A method for manufacturing UNS N08810 alloy seamless heat exchange tube

Through multi-step manufacturing methods, including peeling, PT inspection, cold rolling, heat treatment and straightening, the problems of low inspection pass rate, low material yield and low dimensional accuracy of domestic UNS N08810 alloy seamless heat exchange pipes are solved. , achieves high inspection pass rate and dimensional accuracy, suitable for mass production.

CN117696621BActive Publication Date: 2024-11-26JIANGSU YINHUAN PRECISION STEEL TUBE CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311729215.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-15
Publication Date
2024-11-26
Estimated Expiration
2043-12-15

AI Technical Summary

Technical Problem

The domestic UNS N08810 alloy seamless heat exchange pipe has problems such as low pass rate, low material rate, low dimensional accuracy and poor internal and external surface quality, which is difficult to meet the technical requirements of mass production.

Method used

A multi-step manufacturing method is adopted, including peeling, PT inspection, centering, grinding, heating, perforation, pickling, cold rolling, heat treatment, straightening, ultrasonic vortex current and pipe cutting processes, and the cold rolling deformation is strictly controlled The parameters such as quantity, rolling speed, heat treatment temperature and time, straightening speed and outer diameter deviation ensure high inspection pass rate, material yield and dimensional accuracy of the product.

Benefits of technology

It has achieved high pass rate, high material rate, high dimensional accuracy and good internal and external surface quality. It has stable mechanical properties and is suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004609620500000071
    Figure BDA0004609620500000071
  • Figure BDA0004609620500000072
    Figure BDA0004609620500000072
  • Figure BDA0004609620500000081
    Figure BDA0004609620500000081
Patent Text Reader

Abstract

The present invention relates to a method for manufacturing a UNS N08810 alloy seamless heat exchange tube, comprising: (i) peeling, PT testing, shearing, centering, grinding, heating, perforating, water cooling and testing round steel material; (ii) The N08810 hot perforated billet is pickled, and the pickled billet is inspected for incoming materials and the inner and outer surfaces are ground and repaired; (iii) the obtained billet is cold rolled for intermediate products, and after cold rolling, the intermediate products need to be degreased, heat treated, straightened, cut, pickled, ground and inspected; (iv) the obtained steel pipe is cold rolled for finished products; (v) the obtained steel pipe is degreased; (vi) the obtained steel pipe is heat treated; (vii) the obtained steel pipe is straightened; (viii) the obtained steel pipe is ultrasonically eddy current, water pressure and cut, and samples are taken for physical and chemical tests when cutting; (ix) the obtained steel pipe is subjected to finished product surface inspection, size inspection, cleaning, spraying and finishing processes, and finally packaged and stored. The products produced by this method have a high one-time inspection pass rate and a high yield rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a seamless pipe, in particular to a method for preparing a UNS N08810 alloy seamless heat exchange pipe, and belongs to the technical field of material processing. Background Art

[0002] N08810 nickel-based alloy has been widely used in cold hydrogenation reactors of polycrystalline silicon projects, catalyst tubes for steam / hydrocarbon reforming in the petrochemical industry, cracking tubes in the production of vinyl chloride monomer, steam superheater tubes in the power generation industry, and high-temperature heat exchange tubes in gas-cooled nuclear reactors in recent years due to its many advantages such as good processing performance, high temperature resistance, good oxidation resistance, good anti-sulfurization and anti-carburization performance.

[0003] In the past, UNS N08810 alloy seamless heat exchange tubes were mainly imported from abroad, with long delivery cycles and high prices, so its domestic manufacturing is particularly important. At present, domestically produced N08810 alloy seamless heat exchange tubes have problems such as low first-time inspection pass rate, low material yield rate, low dimensional accuracy, and poor internal and external surface quality.

[0004] At present, patent CN201710887663 discloses a method for manufacturing UNS N08810 iron-nickel-based alloy large-diameter seamless pipes for high-temperature heating furnaces. In the disclosed method, the method for removing oxide scale from UNS N08810 alloy large-diameter seamless pipes is internal and external shot peening + pickling. This method can effectively remove oxide scale, but the cost of shot peening is too high and is not suitable for mass production of small-diameter UNS N08810 heat exchange tubes.

[0005] Based on this, developing a production process for N08810 alloy seamless heat exchange tubes that can overcome the above-mentioned difficulties and developing N08810 alloy seamless heat exchange tubes with a high one-time inspection pass rate, high yield rate, high dimensional accuracy, good inner and outer surface quality, and physical and chemical properties that meet standard technical requirements has become a technical problem that needs to be urgently solved by technical personnel in this field. Summary of the invention

[0006] The technical problem to be solved by the present invention is to propose a method for manufacturing UNSN08810 alloy seamless heat exchange tube in view of the shortcomings of the above-mentioned prior art. The products produced by this method have a high one-time inspection pass rate, a high yield rate, high dimensional accuracy, good inner and outer surface quality, stable organizational performance, strong practicality, and are conducive to batch production.

[0007] The technical solution of the present invention to solve the above technical problems is:

[0008] A method for manufacturing a UNS N08810 alloy seamless heat exchange tube specifically comprises the following steps:

[0009] (1) UNS N08810 round steel is peeled, PT tested, sheared, centered, ground, heated, pierced, water cooled, and tested. The piercing temperature is 1120-1130℃ and the holding time is 8min.

[0010] (ii) The UNS N08810 hot-pierced billet is pickled, and the pickled billet is subjected to incoming material inspection and internal and external surface grinding and repairing, specifically: the hot-pierced billet is subjected to initial inspection + grinding and repair + re-inspection, and the endoscope is used for each re-inspection, and PT is performed on a random basis;

[0011] (iii) cold rolling the tube blank obtained in step (ii) to obtain an intermediate product, and after cold rolling, the intermediate product needs to be degreased, heat treated, straightened, cut, pickled, ground and inspected, wherein:

[0012] When cold rolling the intermediate product, the cold rolling deformation is controlled at 60%-70%, the rolling speed is controlled at ≤60 times / min, the feed amount is ≤3mm / time, the Q value is ≥1.10, the outer diameter deviation after rolling is controlled at ±0.5%Dmm, and the wall thickness deviation is controlled at ±0.5%Smm;

[0013] The specific process of degreasing the intermediate product is: degreasing in an alkali tank → rinsing → soaking in a hot water tank → degreasing in an acid tank → rinsing → inspection;

[0014] The intermediate product heat treatment is carried out in a roller hearth furnace with a slightly oxidizing atmosphere, a heat treatment temperature of 1150±10℃, and a holding time of ≥ wall thickness×4min;

[0015] (iv) cold rolling the steel tube obtained in step (iii);

[0016] When rolling finished products, the cold rolling deformation is 65%-75%, the rolling speed is controlled at ≤120 times / min, the feed amount is ≤2mm / time, and the Q value is ≥0.85;

[0017] When the finished product is cold rolled, the outer diameter deviation after rolling is controlled within ±0.05mm, and the wall thickness deviation is controlled within ±0.05mm;

[0018] (5) degreasing the steel pipe obtained in step (4);

[0019] The specific steps of degreasing finished pipes are: soaking in alkali tank → soaking in clean water tank → wiping the outer surface → taping the inner wall with cloth → inspection;

[0020] (6) subjecting the steel pipe obtained in step (5) to finished product heat treatment;

[0021] The finished product heat treatment is carried out in a bright furnace, and the atmosphere in the furnace is ammonia decomposition or pure hydrogen;

[0022] When heat treating finished products, the heat treatment temperature is controlled to be 1130±10℃, and the holding time is ≥ wall thickness × 3min;

[0023] (7) straightening the steel pipe obtained in step (6);

[0024] (8) subjecting the steel pipe obtained in step (7) to finished product ultrasonic eddy current, water pressure, and pipe cutting, and taking samples for physical and chemical tests when cutting the pipe;

[0025] (IX) The steel pipe obtained in step (VIII) is subjected to finished product surface inspection, dimension inspection, cleaning, spray marking and finishing processes, and finally packaged and stored.

[0026] The technical solution further defined in the present invention is:

[0027] In the aforementioned method for manufacturing UNS N08810 alloy seamless heat exchange tube, in step (iii) of degreasing the intermediate product, the components of the solution in the alkali cylinder are controlled to be degreased in the alkali cylinder in a mass ratio of: degreasing agent: water = 1:7, the alkali cylinder temperature is 70-80°C, and the alkali cylinder immersion time is 30-50min;

[0028] When degreasing the acid cylinder, the components of the solution in the acid cylinder are controlled to be calculated by mass percentage as follows: HF: 1%, HNO3: 10-15%, and the remainder is tap water. The sum of the above components is 100%. The acid cylinder temperature is 60°C and the pickling time is 5 minutes.

[0029] In the aforementioned method for manufacturing UNS N08810 alloy seamless heat exchange tube, when straightening the intermediate product in step (iii), the straightening control speed is ≤8m / min, the curvature after straightening is ≤1.0mm / m, and the outer diameter deviation after straightening is ±0.02mm.

[0030] In the manufacturing method of the aforementioned UNS N08810 alloy seamless heat exchange tube, during the pickling of the intermediate product in step (iii), the components of the solution in the acid cylinder are calculated by mass ratio as follows: HF: 5-8%, HNO3: 10-15%, and the balance is tap water, the sum of the above components is 100%, the acid cylinder temperature is controlled to be: 60°C, the pickling time is controlled to be 5-8 minutes, after 5 minutes, the cylinder needs to be opened every 1 minute to observe the inner and outer surfaces, and the pickling is stopped when the inner and outer surfaces show a uniform and slight oxide scale.

[0031] Technical effect: After 5 minutes, the cylinder needs to be opened every 1 minute to observe the inner and outer surfaces. When the inner and outer surfaces show uniform and slight oxide scale, stop pickling to avoid excessive pickling and affect subsequent work.

[0032] In the aforementioned method for manufacturing the UNS N08810 alloy seamless heat exchange tube, during the grinding and inspection of the intermediate product in step (iii), the grinding is performed by local spot grinding after internal and external polishing, and the inspection is performed by visual inspection + endoscope one by one.

[0033] In the aforementioned method for manufacturing UNS N08810 alloy seamless heat exchange tube, when the finished tube is degreased in step (v), the mass ratio of the solution in the alkali cylinder is, degreasing agent: water = 1:6.5, the alkali cylinder temperature is: 40-60°C, the alkali cylinder immersion time is: 30-60min, and the inner wall is wiped clean with a cloth strip for 5-7 times.

[0034] In the aforementioned method for manufacturing UNS N08810 alloy seamless heat exchange tube, in step (seven), when straightening the finished tube, the straightening machine is controlled to have a speed of ≤10 m / min, a curvature after straightening of ≤0.5 mm / m, and an outer diameter deviation after straightening of ±0.01 mm.

[0035] In the aforementioned method for manufacturing the UNS N08810 alloy seamless heat exchange tube, the first ultrasonic qualified rate in step (eight) is ≥97%, and the first eddy current qualified rate is 100%.

[0036] In the aforementioned method for manufacturing UNS N08810 alloy seamless heat exchange tube, the surface inspection in step (IX) includes visual inspection and dimensional inspection, with a qualified rate of ≥95.5%, and the dimensional accuracy of the finished tube is controlled as follows: outer diameter ±0.05mm, wall thickness ±0.05mm, and the inner and outer surfaces of the finished tube are smooth, with inner and outer wall roughness Ra≤0.6.

[0037] In the aforementioned method for manufacturing the UNS N08810 alloy seamless heat exchange tube, the room temperature tensile test of the manufactured finished tube shows the following results: yield strength of 230-270 MPa, tensile strength of 550-580 MPa, and elongation after fracture of ≥55%.

[0038] The beneficial effects of the present invention are:

[0039] The present invention adopts two cold rolling passes, one pass is for cold rolling of intermediate products, and the cold rolling deformation is controlled at 60%-70%, and the second pass is for cold rolling of finished products, and the cold rolling deformation is controlled at 65%-75%, so that the grains are fully broken and a finer grain size can be obtained after heat treatment. The first pass of cold rolling of intermediate products ensures the surface quality by strictly controlling the feed amount ≤3mm / time, and makes the deformation more uniform by controlling the Q value ≥1.10, thereby improving the dimensional accuracy; similarly, the surface quality and dimensional accuracy of the finished product are ensured by strictly controlling the feed amount ≤2mm / time and controlling the Q value ≥0.85.

[0040] The present invention provides a method for degreasing intermediate products in one pass, including strictly controlling the ratio of the alkali cylinder and the acid cylinder, the temperature and time to ensure the degreasing quality and avoid the risk of carburization during heat treatment. The present invention provides a method for degreasing finished products in two passes, which uses an alkali cylinder for degreasing, a clean water cylinder for soaking, acetone for wiping the outer surface and a cloth strip soaked in acetone to clean the inner wall to remove oil. The alkali cylinder ratio, temperature and time and the inner and outer wall cleaning method are strictly controlled to ensure the degreasing quality of the finished pipe and ensure that there is no risk of carburization during the bright heat treatment of the finished product.

[0041] The present invention stipulates that the solution heat treatment of the intermediate product of the first pass is carried out in a roller bottom furnace, the atmosphere in the furnace is slightly oxidizing, and the heat treatment temperature is 1150±10°C, so as to eliminate the hardening of cold rolling work, ensure that the seamless pipe has good plasticity, and facilitate subsequent cold rolling forming. The insulation time of the intermediate product of the first pass is ≥ wall thickness × 4min, generally taking the nearest integer, the insulation time is slightly longer, the oxide scale is more uniform and loose, and it is easy to remove the oxide scale by pickling. The solution heat treatment of the finished product of the second pass is carried out in a bright furnace, the atmosphere in the furnace is ammonia decomposition or pure hydrogen, and the heat treatment temperature is 1130±10°C. While obtaining good organization and comprehensive mechanical properties, it ensures the brightness of the surface color of the heat exchange tube and the consistency of the overall color.

[0042] The invention specifies the straightening machine model, straightening speed, straightness and outer diameter deviation range after straightening, especially specifies the use of a plastic roller straightening machine for finished product straightening, specifies the straightening speed ≤ 10 m / min, ensures the curvature while avoiding the risk of iron rod straightening scratches and marks, and ensures the quality of finished product straightening. Strictly specifying the outer diameter deviation range after straightening, especially after finished product straightening, can effectively avoid the risk of outer diameter deviation caused by straightening, thereby improving dimensional accuracy.

[0043] The present invention provides a method for pickling an intermediate product in one pass, including strictly controlling the ratio of the acid cylinder, the temperature and the time to ensure the pickling quality. Conventional N08810 pickling often seriously lacks acid to avoid over-acidification, resulting in excessively thick oxide scales, low internal and external polishing efficiency, and low pass rate of one endoscope inspection after polishing, requiring multiple rework and repair. However, the inner and outer walls of the N08810 intermediate product tube washed out by this method have only slight and uniform oxide scales, and no tendency to over-acidification, high internal and external polishing efficiency, high pass rate of one endoscope inspection, greatly reducing the cost of manual polishing, improving production efficiency, and shortening the entire intermediate product production cycle.

[0044] The present invention provides a method for grinding and repairing hot perforated billets and intermediate steel pipes. The purpose of retesting and sampling the hot perforated billets is to avoid residual cracks on the outer surface. The purpose of endoscopes for hot perforated billets is to more accurately and efficiently treat the inner wall defects and avoid the inner wall defects from being transferred to the next cold rolling process and causing the defects to extend. The purpose of endoscopes for intermediate products is to ensure the inner wall quality of the finished cold-rolled products and reduce the risk of endoscope failure due to ultrasonic internal damage and inner wall defects, thereby improving the final ultrasonic qualified rate, surface inspection qualified rate and final yield rate.

[0045] The method of the present invention solves the problems of low first-time inspection pass rate, low material yield rate, low dimensional accuracy and poor inner and outer surface quality by strictly limiting the process optimization of UNS N08810 alloy seamless heat exchange tubes. The products produced by the method have high first-time inspection pass rate, high material yield rate, high dimensional accuracy, good inner and outer surface quality, stable mechanical properties, strong practicality, and are conducive to batch production.

[0046] The N08810 alloy seamless heat exchange tube prepared by the method of the present invention has a first ultrasonic qualified rate of ≥97%, a first eddy current qualified rate of 100%, a first table inspection (visual inspection + size inspection) qualified rate of ≥95%, and a comprehensive first inspection qualified rate (ultrasonic qualified rate×eddy current qualified rate×table inspection qualified rate) of ≥93%.

[0047] The yield rate of the N08810 alloy seamless heat exchange tube prepared by the method of the present invention (round steel→finished tube) is ≥84%; the prepared N08810 alloy seamless heat exchange tube can meet the following dimensional accuracy: outer diameter ±0.05mm, wall thickness ±0.05mm; the prepared seamless heat exchange tube has smooth inner and outer surfaces, and the color is consistent, and the inner and outer wall roughness Ra≤0.6; its room temperature tensile test: yield strength 230-270Mpa, tensile strength 550-580MPa, elongation after fracture ≥55%. DETAILED DESCRIPTION

[0048] The following is a further detailed description of the method for manufacturing the UNS N08810 alloy seamless heat exchange tube in conjunction with the examples, but the embodiments of the invention are not limited to the following examples.

[0049] Example 1

[0050] A method for manufacturing a UNS N08810 alloy seamless heat exchange tube, with a finished product specification of φ25×2×9505mm, and technical requirements that meet both ASME SB163-2021 and NB / T47019.9-2021 standards, specifically comprising the following steps:

[0051] (I) UNS N08810 Yongxing round steel is peeled, PT tested, sheared, centered, ground, heated, pierced, water cooled, and tested. The piercing temperature is 1120-1130℃ and the holding time is 8min.

[0052] (ii) The UNS N08810 hot-pierced billet is pickled, and the pickled billet is inspected and the inner and outer surfaces are ground. The defects of the billet and its grinding method are preliminarily characterized. For the outer surface hot-piercing defects of the billet, it is subjected to spot grinding + external polishing. For some billets with inner burrs and transverse cracks, it is subjected to internal polishing. After the billet is ground, it is re-inspected. During the re-inspection, a random inspection is performed for PT. Only those that pass the re-inspection can be circulated, and unqualified products are subjected to secondary grinding;

[0053] (iii) cold rolling the tube obtained in step (ii) to the intermediate product, and after cold rolling, the intermediate product needs to be degreased, heat treated, straightened, cut, pickled, ground (local spot grinding after internal and external polishing) and inspected (endoscope for each endoscope), wherein:

[0054] When cold rolling the intermediate product, the cold rolling deformation is controlled at 60%-70%, the rolling speed is controlled at ≤60 times / min, the feed amount is ≤3mm / time, the Q value is ≥1.10, the outer diameter deviation after rolling is controlled at ±0.5%Dmm, and the wall thickness deviation is controlled at ±0.5%Smm;

[0055] The specific process of degreasing the intermediate product is: degreasing in an alkali tank → rinsing → soaking in a hot water tank → degreasing in an acid tank → rinsing → inspection;

[0056] The intermediate product heat treatment is carried out in a roller hearth furnace with a slightly oxidizing atmosphere, a heat treatment temperature of 1150±10℃, and a holding time ≥ wall thickness × 4min (rounded to an integer);

[0057] (iv) cold rolling the steel tube obtained in step (iii);

[0058] When rolling finished products, the cold rolling deformation is 65%-75%, the rolling speed is controlled at ≤120 times / min, the feed amount is ≤2mm / time, and the Q value is ≥0.85;

[0059] When the finished product is cold rolled, the outer diameter deviation after rolling is controlled within ±0.05mm, and the wall thickness deviation is controlled within ±0.05mm;

[0060] (5) degreasing the steel pipe obtained in step (4);

[0061] The specific steps of degreasing finished pipes are: soaking in alkali tank → soaking in clean water tank → wiping the outer surface → taping the inner wall with cloth → inspection;

[0062] (6) subjecting the steel pipe obtained in step (5) to finished product heat treatment;

[0063] The finished product heat treatment is carried out in a bright furnace, and the atmosphere in the furnace is ammonia decomposition or pure hydrogen;

[0064] When the finished product is heat treated, the heat treatment temperature is controlled to be 1130±10℃, and the holding time is ≥ wall thickness×3min (rounded to an integer);

[0065] (7) straightening the steel pipe obtained in step (6);

[0066] (8) subjecting the steel pipe obtained in step (7) to finished product ultrasonic eddy current, water pressure, and pipe cutting, and taking samples for physical and chemical tests when cutting the pipe;

[0067] (IX) The steel pipe obtained in step (VIII) is subjected to finished product surface inspection, dimension inspection, cleaning, spray marking and finishing processes, and finally packaged and stored.

[0068] In this embodiment, the cold rolling process of UNS N08810 seamless heat exchange tube is formulated, and the cold rolling deformation of intermediate products and finished products is strictly controlled. A reasonable rolling speed and a relatively small feed amount are selected to ensure the quality of the inner and outer surfaces. The uniformity of the structure in the wall thickness direction is ensured by controlling the Q value, thereby improving the dimensional accuracy and improving the inner wall quality. The specific cold rolling parameters are shown in Table 1 below, and the technical requirements for dimensional accuracy and actual dimensions are shown in Table 2. It can be seen from Table 2 that the dimensional accuracy of the intermediate product tubes and finished tubes in each pass meets the internal control requirements, and the dimensional accuracy of the finished tubes is much higher than the ASME SB163-2021 standard requirements.

[0069] Table 1 UNS N08810 cold rolling parameters

[0070]

[0071] Table 2 UNS N08810 technical requirements dimensional accuracy and actual measured dimensions

[0072]

[0073] The specific process of degreasing the intermediate product of UNS N08810 alloy seamless heat exchange tube in this embodiment is: degreasing by alkali cylinder → rinsing → soaking in hot water cylinder → degreasing in acid cylinder → rinsing → inspection. The main control requirements for degreasing the intermediate product are shown in Table 3. The steps for degreasing the finished tube are: degreasing by soaking in alkali cylinder → soaking in clean water cylinder → wiping the outer surface → taping the inner wall with cloth strips → inspection. The main control requirements for degreasing the finished tube are shown in Table 4. The inner and outer surfaces of the tube degreasing by the above method are clean and free of oil stains, and there is no risk of carburization during heat treatment.

[0074] Table 3 Main control requirements for UNS N08810 intermediate product degreasing process

[0075]

[0076] Table 4 Main control requirements for degreasing process of UNS N08810 finished pipe

[0077]

[0078] In this embodiment, the heat treatment of the intermediate products of UNS N08810 alloy seamless heat exchange tubes is carried out in a roller hearth furnace with an oxidizing atmosphere; the heat treatment of the finished products is carried out in a bright furnace with an atmosphere of ammonia decomposition or pure hydrogen. The heat treatment system is as shown in Table 5.

[0079] 5 UNS N08810 heat treatment system

[0080]

[0081] It can be seen from Table 5 that the solution heat treatment of the intermediate product is carried out in a roller hearth furnace, the atmosphere in the furnace is slightly oxidizing, the furnace has 6 temperature zones, the first three temperature zones T01-T03 are heating zones, the last three temperature zones T04-T06 are insulation zones, the heat treatment temperature is 1150℃, the insulation time is 15min respectively, and the cooling method is water cooling. The heat treatment of the finished product is bright heat treatment, the atmosphere in the furnace is ammonia decomposition or pure hydrogen, the furnace has 5 temperature zones, T01-T02 is the heating zone, T03-T05 is the insulation zone, the heat treatment temperature is 1130℃, the insulation time is 7min, and the cooling method is water jacket cooling.

[0082] The straightening parameters of the intermediate and finished products of the UNS N08810 seamless heat exchange tubes in this embodiment are shown in Table 6. By specifying the straightening machine model, straightening speed, straightness and outer diameter deviation range after straightening, especially the straightening of finished products, it is specified that a plastic roller straightening machine is used, and the straightening speed is specified to be ≤10m / min. While ensuring the curvature, the risk of iron rod straightening causing scratches and marks can be avoided, thereby ensuring the quality of finished product straightening. Strictly specifying the outer diameter deviation range after straightening, especially after straightening of finished products, can effectively avoid the risk of outer diameter deviation caused by straightening, thereby improving dimensional accuracy.

[0083] Table 6 UNS N08810 straightening parameters

[0084]

[0085] In this embodiment 1, the requirements for cutting the intermediate products and finished products of the UNS N08810 alloy seamless heat exchange tubes are shown in Table 7. By strictly controlling the amount of flattening and strictly following the middle cutting method, the middle position must be manually measured and marked before cutting the tube, and visual inspection is not allowed. This can reduce the risk of the intermediate products and finished products being under-lengthened, and improve the final product inspection pass rate and the final yield rate.

[0086] Table 7 UNS N10276 pipe cutting requirements

[0087] Specification equipment Pipe cutting requirements Intermediate product cutting φ48×3.6 Grinding machine Middle cutting requirements: measure the length and mark the middle position, visual inspection is not allowed Finished pipe cutting φ25×2.1 Inline pipe cutting machine Cutting requirements: remove blind areas, cut to size, cut margin +0~3mm

[0088] In this embodiment 1, the main control requirements for pickling of the intermediate product of UNS N08810 alloy seamless heat exchange tube are shown in Table 8 below, including strict control of the ratio of the acid tank, temperature and time to ensure the quality of pickling. Conventional N08810 pickling often results in serious under-acidification to avoid over-acidification, resulting in excessively thick oxide scales, low internal and external polishing efficiency, and low pass rate of one-time endoscopic inspection after polishing, requiring multiple rework and repair. However, the N08810 intermediate product tube washed out by this method has only slight and uniform oxide scales on the inner and outer walls, and has no tendency to over-acidification, high internal and external polishing efficiency, and high pass rate of one-time endoscopic inspection, which greatly reduces the cost of manual polishing, improves production efficiency, and shortens the entire intermediate product production cycle.

[0089] Table 8 Main control requirements for the pickling process of UNS N08810 intermediate products

[0090]

[0091] In this embodiment 1, the inspection and grinding and repairing requirements for the perforated billets and intermediate product tubes of UNS N08810 seamless heat exchange tubes are shown in Table 9 below. The re-inspection and random inspection of the hot perforated billets is to avoid that there are no cracks remaining on the outer surface. The endoscope of the hot perforated billets is to treat the inner wall defects more accurately and efficiently to avoid the inner wall defects from flowing to the next cold rolling process and causing the defects to extend. The endoscope is performed one by one during the grinding and repair of the intermediate products in the second pass to ensure the inner wall quality of the finished cold rolling, reduce the risk of endoscope failure caused by ultrasonic internal damage and inner wall defects, thereby improving the final ultrasonic qualified rate, surface inspection qualified rate and final yield rate.

[0092] Table 9 UNS N08810 grinding and repairing operation requirements

[0093]

[0094] In this embodiment 1, the ultrasonic, eddy current, water pressure, visual and dimensional inspection results of the finished UNS N08810 alloy seamless heat exchange tube are shown in Table 10. It can be seen from Table 10 that the ultrasonic, eddy current and water pressure qualified rates of the N08810 alloy seamless heat exchange tube produced by the production method are as high as 97.37%, and the qualified rates of eddy current and water pressure are both 100.00%, and the qualified rate of dimensional inspection is also 100.00%. The dimensional accuracy is much higher than the dimensional accuracy specified in ASME SB163-2021 and NB / T47019.9-2021 standards, the visual inspection qualified rate is as high as 95.97%, and the one-time inspection qualified rate is as high as 93.55%.

[0095] Table 10 Ultrasonic, eddy current, water pressure, visual and dimensional inspection of finished UNS N08810 pipes

[0096]

[0097] In this embodiment 1, the yield rate of UNS N08810 alloy seamless heat exchange tubes is shown in Table 11. The hot-punched billet round steel is 151.08 tons, and the final finished product φ25×2.1×9505mm has 11,200 pieces in storage and weighs 127.26 tons, with a yield rate of up to 84.23%.

[0098] Table 11 UNS N08810 yield rate

[0099]

[0100] The test method for room temperature tensile properties of finished tubes is ASTM E8, and the test results are shown in Table 12. From Table 12, it can be seen that the N08810 alloy seamless heat exchange tubes manufactured by this method have excellent mechanical properties, with a yield strength of 230-270Mpa under 69 furnace batch numbers, which is higher than the ASME SB163-2021 standard requirement of ≥170Mpa, a stable tensile strength of 550-580Mpa, higher than the standard requirement of ≥450Mpa, and a post-break elongation of ≥55%, which is much higher than the standard requirement of ≥30%.

[0101] Table 12 Room temperature tensile properties of UNS N08810 finished pipe

[0102]

[0103] According to the test requirements of GB / T 242-2007, the expansion test results of all 69 batches of N08810 alloy tubes are: no cracks. According to the test requirements of GB / T 246-2017, the flattening test results of all 69 batches of N08810 alloy tubes are: no cracks.

[0104] According to GB / T 25160-2016B All batches of steel pipes were subjected to crystal corrosion tests, and the results of the crystal corrosion tests are shown in Table 2.15 below.

[0105] Table 13 UNS N08810 crystal corrosion test results

[0106] Crystalline rot test Test solution Test cycle Test results GB / T 25160-2016 Method B <![CDATA[H2SO4-CuSO4]]> 24 hours Flattening test without cracks

[0107] The present invention solves the problems of low first-time inspection pass rate, low material yield rate, low dimensional accuracy and poor inner and outer surface quality by strictly limiting the process optimization of UNS N08810 alloy seamless heat exchange tubes. It can be seen from Tables 10-13 that the products produced by the method have a high first-time inspection pass rate, a high material yield rate, high dimensional accuracy, good inner and outer surface quality, stable mechanical properties, strong practicability, and are conducive to batch production.

[0108] In addition to the above embodiments, the present invention may also have other implementation modes. Any technical solution formed by equivalent replacement or equivalent transformation falls within the protection scope required by the present invention.

Claims

1. A method for manufacturing a UNS N08810 alloy seamless heat exchange tube, characterized in that: The specific steps include: (I) UNS N08810 round steel is peeled, PT tested, sheared, centered, ground, heated, pierced, water cooled and tested. The piercing temperature is 1120-1130℃ and the holding time is 8min. (ii) The UNS N08810 hot-pierced billet is pickled, and the pickled billet is subjected to incoming material inspection and internal and external surface grinding and repairing. Specifically, the hot-pierced billet is subjected to initial inspection + grinding and repair + re-inspection. During the re-inspection, each endoscope is used and PT is randomly inspected; (iii) subjecting the tube blank obtained in step (ii) to a one-pass intermediate product cold rolling, and after the cold rolling, the intermediate product needs to be degreased, heat treated, straightened, cut, pickled, ground and inspected, wherein: When cold rolling the intermediate product, the cold rolling deformation is controlled at 60%-70%, the rolling speed is controlled at ≤60 times / min, the feed amount is ≤3mm / time, the Q value is ≥1.10, the outer diameter deviation after rolling is controlled at ±0.5%Dmm, and the wall thickness deviation is controlled at ±0.5%Smm; The specific process of degreasing the intermediate product is: degreasing in an alkali tank → rinsing → soaking in a hot water tank → degreasing in an acid tank → rinsing → inspection; When degreasing the alkali cylinder, the components of the solution in the alkali cylinder are controlled by mass ratio as follows: degreasing agent: water = 1:7, alkali cylinder temperature: 70-80℃, alkali cylinder soaking time: 30-50min; when degreasing the acid cylinder, the components of the solution in the acid cylinder are controlled by mass percentage as follows: HF: 1%, HNO3: 10-15%, the balance is tap water, the sum of the above components is 100%, acid cylinder temperature: 60℃, pickling time: 5min; The intermediate product heat treatment is carried out in a roller hearth furnace, the atmosphere in the furnace is a slightly oxidizing gas, the heat treatment temperature is 1150±10°C, and the holding time is ≥ wall thickness×4min; When pickling the intermediate product, the components of the solution in the acid tank are calculated by mass ratio: HF: 5-8%, HNO3: 10-15%, and the balance is tap water. The sum of the above components is 100%. The temperature of the acid tank is controlled at: 60℃, and the pickling time is controlled at 5-8 minutes. After 5 minutes, the tank needs to be opened every 1 minute to observe the inner and outer surfaces. When the inner and outer surfaces show uniform and slight oxide scale, the pickling is stopped; (iv) subjecting the steel tube obtained in step (iii) to a single pass of cold rolling; When rolling finished products, the cold rolling deformation is 65%-75%, the rolling speed is controlled at ≤120 times / min, the feed amount is ≤2mm / time, and the Q value is ≥0.85; When the finished product is cold rolled, the outer diameter deviation after rolling is controlled within ±0.05mm, and the wall thickness deviation is controlled within ±0.05mm; (5) degreasing the steel pipe obtained in step (4); The specific steps of degreasing finished pipes are: soaking in alkali tank → soaking in clean water tank → wiping the outer surface → taping the inner wall with cloth → inspection; When degreasing the finished pipe, the mass ratio of the solution in the alkali tank is degreasing agent: water = 1:6.5, the temperature of the alkali tank is 40-60℃, the soaking time of the alkali tank is 30-60min, and the inner wall is wiped clean with a cloth strip for 5-7 times; (vi) subjecting the steel pipe obtained in step (v) to finished product heat treatment; The finished product heat treatment is carried out in a bright furnace, and the atmosphere in the furnace is ammonia decomposition or pure hydrogen; When heat treating finished products, the heat treatment temperature is controlled to be 1130±10℃, and the holding time is ≥ wall thickness × 3min; (VII) straightening the steel pipe obtained in step (VI); (8) subjecting the steel pipe obtained in step (7) to finished product ultrasonic eddy current, water pressure, and pipe cutting, and taking samples for physical and chemical tests when cutting the pipe; (IX) The steel pipes obtained in step (VIII) are subjected to finished product surface inspection, dimension inspection, cleaning, spray marking and finishing processes, and finally packaged and stored.

2. The method for manufacturing the UNS N08810 alloy seamless heat exchange tube according to claim 1, characterized in that: When straightening the intermediate product in the step (iii), the straightening control speed is ≤8m / min, the curvature after straightening is ≤1.0mm / m, and the outer diameter deviation after straightening is ±0.02mm.

3. The method for manufacturing the UNS N08810 alloy seamless heat exchange tube according to claim 1, characterized in that: During the grinding and inspection of the intermediate product in step (iii), the grinding is carried out by local spot grinding after internal and external polishing, and the inspection is carried out by visual inspection + endoscope one by one.

4. The method for manufacturing the UNS N08810 alloy seamless heat exchange tube according to claim 1, characterized in that: In the step (VII), when the finished tube is straightened, the control speed of the straightening machine is ≤10m / min, the curvature after straightening is ≤0.5mm / m, and the outer diameter deviation after straightening is ±0.01mm.

5. The method for manufacturing the UNS N08810 alloy seamless heat exchange tube according to claim 1, characterized in that: In the step (eight), the first ultrasonic qualified rate is ≥97%, and the first eddy current qualified rate is 100%.

6. The method for manufacturing the UNS N08810 alloy seamless heat exchange tube according to claim 1, characterized in that: The surface inspection in step (IX) includes visual inspection and dimensional inspection, with a pass rate of ≥95.5%. The dimensional accuracy of the finished tube is controlled as follows: outer diameter ±0.05mm, wall thickness ±0.05mm, the inner and outer surfaces of the finished tube are smooth, and the inner and outer wall roughness Ra≤0.

6.

7. The method for manufacturing the UNS N08810 alloy seamless heat exchange tube according to claim 1, characterized in that: The room temperature tensile test of the manufactured finished pipe shows the following results: yield strength 230-270 MPa, tensile strength 550-580 MPa, and elongation after fracture ≥55%.