and most preferably 0.020 or less, 0.019 or less, 0.018 or less, 0.017 or less, 0.016 or less, 0.015 or less, 0.014 or less, 0.013 or less, or 0.012 or less. The lower limit value of the dielectric loss at a frequency of 60 GHz is 0.0001 or more, and may also be 0.0005 or more, or 0.0010 or more. Furthermore, the adhesive composition of the first aspect of the present invention preferably has a dielectric loss at a frequency of 60 GHz within the above-mentioned range.

[0063] The adhesive composition of the present invention has a low saturated moisture absorption rate, thus suppressing millimeter-wave radiation loss. The saturated moisture absorption rate of the adhesive composition of the present invention at 25°C and 90% RH is preferably 2.8% or less, more preferably 2.7% or less, further preferably 2.6% or less, more preferably 2.5% or less, particularly preferably 2.4% or less, and most preferably 2.3% or less, 2.2% or less, 2.1% or less, 2.0% or less, 1.9% or less, 1.8% or less, 1.7% or less, 1.6% or less, 1.5% or less, 1.4% or less, 1.3% or less, 1.2% or less, 1.1% or less, 1.0% or less, 0.9% or less, 0.8% or less, 0.7% or less, or 0.6% or less. The lower limit of the above-mentioned saturated moisture absorption rate is not particularly limited; for example, it can be 0.3% or more, or 0.4% or more, or 0.5% or more.

[0064] The adhesive composition of the present invention has a saturated moisture absorption rate of 2.8% or less at 65°C and 90% RH, preferably 2.6% or less, more preferably 2.4% or less, even more preferably 2.3% or less, even more preferably 2.2% or less, particularly preferably 2.1% or less, and most preferably 2.0% or less, 1.9% or less, 1.8% or less, 1.7% or less, 1.6% or less, 1.5% or less, 1.4% or less, 1.3% or less, 1.2% or less, 1.1% or less, 1.0% or less, 0.9% or less, 0.8% or less, or 0.7% or less. The lower limit of the above-mentioned saturated moisture absorption rate is not particularly limited; for example, it can be 0.4% or more, or 0.5% or more, or 0.6% or more. When the saturated moisture absorption rate is low under the conditions of 65°C and 90% RH, millimeter-wave radiation loss can be suppressed even when exposed to high-temperature environments while in the state of applying an adhesive layer or the like.

[0065] The saturated moisture absorption rate of the adhesive composition of the present invention at 85°C and 85% RH is preferably 5.0% or less, more preferably 4.0% or less, even more preferably 3.5% or less, even more preferably 3.0% or less, particularly preferably 2.8% or less, and most preferably 2.6% or less, 2.4% or less, 2.2% or less, 2.0% or less, 1.8% or less, 1.6% or less, 1.4% or less, 1.2% or less, 1.0% or less, or 0.8% or less. The lower limit of the above-mentioned saturated moisture absorption rate is not particularly limited; for example, it can be 0.4% or more, 0.5% or more, or 0.6% or more. When the saturated moisture absorption rate is low at 85°C and 85% RH, millimeter-wave radiation loss can be suppressed even when exposed to high-temperature environments while in the state of applying an adhesive layer or the like.

[0066] The aforementioned saturated moisture absorption rate under various temperature and humidity conditions can be calculated, for example, from the weight of the sample in its dry state (w1) and the weight (w2) at the moment when the weight change of the sample disappears (when the moisture absorption rate is saturated) in an atmosphere of 65°C and 90%RH using the following formula. This can be calculated separately under conditions of 25°C and 90%RH and 85°C and 85%RH. It should be noted that the values ​​of w1 and w2 are measured under the same temperature and humidity.

[0067] Saturated moisture absorption rate (%) = {(w2-w1) / w1} × 100

[0068] The change in dielectric loss due to moisture absorption in the adhesive composition of the present invention is controlled at a low level, thus suppressing millimeter-wave radiation loss and its time-dependent changes. The change in dielectric loss due to moisture absorption in the adhesive composition of the first aspect of the present invention at a frequency of 28 GHz is 0.006 or less, preferably 0.005 or less, and more preferably 0.004 or less. There is no particular limitation on the lower limit value of the change in dielectric loss due to moisture absorption at a frequency of 28 GHz; for example, it can be 0.0001 or more, 0.0002 or more, or 0.0003 or more. When the change in dielectric loss is within the above range, millimeter-wave radiation loss can be stably suppressed in environments ranging from room temperature to high temperature when an adhesive layer is applied. Furthermore, the change in dielectric loss due to moisture absorption at a frequency of 28 GHz in the adhesive composition of the second aspect of the present invention is preferably within the above range.

[0069] The adhesive composition of the second aspect of the present invention exhibits a change in dielectric loss due to moisture absorption at a frequency of 60 GHz of 0.003 or less, preferably 0.002 or less, and more preferably 0.001 or less. The lower limit of the saturated moisture absorption rate is not particularly limited, and can be, for example, 0.0001 or more, or 0.0002 or more, 0.0003 or more, 0.0004 or more, 0.0005 or more, 0.0006 or more, 0.0007 or more, 0.0008 or more, or 0.0009 or more. When the change is within the above range, millimeter-wave radiation loss can be stably suppressed in environments ranging from room temperature to high temperature when an adhesive layer is applied. Furthermore, the adhesive composition of the first aspect of the present invention preferably exhibits a change in dielectric loss due to moisture absorption at a frequency of 60 GHz within the above range.

[0070] The changes in dielectric loss at the frequencies of 28 GHz and 60 GHz can be calculated as follows: After maintaining the environment at 65°C and 90% RH for more than 5 days, the environment is returned to 23°C ± 1°C and 52% ± 1% RH (time elapsed = 0 minutes). The dielectric loss at each frequency is measured every 10 minutes from 4 minutes to 180 minutes, and the maximum value (D) is used to calculate the dielectric loss.fmax ) and minimum value (D fmin The change in dielectric loss at frequencies of 28 GHz and 60 GHz can be calculated using the following formula.

[0071] Change in dielectric loss = D fmax -D fmin

[0072] The water vapor transmission of the adhesive composition of the present invention is controlled at a low level, thus suppressing the movement of water molecules in the adhesive composition and reducing variations in millimeter-wave radiation loss. The water vapor transmission of the adhesive composition of the present invention is preferably 430 g / m² at 40°C and 92% RH. 2 For less than / day, 300g / m² is preferred. 2 Less than / day, further preferably 250g / m 2 Less than / day, and more preferably 200g / m 2 For doses below / day, 150g / m² is particularly preferred. 2 For doses below / day, the optimal value is 100g / m 2 Less than / day, 50g / m 2 / day or less or 30g / m 2 Below / day. There is no particular limit to the lower limit of water vapor permeability; for example, it can be 10 g / m². 2 For more than one day, it can also be 20g / m 2 / day or more or 25g / m 2 / day or more.

[0073] The water vapor transmission rate (WVTR) mentioned above is a value determined based on the cup method. The weight of calcium chloride isolated from the outside by the adhesive layer in a dry state (w1) and the weight of the sample at a specified time (when the moisture absorption rate is saturated) after being placed in an atmosphere of 40°C and 92% RH are measured (w2). The weight change is converted to the value per unit time (1 day) and per unit area of ​​the adhesive layer (1 m²). 2 From this, the water vapor permeability can be calculated.

[0074] The changes in dielectric constant or dielectric loss, saturated moisture absorption rate, water vapor transmission rate, and dielectric loss due to moisture absorption of the adhesive composition of the present invention at 28 GHz or 60 GHz can be adjusted by modifying the monomer composition, the type and content of additives, etc. In this specification, the changes in dielectric constant or dielectric loss, saturated moisture absorption rate, water vapor transmission rate, and dielectric loss due to moisture absorption at 28 GHz or 60 GHz were measured by the methods described in the examples below.

[0075] It should be noted that the dielectric constant, dielectric loss, saturated moisture absorption rate, and water vapor transmission rate of the adhesive composition of the present invention refer to the dielectric constant, dielectric loss, saturated moisture absorption rate, and water vapor transmission rate of the adhesive layer formed by the adhesive composition of the present invention.

[0076] There are no particular limitations on the base polymers constituting the adhesive compositions of the present invention. Examples include: acrylic polymers containing acrylic adhesive compositions as base polymers; rubber polymers containing rubber adhesive compositions (natural rubber adhesive compositions, synthetic rubber adhesive compositions, etc.) as base polymers; polysiloxane polymers containing polysiloxane adhesive compositions as base polymers; polyester polymers containing polyester adhesive compositions as base polymers; urethane polymers containing urethane adhesive compositions as base polymers; polyamide polymers containing polyamide adhesive compositions as base polymers; epoxy polymers containing epoxy adhesive compositions as base polymers; vinyl alkyl ether polymers containing vinyl alkyl ether adhesive compositions as base polymers; and fluoropolymers containing fluorinated adhesive compositions as base polymers. Among these, acrylic polymers and rubber polymers are preferred. It should be noted that two or more base polymers can be used alone or in combination.

[0077] Examples of the aforementioned rubber polymers include: natural rubber, styrene-butadiene rubber (SBR), polyisoprene (PIP), polyisobutylene (PIB), butene polymers (using butene (1-butene, cis-2-butene, or trans-2-butene) and / or 2-methylpropylene (isobutylene) as the main monomer), ABA-type block copolymer rubbers and their hydrides, styrene-butadiene-styrene block copolymer rubber (SBS), styrene-isoprene-styrene block copolymer rubber (SIS), styrene-isobutylene-styrene block copolymer rubber (SIBS), styrene-vinyl-isoprene-styrene block copolymer rubber (SVIS), styrene-ethylene-butene-styrene block copolymer rubber (SEBS) as a hydride of SBS, and styrene-ethylene-propylene-styrene block copolymer rubber (SEPS) as a hydride of SIS, etc., among which polyisobutylene is preferred. These rubber polymers can be used alone or in combination of two or more.

[0078] By including mixtures, partial polymers, or copolymers of methacrylate compounds and (meth)acrylate compounds in the aforementioned acrylic polymers, the dielectric constant and dielectric loss at high frequencies can be controlled at low levels, and moisture absorption, a cause of dielectric loss degradation, can be suppressed. Furthermore, the rate of change in dielectric loss caused by moisture absorption can be suppressed. It should be noted that sometimes the "mixtures, partial polymers, or copolymers" of the aforementioned methacrylate compounds and (meth)acrylate compounds are referred to as methacrylate copolymers. Additionally, "methacrylate compound" refers to a compound having a "methacryloyl group," and "(meth)acrylate compound" refers to a compound having at least one of an "acryloyl group" and a "methacryloyl group." Furthermore, "(meth)acrylic acid" refers to either or both of "acrylic acid" and "methacrylic acid."

[0079] The aforementioned partial polymer refers to a composition in which one or more monomer components constituting the above mixture are partially polymerized.

[0080] In this specification, "base polymer" refers to the main component (the component with the largest proportion) of the polymer composition contained in the adhesive composition, typically referring to a component that accounts for more than 50% by mass of the aforementioned polymer composition. Furthermore, in this specification, when referred to as "base polymer," it includes "a mixture of monomeric components constituting the base polymer or a partial polymer of a mixture of monomeric components constituting the base polymer." In this specification, the aforementioned "mixture of monomeric components" includes cases consisting of a single monomeric component and cases consisting of two or more monomeric components. Additionally, the aforementioned "partial polymer of a mixture of monomeric components" refers to a composition in which one or more of the constituent monomeric components of the aforementioned "mixture of monomeric components" are partially polymerized.

[0081] The content of the above-mentioned base polymer in the adhesive composition of the present invention is not particularly limited, but is preferably 75% by mass or more (e.g., 75% by mass to 99.9% by mass), more preferably 85% by mass or more (e.g., 85% by mass to 99.9% by mass).

[0082] The content of the above-mentioned methacrylic acid copolymer in the adhesive composition of the present invention is not particularly limited, but is preferably 75% by mass or more (e.g., 75% by mass to 99.9% by mass), more preferably 85% by mass or more (e.g., 85% by mass to 99.9% by mass).

[0083] [Mixtures, or portions thereof of polymers or copolymers (methacrylic acid copolymers)]

[0084] The adhesive composition of the present invention is a methacrylic adhesive composition in which a mixture, a portion thereof, or a copolymer (methacrylic acid copolymer) is used as the base polymer. The content of the aforementioned methacrylic acid copolymer is not particularly limited, but is preferably 75% by mass or more (e.g., 75% to 99.9% by mass), and more preferably 85% by mass or more (e.g., 85% to 99.9% by mass), relative to 100% of the total amount of the adhesive composition of the present invention.

[0085] Examples of adhesive compositions of the present invention include, for example, water-dispersible compositions (emulsion compositions) in which the above-mentioned copolymer is an essential component, and active energy ray-cured compositions in which the above-mentioned mixture or a portion thereof is an essential component. Among these, compositions in which the mixture or a portion thereof is an essential component are preferred.

[0086] The methacrylic acid copolymers of the present invention comprise methacrylate compounds having a hydrocarbon group having 6 or more carbon atoms and (meth)acrylate compounds having crosslinkable functional groups as constituent monomers.

[0087] <Methacrylate compounds having 6 or more carbon atoms>

[0088] The methacrylate compounds used in the above-mentioned methacrylate copolymers contain hydrocarbon groups with 6 or more carbon atoms. Preferably, the hydrocarbon groups with 6 or more carbon atoms in the above-mentioned methacrylate compounds are aliphatic groups, alicyclic groups, or aromatic groups. These hydrocarbon-containing methacrylate compounds can be used alone or in combination of two or more.

[0089] It is believed that the main structural units of the aforementioned methacrylic acid copolymers are derived from methacrylate compounds and contain α-methyl groups. Therefore, compared with the cases derived from acrylate compounds, the polarization near the main chain is reduced, resulting in a decrease in dielectric loss. In addition, the methacryloyl group is more hydrophobic than the acryloyl group, which suppresses moisture absorption. Therefore, it is possible to suppress the degradation and change in dielectric loss at high frequencies caused by moisture absorption.

[0090] When the aforementioned methacrylate compounds have alicyclic or aromatic groups, they readily exhibit moderate agglomeration force and strong adhesive properties in methacrylate copolymers. Furthermore, increasing the gel fraction facilitates excellent foaming and peel resistance. Additionally, they readily provide moderate flexibility in the adhesive layer, resulting in excellent stress relaxation and excellent height tracking properties.

[0091] When the hydrocarbon group having 6 or more carbon atoms is an aliphatic group, the number of carbon atoms in the hydrocarbon group is preferably 8 or more, more preferably 9 or more, and even more preferably 10 or more. The number of carbon atoms in the hydrocarbon group is preferably 22 or less, more preferably 20 or less, and even more preferably 16 or less.

[0092] Examples of methacrylate compounds with a hydrocarbon group having 6 or more carbon atoms and an aliphatic group include: hexyl methacrylate, heptyl methacrylate, octyl methacrylate, 2-ethylhexyl methacrylate, isooctyl methacrylate, nonyl methacrylate, isononyl methacrylate, decyl methacrylate, isodecanyl methacrylate, undecyl methacrylate, lauryl methacrylate, tridecyl methacrylate, tetradecyl methacrylate, pentadecyl methacrylate, hexadecyl methacrylate, heptadecanyl methacrylate, octadecyl methacrylate, isostearyl methacrylate, stearyl methacrylate, nonadecanyl methacrylate, and eicosyl methacrylate. Among these, lauryl methacrylate, tridecyl methacrylate, and isodecanyl methacrylate are preferred.

[0093] The content of the methacrylate compound with 6 or more carbon atoms and an aliphatic hydrocarbon group in the methacrylate copolymer of the present invention is not particularly limited, but is preferably 25% by mass or more, more preferably 25.0% to 99.5% by mass, further preferably 30.0% to 99.3% by mass, and even more preferably 40.0% to 99.0% by mass, relative to 100% by mass of all structural units. From the viewpoint of reducing dielectric constant and dielectric loss at high frequencies, 25% by mass or more is preferred.

[0094] When the hydrocarbon group having 6 or more carbon atoms is an alicyclic group, the number of carbon atoms in the hydrocarbon group is preferably 6 or more, more preferably 8 or more. The number of carbon atoms in the hydrocarbon group is preferably 22 or less, more preferably 16 or less.

[0095] Methacrylate compounds that have a hydrocarbon group containing an alicyclic ring as having 6 or more carbon atoms include, for example, cycloalkyl methacrylates having cycloalkane rings (cyclopentane ring, cyclohexane ring, cycloheptane ring, cyclooctane ring, etc.), methacrylates having bicyclic hydrocarbon rings (pinene ring, pinene ring, camphene ring, norcamphene ring, norbornene ring, etc.), and methacrylates having tricyclic or more aliphatic hydrocarbon rings (tetrahydrodicyclopentadiene ring, dihydrodicyclopentadiene ring, adamantane ring, tetrahydrotricyclopentadiene ring, dihydrotricyclopentadiene ring, etc.).

[0096] Examples of the aforementioned cycloalkyl methacrylates include: cyclohexyl methacrylate, 3,3,5-trimethylcyclohexyl methacrylate, cycloheptyl methacrylate, and cyclooctyl methacrylate.

[0097] Examples of methacrylates having a bicyclic hydrocarbon ring include: borneol methacrylate and isoborneol methacrylate.

[0098] Examples of methacrylates having three or more hydrocarbon rings include: tetrahydrodicyclopentadienyl methacrylate, tetrahydrodicyclopentadienyloxyethyl methacrylate, tetrahydrotricyclopentadienyl methacrylate, 1-adamantyl methacrylate, 2-methyl-2-adamantyl methacrylate, and 2-ethyl-2-adamantyl methacrylate.

[0099] When the hydrocarbon group having 6 or more carbon atoms is a group containing an aromatic ring, the number of carbon atoms in the hydrocarbon group is preferably 6 to 14, more preferably 6 to 10.

[0100] As methacrylate compounds with a hydrocarbon group containing an aromatic ring having a carbon atom number of 6 or more, examples include compounds having an aromatic carbon ring (e.g., a monocyclic carbon ring such as a benzene ring, a fused carbon ring such as a naphthalene ring, etc.). Specific examples include benzyl methacrylate, phenyl methacrylate, naphthyl methacrylate, and 6-(1,1'-biphenyl-4-yloxy)hexyl methacrylate.

[0101] The total content of methacrylate compounds in the methacrylate copolymers of the present invention, wherein the hydrocarbon groups having 6 or more carbon atoms are alicyclic or aromatic, is not particularly limited, but is preferably 1.0% to 60.0% by mass relative to 100% by mass of all structural units, more preferably 5.0% to 55.0% by mass, and even more preferably 10.0% to 50.0% by mass.

[0102] The aforementioned methacrylate compound may have a (poly)oxyalkylene chain. When a (poly)oxyalkylene chain is present, it is preferable that the ester portion of the methacrylate compound has a hydrocarbon group having 6 or more carbon atoms at its end. The number of oxygen atoms in the (poly)oxyalkylene chain (i.e., the number of repetitions of the alkylene group) is preferably 1 to 10, more preferably 1 to 3. The hydrocarbon group having 6 or more carbon atoms at the end can be any one of an aliphatic group, an alicyclic group, or an aromatic group, preferably an alicyclic group or an aromatic group, and particularly preferably an aromatic group.

[0103] When the methacrylate compound having the above-mentioned (poly)oxyalkylene chain has an aromatic group at its end, the overall polarizability of the repeating unit is reduced, thus effectively reducing dielectric loss in the high-frequency band.

[0104] The content of the methacrylate compound having the above-mentioned (poly)oxyalkylene chain in the methacrylate copolymer of the present invention is not particularly limited, but is preferably 1.0% to 30.0% by mass, more preferably 5.0% to 25.0% by mass, and even more preferably 10.0% to 20.0% by mass, relative to 100% by mass of all structural units.

[0105] The total content of the methacrylate compounds having 6 or more carbon atoms in the above-mentioned methacrylate copolymers is preferably 25% by mass or more, more preferably 25.0% to 99.5% by mass, even more preferably 30.0% to 99.3% by mass, and particularly preferably 40.0% to 99.0% by mass, relative to 100% by mass of all structural units. From the viewpoint of reducing dielectric constant and dielectric loss at high frequencies, 25% by mass or more is preferred.

[0106] <(meth)acrylate compounds containing cross-linkable functional groups>

[0107] The aforementioned methacrylic acid copolymers contain (meth)acrylate compounds with crosslinkable functional groups in the ester portion. Therefore, crosslinking occurs when a crosslinking agent is used, increasing the gel fraction and easily resulting in excellent foaming and peel resistance. Furthermore, good agglomeration force is readily obtained, thus easily achieving strong adhesiveness. In addition, whitening (whitening) of adhesive sheets generated in high humidity environments is easily suppressed.

[0108] The crosslinkable functional groups in the aforementioned (meth)acrylate compounds containing crosslinkable functional groups, from the viewpoint of easily adjusting the gel fraction, can include, for example, hydroxyl, carboxyl, anhydride, glycidyl, and other epoxy-containing groups, isocyanate groups, aziridinyl, etc. Among these, hydroxyl groups are preferred from the viewpoint of easily adjusting the gel fraction. The aforementioned (meth)acrylate compounds containing crosslinkable functional groups can be used alone or in combination of two or more.

[0109] Examples of (meth)acrylate compounds containing crosslinkable functional groups and having hydroxyl groups include: 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, hydroxyoctyl (meth)acrylate, hydroxydecyl (meth)acrylate, hydroxylauryl (meth)acrylate, and 4-hydroxymethylcyclohexyl (meth)acrylate. Among these, 2-hydroxyethyl (meth)acrylate is preferred from the viewpoint of readily obtaining good cohesive strength and reliable adhesive adhesion at high temperatures.

[0110] The content of the (meth)acrylate compound containing crosslinkable functional groups in the methacrylic copolymer of the present invention is preferably 0.1% to 30.0% by mass relative to 100% by mass of all structural units, more preferably 0.2% to 20.0% by mass, even more preferably 0.3% to 10.0% by mass, and particularly preferably 0.5% to 5.0% by mass. From the viewpoint of adjusting the gel fraction, it is preferable to use 0.1% by mass or more, and from the viewpoint of reducing the dielectric constant and dielectric loss at high frequencies, it is preferable to use 30.0% by mass or less.

[0111] <Copolymerizable monomers>

[0112] In addition to the methacrylate compounds having 6 or more carbon atoms and the (meth)acrylate compounds containing crosslinkable functional groups, the aforementioned methacrylate copolymers may also contain copolymerizable monomers. Copolymerizable monomers may be used alone or in combination of two or more.

[0113] Examples of copolymerizable monomers include: acrylate compounds having hydrocarbon groups with 1 to 24 carbon atoms; methacrylate compounds having hydrocarbon groups with 1 to 5 carbon atoms; substituted methylene compounds where all carbons of the repeating unit of the main chain have side chains; heterocyclic monomers; carboxyl-containing monomers; nitrile-containing monomers; isocyanate-containing monomers; amide-containing monomers; amino-containing monomers; alkoxyalkyl esters of (meth)acrylate having alkoxy groups with 5 or fewer carbon atoms; monomers containing sulfonic acid groups; monomers containing phosphate groups; vinyl esters (vinyl acetate, vinyl propionate, etc.); aromatic vinyl compounds (styrene, vinyltoluene, etc.); olefins or dienes (ethylene, propylene, butadiene, isoprene, isobutylene, etc.); vinyl ethers (vinyl alkyl ethers, etc.); vinyl chloride; vinyl alcohol; macromolecular monomers with a weight average molecular weight of 30,000 or less; and polyfunctional monomers having two or more polymerizable functional groups. These can be used alone or in combination of two or more.

[0114] It should be noted that the adhesive composition of the present invention preferably does not contain or substantially does not contain monomers containing acidic groups (e.g., monomers containing carboxyl groups, monomers containing sulfonyl groups, monomers containing phosphate groups, etc.). From the viewpoint of obtaining excellent anti-corrosion effects on antenna elements or wiring, the above configuration is preferred. It should be noted that the content of monomers containing acidic groups relative to the total amount of the above adhesive composition is preferably 0.05% by weight or less (e.g., 0% to 0.05% by weight), more preferably 0.01% by weight or less (e.g., 0% to 0.01% by weight), and even more preferably 0.001% by weight or less (e.g., 0% to 0.001% by weight), and may be substantially absent.

[0115] Among the aforementioned copolymerizable monomers, monomers containing heterocyclic groups, carboxyl groups, amide groups, amino groups, sulfonic acid groups, and phosphate groups are preferred because they readily exhibit moderate cohesive force in the adhesive layer, easily increasing the 180° peel adhesion to glass or acrylic sheets and thus readily achieving strong adhesiveness. From this perspective, they are preferred. From the perspective of preventing metal corrosion, monomers containing heterocyclic groups are even more preferred.

[0116] Examples of methacrylate compounds having 1 to 5 carbon atoms include: methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, amyl methacrylate, isopropyl methacrylate, isobutyl methacrylate, sec-butyl methacrylate, tert-butyl methacrylate, and isoamyl methacrylate.

[0117] Examples of acrylate compounds having hydrocarbon groups having 1 to 24 carbon atoms include: methyl acrylate, ethyl acrylate, propyl acrylate, isopropyl acrylate, butyl acrylate, isobutyl acrylate, sec-butyl acrylate, tert-butyl acrylate, pentyl acrylate, isoamyl acrylate, hexyl acrylate, heptyl acrylate, octyl acrylate, isooctyl acrylate, 2-ethylhexyl acrylate, nonyl acrylate, decyl acrylate, isodecanyl acrylate, undecyl acrylate, dodecyl acrylate, lauryl acrylate, tridecyl acrylate, tetradecyl acrylate, pentadecyl acrylate, hexadecyl acrylate, and heptadecanyl acrylate. Acrylates, octadecyl acrylate, isostearyl acrylate, stearyl acrylate, nonadecanyl acrylate, eicosyl acrylate, cyclohexyl acrylate, 3,3,5-trimethylcyclohexyl acrylate, cycloheptyl acrylate, cyclooctyl acrylate, borneol acrylate, isoborneol acrylate, tetrahydrodicyclopentadienyl acrylate, tetrahydrodicyclopentadienyloxyethyl acrylate, tetrahydrotricyclopentadienyl acrylate, 1-adamantyl acrylate, 2-methyl-2-adamantyl acrylate, 2-ethyl-2-adamantyl acrylate, phenyl acrylate, naphthyl acrylate, 6-(1,1'-biphenyl-4-yloxy)hexyl acrylate, etc.

[0118] The aforementioned heterocyclic monomers are copolymerizable monomers having the following heterocycles: heterocycles with only a nitrogen atom as a heteroatom (pyrrolidine, pyrrole, imidazole, pyrazole, piperidine, pyridine, pyrimidine, pyrrololine, piperazine, pyrazine, etc.), and heterocycles with both nitrogen and oxygen atoms (pyrrolidone, etc.). azole, isotonic Azole, Morpholine, Morpholinone, Piperidone, Lactam (e.g., azines, morpholinidone, succinimide, itaconitumide, etc.), heterocycles with nitrogen and sulfur atoms (thiazole, isothiazole, thiazide), heterocycles with oxygen atoms (lactone, tetrahydrofuran, furan, tetrahydropyran, dioxane, etc.), and heterocycles with sulfur atoms (tetrahydrothiophene, thiophene, tetrahydrothioran, thioran, etc.).

[0119] The methacrylic acid copolymers of the present invention, when containing heterocyclic monomers, can achieve moderate flexibility in the adhesive layer, and readily obtain excellent stress relaxation and excellent height difference following properties.

[0120] Examples of heterocyclic monomers having only nitrogen atoms as heteroatoms include: N-vinylpyridine, N-vinylpiperidone, N-vinylpyrimidine, N-vinylpiperazine, N-vinylpyrazine, N-vinylpyrrole, N-vinylimidazol, N-(meth)acryloylpiperidine, N-(meth)acryloylpyrrolidine, N-vinylpyrazole, etc.

[0121] Examples of heterocyclic monomers having the aforementioned heterocycles with nitrogen and oxygen atoms as heteroatoms include: N-vinyl-2-pyrrolidone, N-methylvinylpyrrolidone, N-(meth)acryloyl-2-pyrrolidone, N-vinyl... azole, N-vinylisothiazoline azole, N-vinylmorpholine, N-vinyl-3-morpholinone, N-vinyl-2-caprolactam, N,N-dimethyl (meth)acrylamide, N,N-diethyl (meth)acrylamide, N-vinyl-1,3- Azine-2-one, N-vinyl-3,5-morpholinidone, N-(meth)acryloyloxymethylenesuccinimide, N-(meth)acryloyloxyhexamethylenesuccinimide, N-(meth)acryloyloxyhexamethylenesuccinimide, N-methylitconimide, N-ethylitconimide, N-butylitconimide, N-octylitconimide, N-2-ethylhexylitconimide, N-cyclohexylitconimide, N-laurylitconimide, etc.

[0122] Examples of heterocyclic monomers having heterocycles containing nitrogen and sulfur atoms as heteroatoms include N-vinylthiazole and N-vinylisothiazole.

[0123] Of these, N-vinyl-2-pyrrolidone is particularly preferred.

[0124] Examples of the aforementioned carboxyl-containing monomers include (meth)acrylic acid, itaconic acid, maleic acid, fumaric acid, crotonic acid, and isocrotonic acid. Additionally, the aforementioned carboxyl-containing monomers also include anhydride-containing monomers such as maleic anhydride and itaconic anhydride. Furthermore, derivatives obtained by ester bonding with itaconic acid, for example, are also possible.

[0125] Examples of the aforementioned nitrile-containing monomers include (meth)acrylonitrile.

[0126] Examples of monomers containing isocyanate groups include ethyl 2-isocyanate of (meth)acrylate.

[0127] Examples of monomers containing amide groups include: (meth)acrylamide; N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dipropyl(meth)acrylamide, N,N-diisopropyl(meth)acrylamide, N,N-di(n-butyl)(meth)acrylamide, N,N-di(tert-butyl)(meth)acrylamide, and other N,N-dialkyl(meth)acrylamides; N-ethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N-butyl(meth)acrylamide, N-n-butyl(meth)acrylamide, and other N-alkyl(meth)acrylamides; N-vinylacetamide and other N-vinylcarboxylic acid amides; monomers having hydroxyl and amide groups, such as N-(2-hydroxy) N-hydroxyalkyl (methyl)acrylamides, such as ethyl(methyl)acrylamide, N-(2-hydroxypropyl(methyl)acrylamide), N-(1-hydroxypropyl(methyl)acrylamide), N-(3-hydroxypropyl(methyl)acrylamide), N-(2-hydroxybutyl(methyl)acrylamide), N-(3-hydroxybutyl(methyl)acrylamide), and N-(4-hydroxybutyl(methyl)acrylamide); monomers having alkoxy and amide groups, such as N-alkoxyalkyl (methyl)acrylamide, N-methoxyethyl (methyl)acrylamide, and N-butoxymethyl (methyl)acrylamide; and N,N-dimethylaminopropyl (methyl)acrylamide, N-(methyl)acryloylmorpholine, etc.

[0128] In addition, the above-mentioned (meth)acrylamide class also includes various N-alkoxyalkyl (meth)acrylamides, such as N-methoxymethyl (meth)acrylamide, N-butoxymethyl (meth)acrylamide, etc.

[0129] Examples of amino-containing monomers mentioned above include: aminoethyl methacrylate, N,N-dimethylaminoethyl methacrylate, and tert-butylaminoethyl methacrylate.

[0130] Examples of alkoxyalkyl esters of (meth)acrylate having an alkoxy group having 5 or fewer carbon atoms include: 2-methoxyethyl ester of (meth)acrylate, 2-ethoxyethyl ester of (meth)acrylate, methoxytriethylene glycol ester of (meth)acrylate, 3-methoxypropyl ester of (meth)acrylate, 3-ethoxypropyl ester of (meth)acrylate, 4-methoxybutyl ester of (meth)acrylate, 4-ethoxybutyl ester of (meth)acrylate, etc.

[0131] Examples of monomers containing sulfonic acid groups include sodium vinyl sulfonate.

[0132] The aforementioned macromonomers are high-molecular-weight monomers polymerized from multiple monomer components. When using macromonomers, structural units derived from the monomer components constituting the macromonomers exist in the base polymer in a manner of certain continuity. Therefore, by using macromonomers, higher-order structures derived from macromonomers can be introduced into the base polymer, and the properties required as adhesives (adhesive strength, cohesive strength, height tracking, etc.) can be easily adjusted. The weight-average molecular weight of the aforementioned macromonomers is preferably 3000–35000, more preferably 4000–30000, even more preferably 5000–25000, and even more preferably 6000–20000.

[0133] Examples of multifunctional monomers having two or more polymerizable functional groups include: hexanediol di(meth)acrylate, butanediol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, trimethylolpropane tri(meth)acrylate, tetramethylolmethane tri(meth)acrylate, allyl methacrylate, ethylene methacrylate, divinylbenzene, polyester acrylates, and urethane acrylates. Multifunctional monomers can be used alone or in combination of two or more.

[0134] The content of the aforementioned multifunctional monomers in the methacrylic acid copolymers of the present invention is not particularly limited, but is preferably 0.5% by mass or less (e.g., 0% to 0.5% by mass), more preferably 0% to 0.35% by mass, and even more preferably 0% to 0.2% by mass, relative to 100% by mass of all structural units. When the content of the aforementioned multifunctional monomers is 0.5% by mass or less, the adhesive layer has moderate cohesive force, and the adhesion and height difference absorption are easily improved, which is therefore preferred. It should be noted that when using a crosslinking agent, the multifunctional monomers may not be used. When a crosslinking agent is not used, the content of the multifunctional monomers is preferably 0.001% to 0.5% by mass, more preferably 0.001% to 0.35% by mass, and even more preferably 0.002% to 0.2% by mass.

[0135] The total content of the copolymerizable monomers in the above-mentioned methacrylic acid copolymers is not particularly limited, but is preferably 30.0% by mass or less, more preferably 15.0% by mass or less, relative to 100% by mass of all structural units.

[0136] The aforementioned methacrylate copolymers can be obtained by mixing or polymerizing a methacrylate compound having 6 or more carbon atoms, a (meth)acrylate compound containing crosslinkable functional groups, and a copolymerizable monomer, or by polymerizing using a known or conventional polymerization method. Examples of such polymerization methods include solution polymerization, emulsion polymerization, bulk polymerization, and polymerization using active energy rays (active energy ray polymerization). From the viewpoints of transparency, water resistance, and cost of the adhesive layer, solution polymerization and active energy ray polymerization are preferred, with active energy ray polymerization being more preferred.

[0137] The active energy rays used for irradiation during the aforementioned active energy ray polymerization (photopolymerization) can include, for example, ionizing radiation such as alpha rays, beta rays, gamma rays, neutron rays, and electron rays, as well as ultraviolet rays, with ultraviolet rays being particularly preferred. Furthermore, there are no particular limitations on the irradiation energy, irradiation time, or irradiation method of the active energy rays, as long as the reaction is sufficient to activate the photopolymerization initiator and produce monomer components.

[0138] In the polymerization of the aforementioned methacrylic acid copolymers, various common solvents can be used. Examples of such solvents include: esters (ethyl acetate, n-butyl acetate, etc.), aromatic hydrocarbons (toluene, benzene, etc.), aliphatic hydrocarbons (n-hexane, n-heptane, etc.), alicyclic hydrocarbons (cyclohexane, methylcyclohexane, etc.), ketones (methyl ethyl ketone, methyl isobutyl ketone, etc.), and other organic solvents. Solvents can be used alone or in combination of two or more.

[0139] In addition, during the polymerization of the aforementioned methacrylic acid copolymers, depending on the type of polymerization reaction, polymerization initiators such as thermal polymerization initiators and photopolymerization initiators (photoinitiators) can be used. Polymerization initiators can be used alone or in combination of two or more.

[0140] There are no particular limitations on the aforementioned photopolymerization initiators. Examples include: benzoin ether photopolymerization initiators, acetophenone photopolymerization initiators, α-keto alcohol photopolymerization initiators, aromatic sulfonyl chloride photopolymerization initiators, photoactive oxime photopolymerization initiators, benzoin photopolymerization initiators, benzoyl photopolymerization initiators, benzophenone photopolymerization initiators, ketal photopolymerization initiators, thioxanone photopolymerization initiators, etc. Photopolymerization initiators can be used alone or in combination of two or more.

[0141] Examples of photopolymerization initiators for the aforementioned benzoin ethers include: benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, benzoin isopropyl ether, benzoin isobutyl ether, 2,2-dimethoxy-1,2-diphenylethane-1-one, and anisonitrile methyl ether. Examples of photopolymerization initiators for the aforementioned acetophenones include: 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxycyclohexylphenyl ketone, 4-phenoxydichloroacetophenone, and 4-(tert-butyl)dichloroacetophenone. Examples of photopolymerization initiators for the aforementioned α-keto alcohols include: 2-methyl-2-hydroxyphenylacetone and 1-[4-(2-hydroxyethyl)phenyl]-2-methylpropane-1-one. Examples of photopolymerization initiators for the aforementioned aromatic sulfonyl chlorides include: 2-naphthalenesulfonyl chloride. Examples of photoactive oxime photopolymerization initiators include 1-phenyl-1,2-propanedione-2-(O-ethoxycarbonyl)oxime. Examples of benzoin-type photopolymerization initiators include benzoin. Examples of benzoinyl-type photopolymerization initiators include benzoin. Examples of benzophenone-type photopolymerization initiators include benzoyl. Examples of benzophenone-type photopolymerization initiators include benzophenone, benzoylbenzoic acid, 3,3'-dimethyl-4-methoxybenzophenone, polyvinylbenzophenone, and α-hydroxycyclohexylphenyl ketone. Examples of ketal-type photopolymerization initiators include benzoindimethyl ketal. Examples of thioxanthone-type photopolymerization initiators include thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-diisopropylthioxanthone, and dodecylthioxanthone.

[0142] There is no particular limitation on the amount of the above-mentioned photopolymerization initiator used. For example, it is preferably 0.001 to 10.0 parts by mass relative to 100 parts by mass of all structural units of the above-mentioned methacrylic acid copolymer, and more preferably 0.01 to 5.0 parts by mass.

[0143] In addition, examples of the aforementioned thermal polymerization initiators include: azo polymerization initiators, peroxide polymerization initiators (e.g., benzoyl peroxide, tert-butyl maleate peroxide, etc.), and redox polymerization initiators. Among these, the azo polymerization initiators disclosed in Japanese Patent Application Publication No. 2002-69411 are preferred. Examples of the aforementioned azo polymerization initiators include: 2,2'-azobisisobutyronitrile (AIBN), 2,2'-azobis-2-methylbutyronitrile (AMBN), dimethyl 2,2'-azobis(2-methylpropionic acid), and 4,4'-azobis-4-cyanopentanoic acid.

[0144] Regarding the amount of the aforementioned thermal polymerization initiator, for example, in the case of the aforementioned azo polymerization initiator, it is preferably 0.05 to 0.5 parts by mass, and more preferably 0.1 to 0.3 parts by mass, relative to 100 parts by mass of all structural units of the aforementioned methacrylic acid copolymer.

[0145] The weight-average molecular weight (Mw) of the copolymer forming the adhesive layer of the present invention is preferably 100,000 to 5,000,000, more preferably 200,000 to 4,000,000, and even more preferably 300,000 to 3,000,000. From the viewpoint of improving adhesion, maintaining properties, and improving foam peel resistance, a composition with a weight-average molecular weight of 100,000 or more is preferred. From the viewpoint of easily improving adhesion and improving foam peel resistance, a composition with a weight-average molecular weight of 5,000,000 or less is preferred.

[0146] The weight-average molecular weight (Mw) of the above copolymer can be determined by polystyrene conversion using GPC. For example, it can be measured using a high-speed GPC apparatus (product name "HPLC-8120GPC", manufactured by Tosoh Corporation) under the following conditions.

[0147] ·Column: TSK gel SuperHZM-H / HZ4000 / HZ3000 / HZ2000

[0148] Solvent: Tetrahydrofuran

[0149] • Flow rate: 0.6 ml / min

[0150] The glass transition temperature (Tg) of the above-mentioned copolymer is preferably -70°C to 100°C, more preferably -65°C to 50°C, and even more preferably -60°C to 10°C. When the glass transition temperature of the above-mentioned methacrylic acid copolymer is above -70°C, the cohesive strength is improved, and the foaming peel resistance is easily improved, which is preferred. Furthermore, when the glass transition temperature is below 100°C, the adhesive composition has moderate flexibility, easily achieving good adhesion, good height difference absorption, and excellent adhesive reliability, which is also preferred.

[0151] The glass transition temperature (Tg) of the above copolymer is the theoretical value expressed by the following FOX formula. In the formula below, Tg represents the glass transition temperature of the above copolymer (unit: K). i The glass transition temperature (in K) of monomer i when it forms a homopolymer is represented by W. i This represents the mass fraction of monomer i in the total monomer composition (i = 1, 2, ..., n).

[0152] 1 / Tg = W1 / Tg1 + W2 / Tg2 + ... + Wn / Tg n

[0153] The following values ​​can be used for the Tg of the homopolymer of the monomer that constitutes the above copolymer.

[0154]

[0155]

[0156] Additionally, the Tg of homopolymers of monomers not described above can be obtained using the values ​​described in the "Polymer Handbook" (3rd edition, John Wiley & Sons, Inc., 1989). Furthermore, the Tg of homopolymers of monomers not described in the aforementioned literature can be obtained using the values ​​obtained by the above-described measurement methods (based on the peak temperature of tanδ from viscoelasticity tests).

[0157] In the polymerization of the aforementioned methacrylic acid copolymers, chain transfer agents can be used to adjust the molecular weight. Examples of such chain transfer agents include: 2-mercaptoethanol, α-thioglycerol, 2,3-dimercapto-1-propanol, octylthiol, tert-nonylthiol, dodecylthiol (laurylthiol), tert-dodecylthiol, glycidylthiol, mercaptoacetic acid, methyl mercaptoacetate, ethyl mercaptoacetate, propyl mercaptoacetate, butyl mercaptoacetate, tert-butyl mercaptoacetate, 2-ethylhexyl mercaptoacetate, octyl mercaptoacetate, isooctyl mercaptoacetate, decyl mercaptoacetate, dodecyl mercaptoacetate, mercaptoacetate of ethylene glycol, mercaptoacetate of neopentyl glycol, mercaptoacetate of pentaerythritol, and α-methylstyrene dimer. From the viewpoint of suppressing whitening of the adhesive sheet caused by humidification, α-thioglycerol and methyl mercaptoacetate are particularly preferred, with α-thioglycerol being especially preferred. Chain transfer agents can be used alone or in combination of two or more.

[0158] Relative to 100 parts by mass of all structural units of the aforementioned methacrylic acid copolymer, the content of the chain transfer agent is preferably 0.1 to 20 parts by mass, more preferably 0.2 to 15 parts by mass, and even more preferably 0.3 to 10 parts by mass. By keeping the content (amount) of the chain transfer agent within the above range, methacrylic acid copolymers with a weight-average molecular weight controlled between 1,000 and 30,000 can be easily obtained.

[0159] The adhesive composition of the present invention preferably contains a crosslinking agent. When a crosslinking agent is present in the adhesive composition, the base polymer undergoes crosslinking, resulting in a higher gel fraction and improved foaming peel resistance. Examples of such crosslinking agents include: isocyanate crosslinking agents, epoxy crosslinking agents, melamine crosslinking agents, peroxide crosslinking agents, urea crosslinking agents, metal alkoxide crosslinking agents, metal chelate crosslinking agents, metal salt crosslinking agents, and carbodiimide crosslinking agents. Crosslinking agents include zoline-based, aziridine-based, and amine-based agents. Among these, isocyanate-based and epoxy-based crosslinking agents are preferred for improving foaming and peel resistance, with isocyanate-based crosslinking agents being even more preferred. Crosslinking agents can be used alone or in combination of two or more.

[0160] Examples of crosslinking agents (polyfunctional isocyanate compounds) for the aforementioned isocyanates include: lower aliphatic polyisocyanates such as 1,2-ethylidene diisocyanate, 1,4-butylidene diisocyanate, and 1,6-hexamethylene diisocyanate; alicyclic polyisocyanates such as cyclopentylene diisocyanate, cyclohexylene diisocyanate, isophorone diisocyanate, hydrogenated toluene diisocyanate, and hydrogenated xylene diisocyanate; and aromatic polyisocyanates such as 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 4,4'-diphenylmethane diisocyanate, and phenylenediamine diisocyanate. In addition, other commercially available products that can be cited as crosslinking agents of the aforementioned isocyanates include: trimethylolpropane / toluene diisocyanate adduct (trade name "Coronate L", manufactured by Nippon Polyurethanes Co., Ltd.), trimethylolpropane / hexamethylene diisocyanate adduct (trade name "Coronate HL", manufactured by Nippon Polyurethanes Co., Ltd.), and trimethylolpropane / phenylenediamine diisocyanate adduct (trade name "Takenate D-110N", manufactured by Mitsui Chemicals Co., Ltd.).

[0161] Examples of epoxy crosslinking agents (multifunctional epoxy compounds) include: N,N,N',N'-tetraglycidyl-m-phenylenediamine, diglycidyl-aniline, 1,3-bis(N,N-diglycidyl-aminomethyl)cyclohexane, 1,6-hexanediol diglycidyl ether, neopentyl glycol diglycidyl ether, ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, and so on. These include sorbitol polyglycidyl ether, glycerol polyglycidyl ether, pentaerythritol polyglycidyl ether, polyglycerol polyglycidyl ether, sorbitan polyglycidyl ether, trimethylolpropane polyglycidyl ether, diglycidyl adipate, diglycidyl phthalate, triglycidyl-tris(2-hydroxyethyl) isocyanurate, resorcinol diglycidyl ether, bisphenol S diglycidyl ether, and epoxy resins having two or more epoxy groups within their molecules. Additionally, commercially available products such as "Tetrad C" (manufactured by Mitsubishi Gas Chemical Co., Ltd.) can be cited as examples of the aforementioned epoxy crosslinking agents.

[0162] The content of the crosslinking agent in the above-described adhesive composition is preferably 0.001 to 10 parts by weight, and more preferably 0.01 to 5 parts by weight, relative to 100 parts by weight of the methacrylic acid copolymer. When the content of the crosslinking agent is 0.001 parts by weight or more, the foaming peel resistance is easily improved, and therefore this is preferred. On the other hand, when the content of the crosslinking agent is 10 parts by weight or less, the adhesive layer has moderate flexibility, and the adhesive strength is easily improved, and therefore this is preferred.

[0163] From the viewpoint of further reducing the dielectric constant and dielectric loss at high frequencies, the adhesive composition of the present invention may contain inorganic microparticles, organic microparticles, and polymer materials other than the base polymer, in addition to the aforementioned base polymer. These can be used alone or in combination of two or more. From the viewpoint of reducing the dielectric constant and dielectric loss at high frequencies, inorganic microparticles and organic microparticles exhibiting insulating properties (insulating fillers) are preferred as the aforementioned inorganic and organic microparticles.

[0164] (Inorganic particles)

[0165] Inorganic microparticles that can be incorporated into the adhesive composition of the present invention include, for example, metal oxides such as silica, alumina, zirconium oxide, and titanium dioxide; metal salts such as aluminum borate and aluminum hydroxide; minerals such as mica; and inorganic microparticles with hollow structures such as hollow nano-silica. They can be used alone or in combination of two or more.

[0166] From the viewpoint of dispersibility in the base polymer, the aforementioned inorganic particles can be surface-treated. Known or conventional surface-treatment agents can be used without limitation, such as silane coupling agents, titanium coupling agents, organic acids, polyols, organosilicones, etc., with silane coupling agents being preferred. Examples of silane coupling agents include: vinyltrimethoxysilane, vinyltriethoxysilane, dimethylvinylmethoxysilane, dimethylvinylethoxysilane, methylvinyldimethoxysilane, methylvinyldiethoxysilane, vinyl-tri(2-methoxy)silane, vinyltriacetoxysilane, 2-methacryloyloxyethyltriethoxysilane, 3-methacryloyloxypropyltrimethoxysilane, 3-methacryloyloxypropyltriethoxysilane, 3-methacryloyloxypropylmethyldimethoxysilane, triethoxyphenylsilane, trimethoxyphenylsilane, dimethoxydiphenylsilane, methyldiethoxyphenylsilane, dimethoxymethylphenylsilane, etc.

[0167] From the viewpoint of low dielectric constant, low dielectric loss, and transparency of the adhesive composition at high frequencies, the particle size (D50) of the aforementioned inorganic microparticles is preferably 1 nm to 100 nm, more preferably 5 nm to 80 nm, and even more preferably 10 nm to 50 nm. The aforementioned median particle size refers to the particle size (median diameter) when the cumulative value in the particle size distribution measured by laser diffraction scattering method is 50%.

[0168] When the adhesive composition of the present invention contains inorganic microparticles, from the viewpoint of low dielectric constant, low dielectric loss, and transparency of the adhesive composition in the high-frequency band, its content relative to 100 parts by weight of the above-mentioned base polymer is preferably 0.01 parts by weight to 30 parts by weight, more preferably 0.05 parts by weight to 25 parts by weight, even more preferably 0.10 parts by weight to 20 parts by weight, even more preferably 0.15 parts by weight to 10 parts by weight, and particularly preferably 0.2 parts by weight to 5 parts by weight.

[0169] (Organic microparticles)

[0170] Examples of organic microparticles that can be incorporated into the adhesive composition of the present invention include: polymers such as styrene resins, acrylic resins, silicone resins, acrylic-styrene resins, vinyl chloride resins, vinylidene chloride resins, amide resins, urethane resins, phenolic resins, styrene-conjugated diene resins, acrylic-conjugated diene resins, olefin resins, and fluoropolymers; or microparticles composed of crosslinks of these polymers; and microparticles composed of these polymers / polymer crosslinks in a hollow structure. They can be used alone or in combination of two or more.

[0171] From the viewpoint of low dielectric constant, low dielectric loss, and transparency of the adhesive composition at high frequencies, the particle size (D50) of the aforementioned organic microparticles is preferably 1 nm to 100 nm, more preferably 5 nm to 80 nm, and even more preferably 10 nm to 50 nm. The aforementioned median particle size refers to the particle size (median diameter) when the cumulative value in the particle size distribution determined by laser diffraction scattering is 50%.

[0172] When the adhesive composition of the present invention contains organic microparticles, from the viewpoint of low dielectric constant, low dielectric loss, and transparency in the high-frequency band of the adhesive composition, its content is generally 0.01 to 30 parts by mass relative to 100 parts by mass of the base polymer, preferably 0.05 to 25 parts by mass, more preferably 0.1 to 20 parts by mass, further preferably 0.15 to 10 parts by mass, and particularly preferably 0.2 to 5 parts by mass.

[0173] (Polymer materials)

[0174] As polymeric materials capable of being incorporated into the adhesive compositions of the present invention, polymeric materials with low dielectric constant, low dielectric loss, and compatibility with the base polymer are preferred. Examples include: fluoropolymers, fluororubbers, fluorinated functional group (meth)acrylates, polyethylene, polypropylene, polystyrene, polycarbonate, norbornene resins or addition copolymers with olefins, polyphenylene ether, bismaleimide-triazine resins, polyetherimides, polyimides, polyetheretherketones (PEEK), liquid crystal polymers, rubber / elastomers, hydrogenated polyolefin resins, terpenes, isoprene, terpene phenol resins, aromatic modified terpene resins, and their hydrogenated resins. These can be used alone or in combination of two or more.

[0175] When the adhesive composition of the present invention contains a polymer material, its content is not particularly limited. From the viewpoint of low dielectric constant, low dielectric loss and transparency in the high frequency band of the adhesive composition, the content is usually 0.01 parts to 50 parts by mass relative to 100 parts by mass of the base polymer, preferably 0.05 parts to 40 parts by mass, and more preferably 0.1 parts to 30 parts by mass.

[0176] (Rust inhibitor)

[0177] The adhesive composition of the present invention may further contain a rust inhibitor. When the adhesive composition contains a rust inhibitor, it is preferable from the viewpoint that excellent corrosion protection can be obtained for antenna elements and metal wiring.

[0178] Rust inhibitors are compounds that prevent metals from rusting and corroding. Examples of rust inhibitors include amine compounds, benzotriazole compounds, and nitrites. Other examples include ammonium benzoate, ammonium phthalate, ammonium stearate, ammonium palmitate, ammonium oleate, ammonium carbonate, dicyclohexylamine benzoate, urea, hexamethylenetetramine, thiourea, phenyl carbamate, and N-cyclohexylcarbamate (CHC). Rust inhibitors can be used alone or in combination of two or more.

[0179] Examples of the aforementioned amine compounds include: hydroxyl-containing amines such as 2-amino-2-methyl-1-propanol, monoethanolamine, monoisopropanolamine, diethylethanolamine, ammonia or ammonia water; cyclic amines such as morpholine; cyclic alkylamines such as cyclohexylamine; and straight-chain alkylamines such as 3-methoxypropylamine. Additionally, examples of nitrites include: dicyclohexylamine nitrite (DICHAN), diisopropylamine nitrite (DIPAN), sodium nitrite, potassium nitrite, and calcium nitrite.

[0180] The content of the aforementioned rust inhibitor is preferably 0.02 to 15 parts by weight relative to 100 parts by weight of the aforementioned base polymer. A content of 0.02 parts by weight or more readily yields good anti-corrosion performance and is therefore preferred. On the other hand, a content of 15 parts by weight or less readily ensures transparency and, moreover, readily ensures adhesive reliability such as resistance to foaming and peeling, and is therefore preferred.

[0181] From the viewpoint that it can achieve a balanced and high level of adhesive reliability, transparency and corrosion resistance to the above-mentioned base polymer, and can obtain excellent appearance, the above-mentioned rust inhibitor is preferably a benzotriazole compound.

[0182] There are no particular limitations on the benzotriazole compounds mentioned above, as long as they have a benzotriazole skeleton. From the viewpoint of obtaining better anti-corrosion effect, it is preferable to have the structure shown in the following formula (1).

[0183]

[0184] (wherein, in the above formula (1), R) 1 and R 2 Same or different, R 1 Substituents on the benzene ring represent alkyl groups with 1 to 6 carbon atoms, alkoxy groups with 1 to 6 carbon atoms, aryl groups with 6 to 14 carbon atoms, amino groups, and single carbon groups. 1-10 Alkylamino or diC 1-10 Alkylamino, amino-C 1-6 Alkyl, mono-C 1-10 Alkylamino-C 1-6 Alkyl or diC 1-10 Alkylamino-C1-6 Alkyl, mercapto, alkoxycarbonyl with 1 to 6 carbon atoms, or alkoxy group with 1 to 6 carbon atoms, etc., when n is an integer from 0 to 4, and n is 2 or more, n R 1 They can be the same or different, R 2 Represents hydrogen atoms, alkyl groups with 1 to 12 carbon atoms, alkoxy groups with 1 to 12 carbon atoms, aryl groups with 6 to 14 carbon atoms, amino groups, and single carbon atoms. 1-10 Alkylamino or diC 1-10 Alkylamino, amino-C 1-6 Alkyl, mono-C 1-10 Alkylamino-C 1-6 Alkyl or diC 1-10 Alkylamino-C 1-6 Substituents include alkyl, mercapto, alkoxycarbonyl (with 1 to 12 carbon atoms), or alkoxy groups (with 1 to 12 carbon atoms).

[0185] From the perspective of achieving superior corrosion resistance, as R 1 Preferably, it is an alkyl group or alkoxycarbonyl group with 1 to 3 carbon atoms, and more preferably a methyl group. Furthermore, n is preferably 0 or 1. From the same viewpoint, as R... 2 Preferably, hydrogen atoms and single carbon atoms are used. 1-10 Alkylamino-C 1-6 Alkyl or diC 1-10 Alkylamino-C 1-6 Alkyl groups, more preferably hydrogen atoms, two C atoms, etc. 1-8 Alkylamino C 1-4 Alkyl groups, etc.

[0186] The content of the aforementioned benzotriazole compound relative to 100 parts by weight of the aforementioned base polymer is preferably 0.02 parts by weight to 3 parts by weight, more preferably 0.02 parts by weight to 2.5 parts by weight, and even more preferably 0.02 parts by weight to 2 parts by weight. When the amount of benzotriazole compound is within a certain range, it can reliably ensure adhesive reliability such as foaming peel resistance, and can also reliably prevent the increase of haze in the adhesive sheet.

[0187] (Silane coupling agent)

[0188] The adhesive composition of the present invention may further contain a silane coupling agent. When a silane coupling agent is contained in the adhesive composition, excellent adhesion to glass is readily obtained (especially excellent adhesive reliability to glass under high temperature and humidity), which is preferred from this perspective.

[0189] Examples of silane coupling agents include γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, γ-aminopropyltrimethoxysilane, and N-phenyl-aminopropyltrimethoxysilane. γ-glycidoxypropyltrimethoxysilane is preferred. Commercially available products, such as "KBM-403" (manufactured by Shin-Etsu Chemical Co., Ltd.), can also be cited as examples. Silane coupling agents can be used alone or in combination of two or more.

[0190] From the viewpoint of improving the adhesive reliability to glass, the content of the silane coupling agent is preferably 0.01 to 1 part by mass relative to 100 parts by mass of the base polymer, and more preferably 0.03 to 0.5 parts by mass.

[0191] (Other additives)

[0192] The adhesive composition of the present invention may contain, as needed and without impairing the properties of the present invention, known additives such as antioxidants, crosslinking accelerators, tackifying resins (rosin derivatives, polyterpene resins, oil-soluble phenols, etc.), anti-aging agents, colorants (pigments or dyes, etc.), ultraviolet absorbers, chain transfer agents, plasticizers, softeners, surfactants, and antistatic agents. These additives may be used alone or in combination of two or more.

[0193] When the adhesive composition of the present invention contains a tackifier, from the viewpoint of imparting adequate adhesion, its content relative to 100 parts by weight of the base polymer is preferably 0.01 parts by weight or more, more preferably 0.05 parts by weight or more. Furthermore, from the viewpoint of avoiding excessively high peel strength, it is preferably 50 parts by weight or less, more preferably 40 parts by weight or less.

[0194] [Adhesive layer]

[0195] The adhesive layer of the present invention is formed from the adhesive composition of the present invention, and therefore exhibits low dielectric constant and low dielectric loss in millimeter waves at high frequencies (28 GHz to 60 GHz). That is, the adhesive layer of the present invention can suppress radiation loss in millimeter waves.

[0196] The adhesive layer of the present invention has a low dielectric constant at 28 GHz, which can suppress radiation loss of millimeter waves, and is therefore preferred from this point of view. The dielectric constant of the adhesive layer of the present invention at a frequency of 28 GHz is preferably 2.0 to 5.0, more preferably 2.05 to 4.5, even more preferably 2.1 to 4.0, even more preferably 2.15 to 3.5, particularly preferably 2.2 to 3.4, and most preferably 2.2 to 3.3, 2.2 to 3.2, 2.2 to 3.1, 2.2 to 3.0, or 2.2 to 2.9.

[0197] The dielectric constant of the adhesive layer of the present invention at 28 GHz can be adjusted by adjusting the type of base polymer, monomer composition, type and content of additives, etc., of the adhesive composition constituting the adhesive layer.

[0198] The dielectric loss of the adhesive layer of the present invention is controlled at a low level at 28 GHz, which can suppress the radiation loss of millimeter waves, and is therefore preferred. The dielectric loss of the adhesive layer of the present invention at a frequency of 28 GHz is preferably 0.050 or less, more preferably 0.045 or less, even more preferably 0.040 or less, even more preferably 0.035 or less, particularly preferably 0.030 or less, and most preferably 0.025 or less or 0.020 or less. The lower limit value is not particularly limited, but is preferably 0.0001 or more, and may also be 0.0005 or more or 0.0010 or more.

[0199] The dielectric loss of the adhesive layer of the present invention at 28 GHz can be adjusted by adjusting the type of base polymer, monomer composition, type and content of additives, etc., of the adhesive composition constituting the adhesive layer.

[0200] The adhesive layer of the present invention has a low dielectric constant at 60 GHz, which can suppress the radiation loss of millimeter waves, and is therefore preferred. The dielectric constant of the adhesive layer of the present invention at a frequency of 60 GHz is preferably 2.0 to 5.0, more preferably 2.1 to 4.5, even more preferably 2.2 to 4.0, even more preferably 2.2 to 3.5, particularly preferably 2.2 to 3.4, and most preferably 2.2 to 3.3, 2.2 to 3.2, 2.2 to 3.1, 2.2 to 3.0, or 2.2 to 2.9.

[0201] The dielectric constant of the adhesive layer of the present invention at 60 GHz can be adjusted by adjusting the type of base polymer, monomer composition, type and content of additives, etc., of the adhesive composition constituting the adhesive layer.

[0202] The adhesive layer of the present invention preferably controls the dielectric loss at 60 GHz to a low level, which is preferred from the viewpoint of suppressing radiation loss of millimeter waves. The dielectric loss of the adhesive layer of the present invention at a frequency of 60 GHz is preferably 0.050 or less, more preferably 0.045 or less, further preferably 0.040 or less, even more preferably 0.035 or less, particularly preferably 0.030 or less, and most preferably 0.025 or less or 0.020 or less. The lower limit value of the dielectric loss at a frequency of 60 GHz is preferably 0.0001 or more, and can be 0.0005 or more or 0.0010 or more.

[0203] The dielectric loss of the adhesive layer of the present invention at 60 GHz can be adjusted by adjusting the type of base polymer, monomer composition, type and content of additives, etc., of the adhesive composition constituting the adhesive layer.

[0204] The adhesive layer of the present invention is transparent or has transparency. Therefore, it exhibits excellent visual legibility and appearance when viewed through the adhesive composition described above. Consequently, the adhesive layer of the present invention is suitable for optical applications.

[0205] The haze of the adhesive layer of the present invention (according to JIS K7136) is not particularly limited, but is preferably 1.2% or less, more preferably 1.1% or less, even more preferably 1.0% or less, even more preferably 0.9% or less, and particularly 0.8% or less. Excellent transparency and excellent appearance are easily obtained when the haze is, for example, 1.2% or less. The haze can be measured, for example, as follows: the adhesive layer thickness is 25 μm, it is left to stand at normal temperature (23°C, 50% RH) for at least 24 hours, and then it is bonded to a glass slide (e.g., a glass slide with a total transmittance of 91.8% and a haze of 0.4%) as a sample, and measured using a haze meter (product name "HM-150", manufactured by Murakami Color Technology Research Institute Co., Ltd.).

[0206] The total transmittance (according to JIS K7361-1) of the adhesive layer in the visible light wavelength region of the present invention is preferably 85% or more, more preferably 88% or more, further preferably 89% or more, even more preferably 90% or more, particularly preferably 91% or more, and most preferably 92% or more. When the total transmittance is 85% or more, excellent transparency and excellent appearance are easily obtained. The above-mentioned total transmittance can be measured, for example, as follows: the adhesive layer thickness is 25 μm, it is left to stand at normal temperature (23°C, 50% RH) for at least 24 hours, then the spacer is peeled off with the spacer in place, and the adhesive layer is bonded to a glass slide (e.g., a glass slide with a total transmittance of 91.8% and a haze of 0.4%) as a sample, and the haze is measured using a haze meter (product name "HM-150", manufactured by Murakami Color Technology Research Institute Co., Ltd.).

[0207] The haze and total transmittance of the adhesive layer of the present invention can be adjusted by adjusting the monomer composition, the type and content of additives, etc.

[0208] The gel fraction (proportion of insoluble components) of the adhesive layer of the present invention is preferably 30% to 95%, more preferably 35% to 90%, further preferably 40% to 85%, even more preferably 45% to 80%, and particularly preferably 50% to 75%. When the gel fraction is 30% or more, the cohesive force of the adhesive layer is improved, and indentation is less likely to occur during processing. In addition, foaming and peeling at the interface with the adhered object are suppressed under high temperature conditions, and excellent foaming and peeling resistance is easily obtained, so it is preferred. When the gel fraction is 95% or less, moderate softness can be obtained, and the adhesiveness and height difference conformability are further improved. In addition, it is less likely to absorb foreign matter, so it is preferred.

[0209] The gel fraction (the proportion of solvent-insoluble components) mentioned above can be calculated, for example, as described below.

[0210] Approximately 0.1 g of the adhesive layer was taken, wrapped in a porous PTFE sheet (trade name "NTF1122", manufactured by Nitto Denko Corporation) with an average pore size of 0.2 μm, and then secured with kite string. The mass at this point was measured and recorded as the mass before impregnation (Z). This mass before impregnation is the total mass of the adhesive layer, the PTFE sheet, and the kite string. Additionally, the combined mass of the PTFE sheet and the kite string was measured beforehand and recorded as the bag mass (Y).

[0211] Next, the item (referred to as the "sample"), with the adhesive layer wrapped in a tetrafluoroethylene sheet and secured with kite string, was placed in a 50 ml container filled with ethyl acetate or toluene and left to stand at 23°C for 7 days. Then, the sample (after ethyl acetate treatment) was removed from the container, transferred to an aluminum cup, and dried in a desiccator at 130°C for 2 hours to remove the ethyl acetate or toluene. The mass was then measured and recorded as the post-impregnation mass (X). The gel fraction was then calculated using the following formula.

[0212] Gel fraction (%) = {(XY) / (ZY)} × 100

[0213] The gel fraction of the adhesive layer of the present invention can be controlled, for example, by controlling the monomer composition, weight-average molecular weight, amount of crosslinking agent used, and the types and amounts of other additives used.

[0214] The storage modulus of the adhesive layer of the present invention at 25°C is preferably 0.01 MPa or more, more preferably 0.02 MPa or more, even more preferably 0.03 MPa or more, even more preferably 0.04 MPa or more, particularly preferably 0.05 MPa or more, and most preferably 0.10 MPa or more. When the storage modulus is 0.01 MPa or more, indentation is less likely to occur during processing, and good adhesive reliability is easily obtained, therefore it is preferred. Furthermore, from the viewpoint of height difference tracking and foreign matter absorption, the storage modulus of the adhesive layer at 25°C is preferably 5 MPa or less, more preferably 4.5 MPa or less, even more preferably 4.0 MPa or less, even more preferably 3.5 MPa or less, particularly preferably 3.0 MPa or less, and most preferably 2.5 MPa or less or 2.0 MPa or less. The storage modulus of the adhesive layer is a value measured when dynamic viscoelasticity is applied at a frequency of 1 Hz. The above-mentioned storage modulus is the real part of the shear modulus expressed as a complex number, and can be converted to tensile modulus by taking into account the Poisson's ratio of the sample.

[0215] The energy storage modulus of the adhesive layer of the present invention can be controlled by monomer composition, weight-average molecular weight, amount of crosslinking agent used (addition amount), and the type and amount of other additives.

[0216] The 300% tensile residual stress of the adhesive layer in this invention is not particularly limited, but is preferably 2 N / cm. 2 ~24N / cm 2 More preferably 2.5 N / cm 2 ~20N / cm 2 Further preferred is 3N / cm 2 ~16N / cm 2 The residual stress after 300% tensile stress is 2 N / cm. 2 At the above levels, good resistance to foaming and peeling is easily obtained, and the residual stress at 300% tensile strength is 24 N / cm. 2 The following conditions allow for good stress relaxation and easy achievement of good elevation difference tracking, making it the preferred option.

[0217] When the 300% tensile residual stress of the adhesive layer of the present invention is within the above range, excellent stress relaxation properties are easily obtained, and excellent height difference following properties are easily achieved. For example, even for large height differences (about 45 μm, for example, 20 μm to 50 μm height), it can follow well.

[0218] The aforementioned 300% tensile residual stress is calculated as follows: At 23°C and 50% RH, the adhesive layer is stretched along its length to an elongation (strain) of 300%. Maintaining this elongation, the tensile load applied to the adhesive layer 300 seconds after the stretching is completed is calculated. This tensile load is then divided by the initial cross-sectional area of ​​the adhesive layer (the cross-sectional area before stretching) to obtain the value (N / cm²). 2 It should be noted that the initial elongation of the adhesive layer is 100%.

[0219] The 300% tensile residual stress of the adhesive layer of the present invention can be controlled by the monomer composition of the base polymer, the weight-average molecular weight, the amount of crosslinking agent used (added amount), and the types and amounts of other additives.

[0220] The adhesive layer of the present invention can suppress millimeter-wave radiation loss by controlling the saturated moisture absorption rate at a low level. The saturated moisture absorption rate of the adhesive layer of the present invention under conditions of 25°C and 90% RH is preferably 2.8% or less, more preferably 2.7% or less, further preferably 2.6% or less, more preferably 2.5% or less, particularly preferably 2.4% or less, and most preferably 2.3% or less, 2.2% or less, 2.1% or less, 2.0% or less, 1.9% or less, 1.8% or less, 1.7% or less, 1.6% or less, 1.5% or less, 1.4% or less, 1.3% or less, 1.2% or less, 1.1% or less, 1.0% or less, 0.9% or less, 0.8% or less, 0.7% or less, or 0.6% or less. A low saturated moisture absorption rate under conditions of 25°C and 90% RH can suppress millimeter-wave radiation loss near room temperature. There is no particular limitation on the lower limit of the saturated moisture absorption rate; for example, it can be above 0.3%, above 0.4%, or above 0.5%.

[0221] The saturated moisture absorption rate of the adhesive layer of the present invention under conditions of 65°C and 90% RH is preferably 2.8% or less, more preferably 2.6% or less, even more preferably 2.4% or less, even more preferably 2.3% or less, particularly preferably 2.2% or less, and most preferably 2.1% or less, 2.0% or less, 1.9% or less, 1.8% or less, 1.7% or less, 1.6% or less, 1.5% or less, 1.4% or less, 1.3% or less, 1.2% or less, 1.1% or less, 1.0% or less, 0.9% or less, 0.8% or less, or 0.7% or less. The lower limit of the saturated moisture absorption rate is not particularly limited; for example, it can be 0.4% or more, 0.5% or more, or 0.6% or more. When the saturated moisture absorption rate is low under conditions of 65°C and 90% RH, millimeter-wave radiation loss can be suppressed even when exposed to high-temperature environments.

[0222] The saturated moisture absorption rate of the adhesive layer of the present invention under conditions of 85°C and 85%RH is preferably 5.0% or less, more preferably 4.0% or less, even more preferably 3.5% or less, even more preferably 3.0% or less, particularly preferably 2.8% or less, and most preferably 2.6% or less, 2.4% or less, 2.2% or less, 2.0% or less, 1.8% or less, 1.6% or less, 1.4% or less, 1.2% or less, 1.0% or less, or 0.8% or less. The lower limit of the saturated moisture absorption rate is not particularly limited; for example, it can be 0.4% or more, 0.5% or more, or 0.6% or more. When the saturated moisture absorption rate is low under conditions of 85°C and 85%RH, millimeter-wave radiation loss can be suppressed even when exposed to high-temperature environments.

[0223] The aforementioned saturated moisture absorption rate under various temperature and humidity conditions can be calculated, for example, from the weight of the sample in its dry state (w1) and the weight (w2) at the moment when the weight change of the sample disappears (when the moisture absorption rate is saturated) in an atmosphere of 65°C and 90%RH using the following formula. This can be calculated separately under conditions of 25°C and 90%RH and 85°C and 85%RH. It should be noted that the values ​​of w1 and w2 are measured under the same temperature and humidity.

[0224] Saturated moisture absorption rate (%) = {(w2-w1) / w1} × 100

[0225] The adhesive layer of the present invention can suppress millimeter-wave radiation loss by controlling the change in dielectric loss due to moisture absorption to a low level. The change in dielectric loss due to moisture absorption at a frequency of 28 GHz is preferably 0.006 or less, more preferably 0.005 or less, and even more preferably 0.004 or less. The lower limit of the saturated moisture absorption rate is not particularly limited, and for example, it can be 0.0001 or more, 0.0002 or more, or 0.0003 or more.

[0226] The change in dielectric loss of the adhesive layer of the present invention due to moisture absorption at a frequency of 60 GHz is preferably 0.003 or less, more preferably 0.002 or less, and even more preferably 0.001 or less. The lower limit of the saturated moisture absorption rate is not particularly limited, and for example, it can be 0.0001 or more, or 0.0002 or more, 0.0003 or more, 0.0004 or more, 0.0005 or more, 0.0006 or more, 0.0007 or more, 0.0008 or more, or 0.0009 or more.

[0227] The changes in dielectric loss at the aforementioned frequencies of 28 GHz and 60 GHz can be calculated as follows: After maintaining the environment at 65°C and 90% RH for more than 5 days, and then returning to conditions of 23°C ± 1°C and 52% ± 1% RH (time = 0 minutes), the dielectric loss at each frequency is measured every 10 minutes from 4 minutes to 180 minutes. The maximum value among these values ​​(D...) fmax ) and minimum value (D fmin The change in dielectric loss at frequencies of 28 GHz and 60 GHz can be calculated using the following formula.

[0228] Change in dielectric loss = D fmax -D fmin

[0229] The adhesive layer of the present invention can suppress millimeter-wave radiation loss by controlling water vapor transmission at a low level. The water vapor transmission of the adhesive layer of the present invention is preferably 430 g / m² at 40°C and 92% RH. 2 For less than / day, 300g / m² is preferred. 2 Less than / day, further preferably 250g / m 2 Less than / day, and more preferably 200g / m 2 For doses below / day, 150g / m² is particularly preferred. 2 For doses below / day, the optimal value is 100g / m 2 Less than / day, 50g / m 2 / day or less or 30g / m 2 Below / day. When the water vapor permeability is low under conditions of 40°C and 92% RH, the water resistance of the adhesive layer is improved, which can suppress the radiation loss of millimeter waves in the adhesive layer. There is no particular limitation on the lower limit of water vapor permeability; for example, it can be 10 g / m². 2 For more than one day, it can also be 20g / m 2 / day or more or 25g / m 2 / day or more.

[0230] The water vapor transmission rate (WVTR) mentioned above is based on the cup method. The weight (w1) of the calcium chloride in its dry state, isolated from the outside by the adhesive layer, and the weight (w2) of the sample after a specified time (when the moisture absorption rate is saturated) at 40°C and 92% RH were measured. The weight change was converted to per unit time (1 day) and per unit area (1 m²). 2 ), thereby determining the water vapor permeability.

[0231] The dielectric constant or dielectric loss, saturated moisture absorption rate, water vapor permeability, and changes in dielectric loss caused by moisture absorption of the adhesive layer of the present invention at 28 GHz or 60 GHz can be adjusted by adjusting the monomer composition, the type and content of additives, etc.

[0232] The thickness of the adhesive layer in this invention is not particularly limited, but is preferably 10 μm to 500 μm, more preferably 11 μm to 400 μm, and even more preferably 12 μm to 350 μm or 12 μm to 300 μm. When the thickness is above a certain value, height difference tracking and adhesive reliability are easily improved. Furthermore, when the thickness is below a certain value, foreign matter is less likely to be absorbed during processing, and it tends to have excellent manufacturability.

[0233] There are no particular limitations on the manufacturing method of the above-mentioned adhesive layer. For example, the adhesive composition can be applied (coated) to a substrate or release liner, and then dried and cured as needed, or dried and cured at the same time. Curing can be carried out by irradiation with active energy rays, heating and drying, etc.

[0234] It should be noted that the coating (coating) of the above-mentioned adhesive composition can be performed using known coating methods. Coating machines such as gravure roller coaters, reverse roller coaters, contact roller coaters, dip roller coaters, bar coaters, doctor blade coaters, spray coaters, comma coaters, and direct coaters can be used.

[0235] [Adhesive sheet]

[0236] The adhesive sheet of the present invention only needs to have the adhesive layer of the present invention, and there are no other particular limitations.

[0237] The adhesive sheet of the present invention can be a double-sided adhesive sheet with adhesive layer surfaces on both sides, or a single-sided adhesive sheet with adhesive layer surfaces on only one side. From the viewpoint of bonding two components together, a double-sided adhesive sheet is preferred. It should be noted that the term "adhesive sheet" in this specification also includes strip-shaped adhesive sheets, i.e., "adhesive tape." Furthermore, in this specification, the adhesive layer surface is sometimes referred to as the "adhesive surface."

[0238] The adhesive sheet of the present invention can have a spacer (release liner) provided on the adhesive surface until it is used.

[0239] The adhesive sheet of the present invention can be a so-called "substrate-free type" adhesive sheet (hereinafter sometimes referred to as "substrate-free adhesive sheet") without a substrate (substrate layer), or it can be an adhesive sheet with a substrate (hereinafter sometimes referred to as "substrate-supported adhesive sheet"). Examples of the aforementioned substrate-free adhesive sheet include, for instance, a double-sided adhesive sheet containing only the aforementioned adhesive layer, and a double-sided adhesive sheet containing the aforementioned adhesive layer and an adhesive layer other than the aforementioned adhesive layer (sometimes referred to as "other adhesive layers"). On the other hand, examples of substrate-supported adhesive sheets include adhesive sheets having the aforementioned adhesive layer on at least one side of the substrate. Among these, a substrate-free adhesive sheet (substrate-free double-sided adhesive sheet) is preferred, and the aforementioned substrate-free double-sided adhesive sheet containing only the adhesive layer is more preferred. Furthermore, an adhesive sheet having the aforementioned adhesive layer on both sides of the substrate (substrate-supported double-sided adhesive sheet) is also preferred. The adhesive layers on both sides of the aforementioned substrate-supported double-sided adhesive sheet can both be the adhesive layer of the present invention, or one can be the adhesive layer of the present invention and the other can be another adhesive layer. It should be noted that the aforementioned "substrate (substrate layer)" does not include the spacer that is peeled off during the use (application) of the adhesive sheet.

[0240] To avoid millimeter-wave radiation loss due to the substrate, the adhesive sheet of the present invention is preferably a substrate-free adhesive sheet. However, when the substrate is made of a material with low dielectric constant and low dielectric loss, a substrate-supported adhesive sheet may also be used. The substrate is preferably usable regardless of the polarization state of the millimeter waves, therefore a non-stretchable substrate is preferred, and isotropic substrates are particularly preferred.

[0241] The adhesive sheet of the present invention does not have particular limitations on the 180° peel adhesion force (especially the 180° peel adhesion force of the adhesive surface of the glass plate provided by the adhesive layer of the present invention) at a tensile speed of 300 mm / min on the glass plate. If the adhesion force is high, a sufficient tight fit can be obtained for the antenna element. From this point of view, the 180° peel adhesion force is preferably 3 N / 20 mm or more, more preferably 3.5 N / 20 mm or more, further preferably 4 N / 20 mm or more, further more preferably 5 N / 20 mm or more, particularly preferably 6 N / 20 mm or more, and most preferably 7 N / 20 mm or more, 8 N / 20 mm or more, 9 N / 20 mm or more, or 10 N / 20 mm or more. If the above-mentioned peel adhesion force is above a certain value, the adhesion of the glass and the suppression of the bulging of the height difference are even better. It should be noted that the upper limit of the 180° peel adhesive force of the adhesive sheet of the present invention at a tensile speed of 300 mm / min on a glass plate is not particularly limited. For example, it is preferably 30 N / 20 mm or less, more preferably 25 N / 20 mm or less, further preferably 22 N / 20 mm or less, even more preferably 20 N / 20 mm or less, particularly preferably 19 N / 20 mm or less, and most preferably 18 N / 20 mm or less, 17 N / 20 mm or less, 16 N / 20 mm or less, 15 N / 20 mm or less, 14 N / 20 mm or less, 13 N / 20 mm or less, 12 N / 20 mm or less, or 11 N / 20 mm or less. The 180° peel adhesive force at a tensile speed of 300 mm / min on a glass plate can be determined by the following method for measuring 180° peel adhesive force.

[0242] Examples of the aforementioned glass sheets include, for instance, "Soda lime glass #0050" (manufactured by Matsunami Glass Industry Co., Ltd.). Other examples include alkali-free glass and chemically strengthened glass.

[0243] The 180° peel adhesive force of a glass plate at a tensile speed of 300 mm / min can be determined by the following method. The adhesive side of the adhesive sheet is attached to the substrate and pressed under a 2 kg roller with one reciprocating pressing action. The sheet is then cured for 30 minutes at 23°C and 50% RH. Following JIS Z0237, the adhesive sheet is peeled from the substrate at 23°C and 50% RH, with a tensile speed of 300 mm / min and a peel angle of 180°. The 180° peel adhesive force (N / 20 mm) is then measured.

[0244] The 180° peel adhesive force of the adhesive sheet of the present invention can be controlled by the monomer composition, weight-average molecular weight of the base polymer (acrylic polymer), the amount of crosslinking agent used (added amount), and the types and amounts of other additives.

[0245] The thickness (total thickness) of the adhesive sheet of the present invention is not particularly limited, but is preferably 10 to 500 μm, more preferably 11 μm to 400 μm, even more preferably 12 μm to 350 μm, and even more preferably 12 μm to 300 μm. When the thickness is above a certain value, peeling at height difference areas is less likely to occur. Furthermore, when the thickness is below a certain value, it is easier to maintain an excellent appearance during manufacturing. It should be noted that the thickness of the adhesive sheet of the present invention does not include the thickness of the spacer.

[0246] The haze of the adhesive sheet of the present invention (according to JIS K7136) is not particularly limited, but is preferably 1.2% or less, more preferably 1.1% or less, even more preferably 1.0% or less, even more preferably 0.9% or less, and particularly preferably 0.8% or less. When the haze is 1.2% or less, excellent transparency and excellent appearance are easily obtained. The above-mentioned haze can be measured, for example, by making the adhesive layer thickness 25 μm, letting it stand at normal temperature (23°C, 50% RH) for at least 24 hours, and then bonding it to a glass slide (e.g., total transmittance 91.8%, haze 0.4%) as a sample, and measuring it using a haze meter (product name "HM-150", manufactured by Murakami Color Technology Research Institute Co., Ltd.).

[0247] The total transmittance (according to JIS K7361-1) of the adhesive sheet of the present invention in the visible light wavelength region is preferably 85% or more, more preferably 88% or more, further preferably 89% or more, even more preferably 90% or more, particularly preferably 91% or more, and most preferably 92% or more. When the total transmittance is 85% or more, excellent transparency and excellent appearance are easily obtained. The above-mentioned total transmittance can be measured, for example, as follows: the adhesive layer thickness is 25 μm, it is left to stand at normal temperature (23°C, 50% RH) for at least 24 hours, and then the spacer is peeled off with the spacer in place. The adhesive layer is then bonded to a glass slide (e.g., total transmittance 91.8%, haze 0.4%) as a sample, and the haze is measured using a haze meter (product name "HM-150", manufactured by Murakami Color Technology Research Institute Co., Ltd.).

[0248] The haze and total transmittance of the adhesive layer of the present invention can be adjusted by adjusting the monomer composition, the type and content of additives, etc.

[0249] The adhesive sheet of the present invention is not particularly limited, and it is preferably manufactured according to a known or conventional manufacturing method. For example, when the adhesive sheet of the present invention is a substrate-free adhesive sheet, it is obtained by forming the adhesive layer on the spacer using the above method. In addition, when the adhesive sheet of the present invention is a substrate-supported adhesive sheet, it can be obtained by directly forming the adhesive layer on the surface of the substrate (direct forming method); or by first forming the adhesive layer on the spacer and then transferring (laminating) it to the substrate to provide the adhesive layer on the substrate (transfer method).

[0250] The adhesive sheet of the present invention may have other layers besides the adhesive layer described above. Examples of other layers include other adhesive layers (adhesive layers other than the adhesive layer described above (adhesive layers other than the adhesive layer formed by the adhesive composition of the present invention)), intermediate layers, and primer layers. It should be noted that the adhesive sheet of the present invention may have two or more other layers.

[0251] Examples of substrates for the adhesive sheet of the present invention, when the adhesive sheet is not attached to the substrate, include various optical films such as plastic films, anti-reflective (AR) films, polarizing plates, and retardation plates. Examples of raw materials for the aforementioned plastic films include polyester resins such as polyethylene terephthalate (PET), (meth)acrylic resins such as polymethyl methacrylate (PMMA), polycarbonate, triacetyl cellulose (TAC), polysulfone, polyarylate, polyimide, polyvinyl chloride, polyvinyl acetate, polyethylene, polypropylene, ethylene-propylene copolymer, cyclic olefin polymers such as "ARTON" (a cyclic olefin polymer manufactured by JSR Corporation) and "ZEONOR" (a cyclic olefin polymer manufactured by Zeon Corporation of Japan), and fluoropolymers. It should be noted that these plastic materials can be used alone or in combination of two or more. Furthermore, the term "substrate" refers to the portion of the adhesive sheet that is attached to the substrate along with the adhesive layer when the adhesive sheet is attached to the substrate. The spacer (release liner) that is peeled off during the use (application) of the adhesive sheet is not included in the "substrate".

[0252] The aforementioned substrate is preferably transparent. The total transmittance of the aforementioned substrate in the visible light wavelength region (according to JISK 7361-1) is preferably 85% or more, more preferably 88% or more, further preferably 89% or more, even more preferably 90% or more, particularly preferably 91% or more, and most preferably 92% or more. Furthermore, the haze of the aforementioned substrate (according to JISK 7136) is preferably 1.0% or less, more preferably 0.8% or less. Examples of such transparent substrates include PET films, non-oriented films such as those with the trade name "ARTON" and "ZEONOR". Non-oriented films are particularly preferred because their characteristics do not depend on the direction of the millimeter-wave electric field.

[0253] The thickness of the aforementioned substrate is not particularly limited, but is preferably 12 μm to 500 μm. It should be noted that the substrate can be either single-layer or multi-layer. Furthermore, the surface of the substrate can be subjected to conventional surface treatments, such as physical treatments like corona discharge treatment, plasma treatment, and electron beam treatment, or chemical treatments like primer treatment.

[0254] The adhesive sheet of the present invention can have spacers (release liner) on the adhesive surface until use. It should be noted that when the adhesive sheet of the present invention is a double-sided adhesive sheet, each adhesive surface can be protected by two spacers respectively, or a single spacer with both sides as release surfaces can be used for protection in a rolled-up form. The spacers serve as protective materials for the adhesive layer and are peeled off when attached to the substrate. Furthermore, when the adhesive sheet of the present invention is a substrate-free adhesive sheet, the spacers also function as supports for the adhesive layer. It should be noted that spacers may also be unnecessary.

[0255] As the aforementioned spacer, conventional release paper or similar materials can be used without particular limitation. Examples include: substrates with a release layer, low-adhesion substrates containing fluoropolymers, and low-adhesion substrates containing non-polar polymers. Examples of substrates with a release layer include plastic films and papers obtained by surface treatment with release agents such as polysiloxanes, long-chain alkyl groups, fluorinated types, and molybdenum sulfide. Examples of fluoropolymers in the aforementioned low-adhesion substrates containing fluoropolymers include: polytetrafluoroethylene, polychlorotrifluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride, tetrafluoroethylene-hexafluoropropylene copolymer, and chlorofluoroethylene-vinylidene fluoride copolymer. Furthermore, examples of non-polar polymers include: olefin resins (e.g., polyethylene, polypropylene), and polyester substrates (polyethylene terephthalate substrates, polyethylene naphthalate substrates, polybutylene terephthalate substrates, etc.). It should be noted that the spacer can be formed using known or conventional methods. In addition, there are no particular restrictions on the thickness of the spacers.

[0256] The adhesive sheet of the present invention exhibits excellent adhesion and resistance to foaming and peeling due to the adhesive layer of the present invention. Furthermore, it demonstrates excellent stress relaxation properties and excellent height difference tracking. Therefore, it exhibits excellent adhesive reliability, particularly at high temperatures. Additionally, it has excellent appearance.

[0257] Therefore, the adhesive sheet of the present invention can be usefully used for bonding components that are prone to foaming at the interface at high temperatures. For example, polymethyl methacrylate (PMMA) resin sometimes contains unreacted monomers and is prone to foaming due to foreign matter at high temperatures. In addition, polycarbonate (PC) is prone to releasing water and carbon dioxide at high temperatures. The adhesive sheet of the present invention has excellent resistance to foaming and peeling, and therefore can also be effectively used for plastic substrates containing such resins.

[0258] Furthermore, the adhesive sheet of the present invention can be effectively used not only for adherends with small coefficients of linear expansion, but also for adherends with large coefficients of linear expansion. It should be noted that examples of adherends with small coefficients of linear expansion include, for instance, glass plates (with a coefficient of linear expansion of 0.3 × 10⁻⁶). -5 / ℃~0.8×10 -5 / ℃), polyethylene terephthalate substrate (PET film, linear expansion coefficient of 1.5×10 -5 / ℃~2×10 -5 / ℃), etc. Furthermore, as substrates with a high coefficient of linear expansion, examples include resin substrates with a high coefficient of linear expansion; more specifically, examples include polycarbonate resin substrates (PC, with a coefficient of linear expansion of 7×10⁻⁶). -5 / ℃~8×10 -5 / ℃), polymethyl methacrylate resin substrate (PMMA, linear expansion coefficient is 7×10 -5 / ℃~8×10 -5 / ℃), cyclic olefin polymer substrate (COP, linear expansion coefficient is 6×10) -5 / ℃~7×10 -5 / ℃), product name "ZEONOR" (manufactured by Japan Zeon Corporation), product name "ARTON" (manufactured by JSR Corporation), etc.

[0259] The adhesive sheet of the present invention can be effectively used for bonding substrates with small coefficients of linear expansion to substrates with large coefficients of linear expansion. Specifically, the adhesive sheet of the present invention is preferably used for bonding glass substrates (e.g., glass plates, chemically strengthened glass, glass lenses, etc.) to the aforementioned resin substrates with large coefficients of linear expansion.

[0260] As described above, the adhesive sheet of the present invention is useful for bonding various raw materials together, and is particularly effective for bonding glass and plastic substrates. It should be noted that the plastic substrate can be an optical film such as a plastic film having an ITO (indium and tin oxide) layer on its surface.

[0261] Furthermore, the adhesive sheet of the present invention can be effectively used not only for substrates with smooth surfaces, but also for substrates with surface height differences. In particular, even if at least one of the glass substrate and the aforementioned resin substrate with a high coefficient of linear expansion has a surface height difference, the adhesive sheet of the present invention can be effectively used for bonding the glass substrate to the aforementioned resin substrate with a high coefficient of linear expansion.

[0262] The adhesive sheet of the present invention is preferably used in the manufacture of portable electronic devices. Examples of such portable electronic devices include: mobile phones, PHS devices, smartphones, tablet computers, mobile computers, portable information terminals (PDAs), electronic notebooks, portable televisions, portable radios and other portable transmitters and receivers, portable game consoles, portable audio players, portable DVD players, digital cameras and other cameras, and portable camcorders.

[0263] The adhesive sheet of the present invention is preferably used, for example, for attaching components and modules of portable electronic devices to each other, and for fixing components and modules of portable electronic devices to a housing. More specifically, examples include attaching cover glass, lenses (especially glass lenses) to touch panels, touch sensors, and antenna modules; fixing cover glass, lenses (especially glass lenses) to a housing; fixing display panels to a housing; fixing antenna modules to a housing; fixing input devices such as keypads and touch panels to a housing; attaching protective panels of information display sections to a housing; attaching housings to each other; attaching housings to decorative sheets; and fixing and attaching various components and modules of portable electronic devices. It should be noted that, in this specification, a display panel refers to a structure consisting of at least a lens (especially a glass lens) and a touch panel. Furthermore, the concept of a lens in this specification includes both transparent bodies that refract light and transparent bodies that do not refract light. That is, the lens in this specification also includes simple window panels that do not refract light.

[0264] Furthermore, the adhesive sheet of the present invention is preferably used for optical applications. That is, the adhesive sheet of the present invention is preferably an optical adhesive sheet for optical applications. More specifically, for example, it is preferably used for bonding optical components (for bonding optical components), manufacturing articles using the above-mentioned optical components (optical articles), etc.

[0265] As an optical component, examples include optical components having at least the aforementioned adhesive sheet and substrate, wherein the substrate has at least one side with metal electrodes and wiring (e.g., copper, silver, ITO wiring, etc.), and the adhesive layer of the present invention is adhered to the side of the substrate having the metal electrodes and wiring. It should be noted that the aforementioned adhesive sheet may have a spacer on the adhesive surface until use, but the adhesive sheet in the optical component of the present invention is an adhesive sheet for use and therefore does not have a spacer.

[0266] Furthermore, the optical component preferably has the adhesive layer on the side of the substrate opposite to the side having the metal electrode and wiring, and more preferably the adhesive layer is attached to the side of the substrate opposite to the side having the metal electrode and wiring.

[0267] Examples of materials constituting the aforementioned metal electrodes and wiring include: titanium, silicon, niobium, indium, zinc, tin, gold, silver, copper, aluminum, cobalt, chromium, nickel, lead, iron, palladium, platinum, tungsten, zirconium, tantalum, hafnium, and other metal oxides such as ITO (oxide of indium and tin), zinc oxide, and tin oxide. Additionally, materials containing two or more of these metals or metal oxides, and alloys with these metals as the main component, can also be listed. From the viewpoint of conductivity, gold, silver, copper, and ITO are preferred; from the viewpoint of conductivity and cost, silver, copper, and ITO are more preferred; and from the viewpoint of transparency, ITO is further preferred. That is, the aforementioned metal electrodes and wiring are preferably silver, copper, or ITO wiring, and particularly preferably ITO wiring. It should be noted that the materials constituting the millimeter-wave antenna elements described later are also preferred. To prevent reduced visual visibility due to metal reflection and for the purpose of concealing the electrodes and / or wiring, the aforementioned metal electrodes and wiring can also be blackened by forming a coating of the metal such as a nitride, oxide, or sulfide.

[0268] Optical components refer to components that have optical properties (such as polarization, refraction, scattering, reflection, transmission, absorption, diffraction, rotation, visual recognition, electromagnetic wave transmission, etc.). Examples of substrates constituting the aforementioned optical components include: substrates constituting display devices (image display devices), input devices, and other equipment (optical devices), antenna modules, or substrates used in these devices. Examples include: polarizing plates, wavelength plates, retardation plates, optical compensation films, brightness enhancement films, light guide plates, reflective films, antireflective films, antenna substrates, hard-coated films (films obtained by hard coating at least one side of a plastic film such as PET film), transparent conductive films (e.g., plastic films with an ITO layer on the surface (preferably PET-ITO, polycarbonate, cyclic olefin polymer, etc. ITO films)), appearance design films, decorative films, surface protection plates, prisms, lenses, color filters, transparent substrates (glass sensors, glass display panels (LCDs, etc.), glass substrates with transparent electrodes, etc.), and substrates further laminated with these (sometimes collectively referred to as "functional films"). Furthermore, these films may have metal nanowire layers, conductive polymer layers, etc. Additionally, these films may have fine metal lines screen-printed on them. Furthermore, these films may contain antenna elements. It should be noted that the terms "plate" and "film" mentioned above encompass plate-like, membrane-like, and sheet-like forms, respectively. For example, "polarizing film" includes "polarizing plate" and "polarizing film," etc. In addition, "film" includes membrane sensors, etc.

[0269] To prevent reduced visual recognition due to metal reflection and for concealment purposes, the aforementioned fine metal wires can be blackened by forming a coating of nitrides, oxides, sulfides, or other metals.

[0270] Examples of display devices include liquid crystal displays (LCDs), organic EL (electroluminescent) displays, PDPs (plasma display panels), and electronic paper. Examples of input devices include touch panels. Furthermore, examples of antenna modules include millimeter-wave antennas, which will be described later.

[0271] Examples of substrates constituting the aforementioned optical components include substrates comprising glass, (meth)acrylic resins, polycarbonate, polyethylene terephthalate, cyclic olefin polymers, metal films, etc. (e.g., sheet-like, film-like, plate-like substrates, etc.). It should be noted that the "optical component" in this invention, as described above, also includes components that maintain the visual recognizability of the display device and input device while serving a decorative and protective function (such as appearance design films, decorative films, surface protective films, etc.).

[0272] If the adhesive sheet of the present invention is an adhesive sheet with a substrate and the adhesive sheet constitutes a component with optical properties, then the substrate can be regarded as the substrate and the adhesive sheet can be referred to as the optical component of the present invention.

[0273] The adhesive sheet of the present invention is an adhesive sheet with a substrate. When the above-mentioned functional film is used as the substrate, the adhesive sheet of the present invention can be used as an "adhesive-type functional film" having the above-mentioned adhesive layer on at least one side of the functional film.

[0274] [Millimeter-wave antenna]

[0275] The adhesive sheet of the present invention, having an adhesive layer (the adhesive layer of the present invention) with low dielectric constant and low dielectric loss in high-frequency bands such as millimeter waves, can suppress the radiation loss of millimeter waves. Therefore, the adhesive sheet of the present invention is useful for bonding components constituting antennas (millimeter-wave antennas) used in millimeter-wave communication.

[0276] In this specification, "millimeter wave communication" refers to communication in the frequency band of 20 GHz to 300 GHz.

[0277] As components constituting a millimeter-wave antenna, examples include a substrate (hereinafter sometimes referred to as a "millimeter-wave antenna substrate") having at least one side of an antenna element (hereinafter sometimes referred to as a "millimeter-wave antenna element") for transmitting and receiving millimeter waves.

[0278] As a substrate for millimeter-wave antennas, the plastic film used in the substrate of the adhesive sheet described above can be used as an example. From the viewpoint of suppressing the radiation loss of millimeter waves, raw materials with low dielectric constant and low dielectric loss are preferred, and cyclic olefin polymers such as "ARTON" (manufactured by JSR Corporation) and "ZEONOR" (manufactured by Zeon Corporation) are particularly preferred.

[0279] From the viewpoint of suppressing radiation loss of millimeter waves, the dielectric constant of the millimeter wave antenna substrate at 28 GHz and / or 60 GHz is preferably 2.0 to 5.0, more preferably 2.1 to 4.5, even more preferably 2.2 to 4.0, even more preferably 2.2 to 3.5, particularly preferably 2.2 to 3.4, and most preferably 2.2 to 3.3, 2.2 to 3.2, 2.2 to 3.1 or 2.2 to 3.0. Furthermore, from the viewpoint of suppressing the radiation loss of millimeter waves, the dielectric loss of the millimeter wave antenna substrate at 28 GHz and / or 60 GHz is preferably 0.0001 to 0.05, more preferably 0.001 to 0.029, even more preferably 0.002 to 0.028, even more preferably 0.003 to 0.027, particularly preferably 0.004 to 0.026, and most preferably 0.005 to 0.025, 0.006 to 0.024, 0.007 to 0.023, 0.008 to 0.022, 0.009 to 0.021, 0.010 to 0.020, 0.011 to 0.019, 0.012 to 0.018, 0.013 to 0.017, 0.014 to 0.016, or 0.014 to 0.015.

[0280] The millimeter-wave antenna substrate is preferably transparent. The total transmittance of the millimeter-wave antenna substrate in the visible light wavelength region (according to JIS K7361) is preferably 85% or more, more preferably 88% or more, further preferably 89% or more, even more preferably 90% or more, particularly preferably 91% or more, and most preferably 92% or more. Furthermore, the haze of the millimeter-wave antenna substrate (according to JIS K7136) is not particularly limited, but is preferably 1.2% or less, more preferably 1.1% or less, even more preferably 1.0% or less, even more preferably 0.9% or less, and particularly preferably 0.8% or less.

[0281] From the viewpoint of suppressing millimeter-wave radiation loss while mounting millimeter-wave antenna elements, the thickness of the millimeter-wave antenna substrate is preferably 5μm to 250μm. It should be noted that the millimeter-wave antenna substrate can have any shape, whether single-layer or multi-layered. Furthermore, the surface of the millimeter-wave antenna substrate can be appropriately subjected to commonly known surface treatments such as physical treatments like corona discharge treatment and plasma treatment, chemical treatments like primer treatment, and coating layers like hard coating.

[0282] As a millimeter-wave antenna element in a millimeter-wave antenna substrate, there are no particular restrictions as long as it can transmit and receive millimeter waves. From the perspective of effectively receiving millimeter waves using portable communication devices such as smartphones, phased array antennas are preferred. A phased array antenna is an antenna that achieves transmission and reception in a desired direction by arranging multiple antenna elements in an array and controlling the phase of each antenna element. That is, regardless of the antenna's orientation, a phased array antenna can transmit or receive radio waves in a desired direction by electronically controlling the phase of each antenna element (beam control).

[0283] As millimeter-wave antenna elements, known antennas can be used without particular restrictions, such as: loop antenna structures, patch antenna structures, stacked patch antenna structures, patch antenna structures with parasitic elements, inverted-F antenna structures, slot antenna structures, planar inverted-F antenna structures, monopole, dipole, and helical antenna structures, Yagi (Yagi / Uda) antenna structures, surface-integrated waveguide structures, and antenna elements with resonant elements formed by hybrids of these designs. Different types of millimeter-wave antenna elements can be used for combinations of different frequency bands. From the viewpoint of effectively receiving millimeter waves in portable communication devices such as smartphones, a phased array antenna with patch antenna elements arranged in an array is preferred.

[0284] There are no particular limitations on the raw materials used to construct millimeter-wave antenna elements. Examples include: titanium, silicon, niobium, indium, zinc, tin, gold, silver, copper, aluminum, cobalt, chromium, nickel, lead, iron, palladium, platinum, tungsten, zirconium, tantalum, hafnium, and other metal oxides such as ITO (oxide of indium and tin), zinc oxide, and tin oxide. Furthermore, materials containing two or more of these metals or metal oxides, and alloys with these metals as the main component, can also be included. From the viewpoint of conductivity, silver, copper, and ITO are preferred; from the viewpoint of transparency and visual visibility, ITO is more preferred. That is, the aforementioned millimeter-wave antenna elements are particularly preferably made of ITO.

[0285] In addition, when the antenna element is made of metals such as silver or copper, in order to conceal the antenna element by preventing a decrease in visual recognition caused by metal reflection, a blackening treatment can be carried out by forming a coating of the metal such as nitride, oxide, or sulfide.

[0286] Furthermore, the millimeter-wave antenna substrate can have transmission line paths for transmitting signals from the millimeter-wave antenna element to the transmitter / receiver circuitry. These transmission line paths can include coaxial cable paths, microstrip transmission lines, stripline transmission lines, edge-coupled microstrip transmission lines, edge-coupled stripline transmission lines, waveguide structures for transmitting signals through the millimeter-wave band (e.g., coplanar waveguides or grounded coplanar waveguides), and transmission lines formed by combinations of these types of transmission lines. There are no particular limitations on the raw materials used to construct the transmission line paths; raw materials used to construct millimeter-wave antenna elements can be used.

[0287] As components constituting a millimeter-wave antenna, examples include cover components that are stacked on the millimeter-wave antenna substrate to protect the millimeter-wave antenna elements arranged on the substrate. For example, optical films such as glass or plastic films can be used as cover components.

[0288] Raw materials used for plastic films include, for example: polyester resins such as polyethylene terephthalate (PET); (meth)acrylic resins such as polymethyl methacrylate (PMMA); polycarbonate; triacetyl cellulose (TAC); polysulfone; polyarylate; polyimide; transparent polyimide; polyvinyl chloride; polyvinyl acetate; fluoropolymers; polyolefin resins such as polyethylene, polypropylene, and ethylene-propylene copolymers; and cyclic olefin polymers such as those marketed under the trade names "ARTON" (manufactured by JSR Corporation) and "ZEONOR" (manufactured by Zeon Corporation). These plastic materials can be used alone or in combination of two or more.

[0289] From the viewpoint of suppressing radiation loss of millimeter waves, the dielectric constant of the cover member at 28 GHz and / or 60 GHz is preferably 2.0 to 5.0, more preferably 2.1 to 4.5, even more preferably 2.2 to 4.0, even more preferably 2.2 to 3.5, particularly preferably 2.2 to 3.4, and most preferably 2.2 to 3.3, 2.2 to 3.2, 2.2 to 3.1 or 2.2 to 3.0. Furthermore, from the perspective of suppressing the radiation loss of millimeter waves, the dielectric loss of the cover member at 28 GHz and / or 60 GHz is preferably 0.0001 to 0.050, more preferably 0.001 to 0.02, even more preferably 0.002 to 0.019, even more preferably 0.003 to 0.018, particularly preferably 0.004 to 0.017, and most preferably 0.005 to 0.016, 0.006 to 0.015, 0.007 to 0.014, 0.008 to 0.013, 0.009 to 0.012 or 0.010 to 0.011.

[0290] The aforementioned cover member is preferably transparent. The total transmittance of the cover member in the visible light wavelength region (according to JISK 7361-1) is preferably 85% or more, more preferably 88% or more, further preferably 89% or more, even more preferably 90% or more, particularly preferably 91% or more, and most preferably 92% or more. Furthermore, the haze of the cover member (according to JISK 7136) is preferably 1.2% or less, more preferably 1.1% or less, even more preferably 1.0% or less, even more preferably 0.9% or less, and particularly preferably 0.8% or less.

[0291] From the viewpoint of suppressing millimeter-wave radiation loss, the thickness of the cover member is preferably 0.025 mm to 1.5 mm. It should be noted that the cover member can have any shape, whether single-layer or multi-layered. Furthermore, the surface of the cover member can be appropriately subjected to known and conventional surface treatments such as physical treatments like corona discharge treatment and plasma treatment, chemical treatments like primer treatment, and coatings like hard coating.

[0292] The adhesive sheet of the present invention is preferably used in the manufacture of millimeter-wave antennas for use in portable communication devices. Examples of such portable communication devices include: mobile phones, PHS, smartphones, tablet computers, mobile computers, portable information terminals (PDAs), etc.

[0293] Millimeter-wave antennas can have components other than the aforementioned millimeter-wave antenna substrate, cover component, and adhesive sheet. For example, they can include polarizing plates, wavelength plates, phase retardation plates, optical compensation films, brightness enhancement films, light guide plates, reflective films, anti-reflective films, hard coatings, transparent conductive films, appearance design films, decorative films, surface protection plates, prisms, lenses, color filters, transparent substrates, and image display panels (e.g., liquid crystal display panels, organic EL panels, plasma display panels, etc.). The image display panel can also include a touch sensor.

[0294] Millimeter-wave antennas can be positioned anywhere on a portable communication device, specifically on the front, back, or sides. It's important to note that the front of a portable communication device refers to the side facing the user when using the device; for example, the side with the display panel is the front. The back and sides are considered part of the casing. It should also be noted that the display panel refers to a structure consisting of at least a lens (particularly a glass lens) and a touch panel.

[0295] There are no limitations on the size (width) of millimeter-wave antennas; they can be formed on an entire surface of a portable communication device or configured on a portion of it. Furthermore, there are no particular limitations on the shape of millimeter-wave antennas; they can be quadrilateral, circular, or wire-like. They can also be configured as a frame. Moreover, there is no limit to the number of millimeter-wave antennas configured in a portable communication device; there can be one or multiple antennas configured in any location. When multiple millimeter-wave antennas are configured, their sizes (widths) can be the same or different. For areas of the portable communication device without millimeter-wave antennas, dummy patterns without antennas can be configured to improve visual visibility.

[0296] The millimeter-wave antenna of the present invention is a millimeter-wave antenna having at least the aforementioned adhesive sheet and substrate. It is only necessary that the substrate has an antenna element (millimeter-wave antenna element) on one side, and that the adhesive sheet is attached to the side of the substrate (millimeter-wave antenna substrate) having the antenna element; there are no other particular limitations. It should be noted that the adhesive sheet of the millimeter-wave antenna of the present invention is an adhesive sheet used in actual use, and therefore does not have a spacer.

[0297] As described above, the millimeter-wave antenna is preferably constructed by bonding the millimeter-wave antenna substrate with other optical components (which may or may not have the aforementioned adhesive sheet; having the adhesive sheet is preferred from the viewpoint of further suppressing millimeter-wave radiation loss). Furthermore, the aforementioned other optical components may be a single component or multiple components.

[0298] Examples of ways to bond the millimeter-wave antenna of the present invention to the other optical components described above include: (1) bonding the millimeter-wave antenna substrate of the present invention to the other optical components via the adhesive sheet of the present invention; (2) bonding the adhesive sheet of the present invention, which includes or constitutes the millimeter-wave antenna substrate, to the other optical components; (3) bonding the millimeter-wave antenna substrate to a component other than the millimeter-wave antenna substrate via the adhesive tape of the present invention; and (4) bonding the adhesive tape of the present invention, which includes or constitutes the millimeter-wave antenna substrate, to a component other than the millimeter-wave antenna substrate. It should be noted that in method (2) above, the adhesive sheet of the present invention preferably has a double-sided adhesive sheet of the millimeter-wave antenna substrate as its substrate.

[0299] Hereinafter, a preferred embodiment of the millimeter-wave antenna of the present invention will be described with reference to the accompanying drawings.

[0300] Figure 1 A millimeter-wave antenna 1A is described, which has at least an adhesive sheet 10 and a substrate as a millimeter-wave antenna substrate 11, wherein the millimeter-wave antenna substrate 11 has a millimeter-wave antenna element 2 on one side, and the adhesive sheet 10 is attached to the side of the millimeter-wave antenna substrate 11 with the millimeter-wave antenna element 2.

[0301] Figure 2 A millimeter-wave antenna 1B is described, comprising a cover member 12, an adhesive sheet 10, and a millimeter-wave antenna substrate 11 arranged in a contacting manner. The millimeter-wave antenna substrate 11 has a millimeter-wave antenna element 2 on the side facing the adhesive sheet 10, and the adhesive sheet 10 is attached to the side of the millimeter-wave antenna substrate 11 facing the millimeter-wave antenna element 2. The cover member 12 is preferably glass, the millimeter-wave antenna substrate 11 is preferably COP from the viewpoint of low dielectric constant and low dielectric loss, and the millimeter-wave antenna element 2 is preferably copper, silver, or ITO.

[0302] Figure 3 A millimeter-wave antenna 1C is described, comprising a cover member 12, an adhesive sheet 10a, a millimeter-wave antenna substrate 11, an adhesive sheet 10b, and an image display panel 13 arranged in a contacting manner. The millimeter-wave antenna substrate 11 has a millimeter-wave antenna element 2 on the side of the adhesive sheet 10a, and the adhesive sheet 10a is attached to the side of the millimeter-wave antenna substrate 11 containing the millimeter-wave antenna element 2. The cover member 12 is preferably glass, and the millimeter-wave antenna substrate 11 is preferably COP from the viewpoint of low dielectric constant and low dielectric loss. The millimeter-wave antenna element 2 is preferably ITO, or silver or copper that has undergone blackening treatment with a coating of nitride, oxide, sulfide, etc., from the viewpoint of transparency and visual recognizability. The adhesive sheet 10b may or may not be the adhesive sheet of the present invention, but is preferably the adhesive sheet of the present invention. The image display panel 13 may have a touch sensor (not shown).

[0303] Figures 1-3 In the millimeter-wave antennas 1A to 1C, the adhesive sheets 10, 10a, and preferably 10b are composed of the adhesive layer of the present invention, which has a low dielectric constant and low dielectric loss at high frequencies. Therefore, the radiation loss of millimeter waves is suppressed, and millimeter-wave communication can be effectively performed. In addition, since millimeter-wave communication can be effectively performed, the antenna area can be miniaturized, and the antenna can be made finer.

[0304] Example

[0305] The present invention will now be described in more detail based on embodiments, but the present invention is not limited to these embodiments in any way.

[0306] (Example 1)

[0307] A 13% by weight adhesive composition (solution) was prepared by mixing 100 parts by weight of polyisobutylene (trade name "OPPANOL N80", Mw: 1050000, Mn: 440000, Mw / Mn: 2.4, manufactured by BASF) and 22 parts by weight of fully hydrogenated terpene phenol (softening point: 135°C, hydroxyl value: 160) as a tackifier. The obtained adhesive composition (solution) was coated onto a PET separator (trade name "MRF50", manufactured by Mitsubishi Chemical Corporation) to a final thickness (adhesive layer thickness) of 75 μm, thereby forming a coating layer (adhesive composition layer). The coating layer was then dried at 130°C for 5 minutes to form an adhesive layer, thus producing an adhesive sheet with an adhesive layer thickness of 75 μm. In addition, a PET spacer (trade name "MRF38", manufactured by Mitsubishi Chemical Corporation) is bonded to the adhesive side of the adhesive sheet in such a way that the peel-off surface contacts the adhesive layer. This results in a substrate-free double-sided adhesive sheet in which the adhesive layer is protected on both sides by the spacer.

[0308] (Example 2)

[0309] In a reaction vessel equipped with a condenser, nitrogen inlet, thermometer, and stirrer, a mixture of 99 parts by mass of lauryl methacrylate (LMA), 1.0 part by mass of hydroxyethyl methacrylate (HEMA), 0.2 parts by mass of 2,2'-azobisisobutyronitrile (AIBN) as a thermal polymerization initiator, and ethyl acetate as a polymerization solvent were added at a monomer content of 70% by mass. Nitrogen gas was purged for approximately 1 hour while stirring. The reaction vessel was then heated to 70°C and reacted for 6 hours. Alternatively, the reaction vessel was heated to 80°C and reacted for 3 hours to obtain a (meth)acrylic acid polymer with a weight-average molecular weight (Mw) of 400,000. The adhesive composition of this example was prepared by adding 0.1 parts by weight of an isocyanate crosslinking agent (trade name "Coronate HX", manufactured by Tosoh Co., Ltd., 100% solid content) as a solid content basis, 0.01 parts by weight of dioctyltin dilaurate (trade name "EMBILIZEROL 1", manufactured by Tokyo Fine Chemicals Co., Ltd.) as a crosslinking accelerator, and 5 parts by weight of acetylacetone as a crosslinking delay agent, and mixing them uniformly.

[0310] The adhesive composition described above was coated onto a polyethylene terephthalate (PET) spacer (trade name "MRF38", manufactured by Mitsubishi Chemical Corporation) with a final thickness (adhesive layer thickness) of 25 μm, thereby forming a coating layer (adhesive composition layer). Next, it was dried in a dryer at 130°C for 120 minutes to allow residual monomers to evaporate. Furthermore, a PET spacer (trade name "MRE38", manufactured by Mitsubishi Chemical Corporation) was placed on the coating layer, thereby obtaining a substrate-free double-sided adhesive sheet containing only the adhesive layer, with both sides of the adhesive layer protected by spacers.

[0311] (Example 3)

[0312] Using a monomer mixture consisting of 80 parts by weight of lauryl methacrylate (LMA) and 20 parts by weight of hydroxyethyl methacrylate (HEMA), a substrate-free double-sided adhesive sheet was obtained, except that the procedure was the same as in Example 2.

[0313] (Comparative Example 1)

[0314] In a reaction vessel equipped with a condenser, nitrogen inlet, thermometer, and stirrer, 100 parts by mass of butyl acrylate (BA), 5 parts by mass of acrylic acid (AA), and 1 part by mass of 4-hydroxybutyl acrylate (4-HBA) were added to obtain a monomer mixture. Furthermore, relative to the total monomer mixture of 100 parts by mass, 0.2 parts by mass of 2,2'-azobisisobutyronitrile (AIBN) as a thermal polymerization initiator and ethyl acetate as a polymerization solvent were added at a monomer content of 40% by mass. Nitrogen gas was introduced into the flask, and nitrogen purging was performed while stirring slowly. The reaction vessel was then heated to 60°C and reacted for 8 hours to obtain an acrylic polymer with a weight-average molecular weight (Mw) of 1.8 million. The adhesive composition of this example was prepared by adding 0.25 parts by weight of an epoxy crosslinking agent (trade name "TETRAD C", manufactured by Mitsubishi Gas Chemical Co., Ltd., 100% solid content) based on the solid content to a solution of the acrylic polymer (100 parts by weight of solid content) and mixing it uniformly.

[0315] The adhesive composition described above was coated onto a polyethylene terephthalate (PET) spacer (trade name "MRF38", manufactured by Mitsubishi Chemical Corporation) with a final thickness (adhesive layer thickness) of 25 μm, thereby forming a coating layer (adhesive composition layer). Next, it was dried in a dryer at 130°C for 120 minutes to allow residual monomers to evaporate. Furthermore, a PET spacer (trade name "MRE38", manufactured by Mitsubishi Chemical Corporation) was placed on the coating layer, thereby obtaining a substrate-free double-sided adhesive sheet containing only the adhesive layer, with both sides of the adhesive layer protected by spacers.

[0316] [Feature Evaluation]

[0317] The substrate-free double-sided adhesive sheets of the Examples and Comparative Examples were subjected to the following measurements or evaluations. The evaluation results are shown in Table 1.

[0318] (1) Evaluation of dielectric constant and dielectric loss

[0319] For the adhesive layer itself obtained in the examples or comparative examples (the adhesive layer obtained by peeling a polysiloxane-treated PET spacer from a double-sided adhesive sheet), the dielectric constant and dielectric loss at frequencies of 28 GHz and 60 GHz were measured using the following apparatus. Measurements were performed on a circular area with a diameter of 8 cm at 28 GHz. At least three samples were prepared for each test subject, and the average value of the measured values ​​of these three samples, after excluding the maximum and minimum values, was taken as the dielectric constant and dielectric loss at each frequency.

[0320] • Measurement method: Open resonator method JIS R1660-2

[0321] • Apparatus: Interferometric resonator method dielectric constant measurement system manufactured by KEYCOM Corporation

[0322] Measurement environment: 23℃±1℃, 52%±1%RH

[0323] (2) Saturated moisture absorption rate

[0324] Take 10 mg of the adhesive layer obtained from the examples or comparative examples as a sample. Place this sample in a microcalorimetric analyzer with humidification (IGA Sorp: model IG-SA-116, manufactured by Hiden Corporation), using a detector capable of measuring at the 0.001 mg level, and continuously heat at 130°C until no weight change is observed. Then, maintain the environment in the apparatus at 65°C and 0% RH for at least 1 hour, and measure its weight (w1) at the point when no weight change is observed (dry state). Furthermore, set the atmosphere in the apparatus to 65°C and 90% RH, and track weight changes for at least 10 hours. Measure its weight (w2) at the point when the weight change of the sample disappears (when the moisture absorption rate is saturated). Calculate the saturated moisture absorption rate from the above results using the following formula.

[0325] Saturated moisture absorption rate (%) = {(w2-w1) / w1} × 100

[0326] (3) Change in dielectric loss

[0327] For each adhesive layer monomer obtained in the examples or comparative examples (the object after peeling the polysiloxane-treated PET spacer from the double-sided adhesive sheet), humidification was carried out at 65°C and 90% RH for at least 5 days. For each sample, the dielectric constant and dielectric loss were measured at frequencies of 28 GHz and 60 GHz using an interferometric resonator method dielectric constant measurement system (manufactured by Keycom Co., Ltd.) according to the above-described open resonator method (JIS R1660-2) every 10 minutes from 4 minutes to 180 minutes. The dielectric loss of each sample was obtained as the average of three detectors.

[0328] Of the dielectric losses obtained for each adhesive layer after humidification (after a time interval of 4 minutes to 180 minutes), the maximum value (D) is used. fmax ) and minimum value (D fmin The change in dielectric loss is calculated using the following formula.

[0329] Change in dielectric loss = D fmax -D fmin

[0330] (4) Total transmittance and haze

[0331] One spacer was peeled off from the double-sided adhesive sheet obtained in the examples or comparative examples, and the double-sided adhesive sheet was then attached to a glass slide (manufactured by Matsunami Glass Industry Co., Ltd., "White Grinding No. 1", thickness 0.8mm to 1.0mm, total transmittance 92%, haze 0.2%). The other spacer was then peeled off, thus creating a test piece consisting of a double-sided adhesive sheet (adhesive layer) and a glass slide. The total transmittance and haze in the visible light region of the above test piece were measured using a haze meter (product name "HM150", manufactured by Murakami Color Research Institute Co., Ltd.) at an environment of 23°C ± 1°C and 52% ± 1% RH. Three samples were prepared for each test subject, and the average of the measured values ​​of the three samples was taken as the total transmittance and haze in the visible light region. It should be noted that the greater the thickness of the test piece, the lower the total transmittance and the greater the haze.

[0332] (5) Water vapor transmission rate (WVTR)

[0333] The water vapor permeability of the adhesive layer obtained in the examples or comparative examples was evaluated based on the cup method. The weight (w1) of the calcium chloride isolated from the outside by the adhesive layer in its dry state was measured, and the weight (w2) of the sample after a specified time (when the moisture absorption rate is saturated) at 40°C and 92% RH was measured. The weight change was converted to per unit time (1 day) and per unit area (1 m²). 2This is used as the water vapor transmission rate (g / m). 2 / day). w2 is calculated using the values ​​obtained 24 to 48 hours after humidification begins.

[0334] (6) Transmit and receive characteristics

[0335] The transmitting and receiving characteristics of the adhesive layer (obtained by peeling a polysiloxane-treated PET spacer from a double-sided adhesive sheet) obtained in the embodiments or comparative examples utilize Figure 4 The square microstrip antenna shown is evaluated (refer to Chapter 5, Volume 2, Group 4, Electron Communications Information Society, "Planar Antennas", URL: http: / / www.ieicehbkb.org / files / 04 / 04Gun_02hen_05.pdf). Specifically, antenna film 46 is fabricated, which has a layer formed on the surface of a 100μm thick COP substrate (trade name: ZEONOR, manufactured by Zeon Corporation, Japan) serving as antenna substrate 44. Figure 4 The millimeter-wave patch antenna 43, as shown, has a 1 μm thick copper ground layer 45 formed on its back side. The dimensions of the millimeter-wave patch antenna 43 are adjusted in a manner optimal for lamination with the adhesives of the various embodiments and comparative examples (vertical A: 2.8 mm to 3.2 mm, horizontal B: 4.13 mm). The adhesive layers 42 of the various embodiments and comparative examples are attached to the patch antenna 43 side of the antenna film 46 in a manner that prevents the entry of air bubbles and foreign matter. Then, it is bonded to a 0.7 mm thick chemically strengthened glass (manufactured by Corning Incorporated) serving as the cover glass 41, thereby creating an antenna laminate 4 consisting of cover glass 41 / adhesive layer 42 / antenna film 46. Powered by a microstrip line 43a connected to a millimeter-wave patch antenna 43 of various antenna stacks 4, the transmit and receive characteristics in the 30 GHz band are evaluated. Stacks that show improved gain (5.7 dB) compared to those without an adhesive layer (stacks with antenna films 46 arranged adjacent to each other on the cover glass 41) are rated as 0, while stacks that show decreased gain (deterioration) compared to those without an adhesive layer are rated as ×.

[0336]

[0337] Label Explanation

[0338] 1A, 1B, 1C millimeter-wave antennas

[0339] 10, 10a, 10b Adhesive sheets

[0340] 11 mmWave antenna substrate

[0341] 12 Cover components

[0342] 2 mmWave antenna elements

[0343] 13 Image display panel

[0344] 4 Antenna stack

[0345] 41 Cover glass

[0346] 42 Adhesive layer

[0347] 43 mmWave Patch Antenna

[0348] 43a Microstrip Line

[0349] 44 Antenna substrate

[0350] 45 Copper grounding layer

[0351] 46 Antenna membrane

Claims

1. An adhesive composition comprising at least one base polymer selected from the group consisting of acrylic polymers and rubber polymers, wherein, The adhesive composition has a dielectric constant of 2.0 to 5.0 at a frequency of 28 GHz. The dielectric loss of the adhesive composition at a frequency of 28 GHz is 0.0001 to 0.

05. The adhesive composition has a saturated moisture absorption rate of less than 2.8% under conditions of 65°C and 90% RH. In cases involving the acrylic polymer, the acrylic polymer comprises a mixture of methacrylate compounds and (meth)acrylate compounds, a portion thereof, or a copolymer thereof. The copolymer has a weight-average molecular weight of 300,000 to 5,000,000. The mixture, a portion thereof, is a methacrylic acid copolymer containing at least one of (i) to (iii) below, and containing 1.0% to 30.0% by mass of a methacrylate compound with hydroxyl groups and crosslinkable functional groups as a monomer component. Relative to all 100 parts by weight of the methacrylic acid copolymer, 0.1 to 0.3 parts by weight of an azo polymer initiator are included as the polymerization initiator. In the case of containing the rubber-based polymer, the rubber-based polymer contains at least one selected from the group consisting of natural rubber, polyisoprene, polyisobutylene, and butylene-based polymer, and the adhesive composition has a water vapor transmission rate of 20 g / m 2 / day to 430 g / m 2 / day under the condition of 40°C, 92% R.H. The change in dielectric loss calculated by the following formula is less than 0.

006. The amount of change in dielectric loss = D fmax - D fmin D fmax : the maximum value shown by the dielectric loss at a frequency of 28 GHz during the period in which the dielectric loss is tracked over time at 23°C ± 1°C, 52% ± 1% R.H. after the adhesive composition has been humidified to saturation at 65°C, 90% R.H.; D fmin : the minimum value shown by the dielectric loss at a frequency of 28 GHz during the period in which the dielectric loss was traced over time under conditions in which the adhesive composition was humidified to a saturated state at 65°C, 90% R.H., and then under conditions of 23°C ± 1°C, 52% ± 1% R.H., (i) The content of methacrylate compounds having aliphatic groups having 10 or more carbon atoms, or structural units derived from such compounds, is 80% by mass or more. (ii) The content of methacrylate compounds having alicyclic groups having 6 or more carbon atoms, or structural units derived from such compounds, is 10.0% to 50.0% by mass. (iii) The content of methacrylate compounds having a group containing an aromatic ring with 6 or more carbon atoms or structural units derived from such compounds is 10.0% to 50.0% by mass.

2. The adhesive composition according to claim 1, wherein, The dielectric constant of the adhesive composition at a frequency of 60 GHz is 2.0 to 5.

0.

3. An adhesive composition comprising at least one base polymer selected from the group consisting of acrylic polymers and rubber polymers, wherein, The dielectric constant of the adhesive composition at a frequency of 60 GHz is 2.0–5.

0. The dielectric loss of the adhesive composition at a frequency of 60 GHz is 0.0001 to 0.

05. The adhesive composition has a saturated moisture absorption rate of less than 2.8% under conditions of 65°C and 90% RH. In cases involving the acrylic polymer, the acrylic polymer comprises a mixture of methacrylate compounds and (meth)acrylate compounds, a portion thereof, or a copolymer thereof. The copolymer has a weight-average molecular weight of 300,000 to 5,000,000. The mixture, a portion thereof, is a methacrylic acid copolymer containing at least one of (i) to (iii) below, and containing 1.0% to 30.0% by mass of a methacrylate compound with hydroxyl groups and crosslinkable functional groups as a monomer component. Relative to all 100 parts by weight of the methacrylic acid copolymer, 0.1 to 0.3 parts by weight of an azo polymer initiator are included as the polymerization initiator. In the case of comprising the rubber-like polymer, the rubber-like polymer comprises at least one selected from the group consisting of natural rubber, polyisoprene, polyisobutylene, and butene polymers, and the adhesive composition has a water vapor permeability of 20 g / m at 40°C and 92% RH. 2 / day ~430g / m 2 / sky, The change in dielectric loss calculated by the following formula is less than 0.

003. Change in dielectric loss = D fmax -D fmin D fmax The maximum dielectric loss was observed at a frequency of 60 GHz during the period when the adhesive composition was humidified to saturation at 65°C and 90%RH, and then the dielectric loss was tracked over time at 23°C ± 1°C and 52% ± 1%RH. D fmin The minimum dielectric loss was observed at a frequency of 60 GHz during the period when the adhesive composition was humidified to saturation at 65°C and 90%RH, and then tracked over time at 23°C ± 1°C and 52% ± 1%RH. (i) The content of methacrylate compounds having aliphatic groups having 10 or more carbon atoms, or structural units derived from such compounds, is 80% by mass or more. (ii) The content of methacrylate compounds having alicyclic groups having 6 or more carbon atoms, or structural units derived from such compounds, is 10.0% to 50.0% by mass. (iii) The content of methacrylate compounds having a group containing an aromatic ring with 6 or more carbon atoms or structural units derived from such compounds is 10.0% to 50.0% by mass.

4. The adhesive composition according to any one of claims 1 to 3, wherein, The total light transmittance of the adhesive layer with a thickness of 25 μm formed from the adhesive composition was measured to be 85% or more.

5. The adhesive composition according to any one of claims 1 to 3, wherein, The haze of the adhesive layer with a thickness of 25 μm formed from the adhesive composition was measured to be less than 1.0%.

6. An adhesive layer, wherein, The adhesive layer is formed from the adhesive composition according to any one of claims 1 to 5.

7. An adhesive sheet, wherein, The adhesive sheet has the adhesive layer as described in claim 6.

8. A millimeter-wave antenna, said millimeter-wave antenna having at least a substrate and the adhesive sheet of claim 7, wherein, The substrate has an antenna element on at least one side, and the adhesive sheet is attached to the side of the substrate having the antenna element.

Citation Information

Patent Citations

  • Acrylic adhesives and its production method

    JP2002069411A

  • Adhesive and adhesive sheet

    JP2015183178A

  • Electronic device antenna arrays mounted on dielectric layer

    JP2019186942A

  • Adhesive layer and adhesive film

    JP2020007570A

  • Adhesive sheet

    CN107629712A