A curing type high temperature and high pressure resistant thread sealant

Through the cross-linking effect of bis-alkenyl organosilicon borane and glycidyl methacrylate and other materials, combined with mica powder and other additives, a curing thread sealant is prepared, which solves the problem of existing sealants sealing under high temperature and high pressure. It solves the problem of poor performance and achieves good sealing performance and environmental protection, which is suitable for the harsh conditions of oil drilling.

CN117700609BActive Publication Date: 2024-10-18QINGDAO TOP PETROCHEMICAL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311702138.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-12
Publication Date
2024-10-18
Estimated Expiration
2043-12-12

AI Technical Summary

Technical Problem

Existing thread sealants have poor sealing effect under high temperature and high pressure conditions, are prone to leakage, and contain harmful heavy metals, making it difficult to meet the stringent requirements of oil drilling.

Method used

A cured high-temperature and high-pressure resistant thread seal is prepared by using bis-alkenyl silicone borane, glycidyl methacrylate, carboxyl silicone boron-modified graphene and other materials for double cross-linking, combined with mica powder and other additives. Agent to form a resilient cross-linked polymer to enhance sealing and lubrication properties.

Benefits of technology

The sealant maintains good sealing performance under high temperature and high pressure environments, prevents leakage, does not contain heavy metals, adapts to bending and stress changes in threaded connection parts, extends the service life of oil casings, and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure GDA0004937944400000031
    Figure GDA0004937944400000031
  • Figure GDA0004937944400000032
    Figure GDA0004937944400000032
Patent Text Reader

Abstract

The invention relates to the technical field of thread sealants, and discloses a curing type high temperature and high pressure resistant thread sealant. The high temperature and anaerobic environment generated by the thread surface being applied and buckled can promote the curing of the sealant. The molecular structure of diene organic silicon borane contains silicon oxygen boron chemical bonds with high bond energy, has a conjugation effect, and has excellent high temperature resistance. Glycidyl methacrylate can be double-crosslinked with carboxyl organic silicon boron modified graphene and diene organic silicon borane monomers, and still has good sealing performance under high temperature, high pressure and corrosive environment. The unsaturated double bond activity is relatively high, and a three-dimensional network structure is formed in the rapid crosslinking and curing process of the sealant, thereby improving the crosslinking density, ensuring the sealing after curing and maintaining good corrosion resistance and high pressure resistance in a petroleum immersion environment. The sealant does not contain heavy metal components, grease and other non-biodegradable materials, and is green and environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of thread sealants, in particular to a curing type high temperature and high pressure resistant thread sealant. Background Art

[0002] Casing is the largest type of pipe used in oil and gas exploration and development, and occupies a pivotal position in the oil industry. During the development of oil fields, the oil pipes downhole are connected into downhole pipe strings through threads at both ends, and the crude oil mined underground is transmitted to the ground through the oil well pipe string; as people's environmental awareness continues to increase, more and more attention is paid to environmental protection during oil drilling and production. Traditional thread sealants are not only oil-based greases that are toxic, but also contain heavy metals such as lead, which are very harmful to people and the environment; in addition, with the continuous deepening of oil and gas exploration and development, the drilling and production conditions of oil fields are becoming more and more harsh, and higher requirements are put forward for the sealing, high temperature resistance, and corrosion resistance of oil pipe threads. Therefore, there is an urgent need for a new type of efficient thread sealant that is safe, environmentally friendly, and can adapt to harsh working conditions.

[0003] Oil extraction is becoming more and more difficult and the well conditions are more complex. For example, the sealing requirements of high-temperature and high-pressure steam pipeline threads in thermal wells, shale oil wells, etc. are more stringent. The conventional thread sealants on the market currently have poor sealing effects and are prone to failure at high temperatures. Crude oil is easy to leak from the threaded parts, reducing oil recovery efficiency. At the same time, crude oil will also have a corrosive effect on the threads, further reducing oil recovery efficiency, and cannot meet the requirements of high-temperature and high-pressure oil and gas well extraction. In addition, conventional thread sealants are prone to denaturation under high temperature conditions, causing threaded fasteners to get stuck and not easy to disassemble, repair and assemble. The commonly used ordinary API thread sealant still maintains its viscous paste state after being threaded, and can also play a sealing role under general well conditions. When it is in gas wells, deep wells and high-temperature well conditions, its auxiliary sealing performance is greatly reduced. Under the combined effect of high temperature and pressure, grease and thick layers of sediment will be squeezed out of the threads. Even at room temperature for a long time, the API thread sealant will also produce a "drying" phenomenon. At this time, the volume of the thread sealant will shrink and produce gaps, thereby causing leakage.

[0004] The present invention introduces diene organic silicon borane monomers as a matrix, which undergo double cross-linking with glycidyl methacrylate and carboxyl organic silicon boron modified graphene. The addition of additives enhances the lubrication performance and compensates for the disadvantage of volume shrinkage produced after the polymer material is polymerized, so that the prepared thread sealant still has good sealing performance under high temperature, high pressure and corrosive environments. Summary of the invention

[0005] The technical problem solved by the invention is to provide a solidified high temperature and high pressure resistant thread sealant, which is mainly used for lubrication and auxiliary sealing of special oil pipe threads.

[0006] The technical solution of the present invention is:

[0007] A curing type high temperature and high pressure resistant thread sealant comprises the following components in parts by weight: 5-10 parts of component A, 1 part of component B, 200 parts of component C, and 300-350 parts of component D.

[0008] The component A comprises the following ingredients in proportion by weight: 60-84% ethylene glycol, 15-30% water, and 1-10% EDTA.

[0009] The B component includes the following ingredients in weight proportions: 40-78% ethyl methacrylate, 2-10% p-benzoquinone, and 20-50% propylene glycol adipate.

[0010] The C component includes the following ingredients in weight ratio: 20-50% hydroxypropyl methacrylate, 30-35% tetraethylene glycol diisooctanoate, 15-30% glycidyl methacrylate, 5-20% of the structural formula Diolefin organosilicon borane.

[0011] The D component includes the following ingredients in weight proportion: 20-25% dibutyl ester, 22-26% mica powder, 30-45% carboxyl organic silicon boron modified graphene, 5-12.5% ​​carbon fiber, 0.5-2% initiator, and 3-7% fumed silica.

[0012] The preparation method of the curing type high temperature and high pressure resistant thread sealant is as follows: adding component A and component B into a reaction bottle according to the ratio of the above formula, mixing and stirring evenly at room temperature, then adding component C, stirring and dispersing, and finally adding component D and stirring evenly to obtain the curing type high temperature and high pressure resistant thread sealant.

[0013] Preferably, the initiator is any one of cumene hydroperoxide, dicumyl hydroperoxide, dilauroyl peroxide, and dibenzoyl peroxide.

[0014] Preferably, the preparation method of the bis-alkenyl organosilicon borane is:

[0015] (1) Add tetrahydrofuran, dichlorodimethylsilane and 1-hydroxy-1,3-dihydrobenzo[c][1,2]oxaborole-5-carboxylic acid into a reaction flask, react at 65-75° C. for 1-2 h under a nitrogen atmosphere, cool, filter, wash with acetone, and dry to obtain a dicarboxyl organosilicon borane. The preparation process is as follows:

[0016]

[0017] (2) Add dicarboxyl organosilicon borane and N,N-dimethylformamide to a reaction flask, stir evenly, then add 3-butene-1-ol, 4-dimethylaminopyridine and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, stir and react under nitrogen atmosphere, after the reaction is completed, add ethyl acetate and deionized water for extraction, concentrate the organic phase, separate by column chromatography, and dry to obtain diolefin organosilicon borane. The preparation process is as follows:

[0018]

[0019] Preferably, in the step (1), the amount of dichlorodimethylsilane is 100 parts by weight and the amount of 1-hydroxy-1,3-dihydrobenzo[c][1,2]oxaborole-5-carboxylic acid is 255-310 parts by weight.

[0020] Preferably, in step (2), the dicarboxyl organosilicon borane is 100 parts, 3-butene-1-ol is 35-45 parts, 4-dimethylaminopyridine is 3-6 parts, and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride is 140-190 parts by weight.

[0021] Preferably, in step (2), the reaction temperature is 20-35° C. and the reaction time is 12-24 h.

[0022] Preferably, the preparation method of the carboxyl organic silicon boron modified graphene is: add hydroxylated graphene and deionized water into a reaction flask, stir evenly, add dicarboxyl organic silicon borane, 4-dimethylaminopyridine and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, react at 25-40°C for 5-10h, filter, wash with ethanol and deionized water, and dry to obtain carboxyl organic silicon boron modified graphene.

[0023] Preferably, in parts by weight, the hydroxylated graphene is 100 parts, the dicarboxyl organosilicon borane is 80-150 parts, the 4-dimethylaminopyridine is 5-10 parts, and the 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride is 210-240 parts.

[0024] The beneficial technical effects of the present invention are as follows:

[0025] The invention first synthesizes a high-temperature resistant diene organic silicon boron monomer, reacts dichlorodimethylsilane with 1-hydroxy-1,3-dihydrobenzo[c][1,2]oxaborole-5-carboxylic acid to obtain a dicarboxyl organic silicon borane, then esterifies 3-butene-1-ol in the presence of a condensing agent to obtain a diene organic silicon borane, then esterifies the carboxyl group of the dicarboxyl organic silicon borane with the hydroxyl group on the surface of hydroxylated graphene to obtain carboxyl organic silicon boron modified graphene, and then cures and crosslinks using the alkenyl group of the diene organic silicon borane, the carboxyl group of the carboxyl organic silicon boron modified graphene, the epoxy group and alkenyl group of glycidyl methacrylate and other acrylic ester monomers, additives, etc. to obtain a cured high-temperature and high-pressure resistant thread sealant.

[0026] The molecular structure of diene organosilicon borane contains high-energy silicon-oxygen-boron chemical bonds, which have a conjugation effect and have excellent performance in high-temperature environments; glycidyl methacrylate can undergo dual cross-linking with carboxyl organosilicon-boron modified graphene and diene organosilicon borane monomers, and still has good sealing performance in high-temperature, high-pressure and corrosive environments; the unsaturated double bonds are highly active and form a three-dimensional network structure during the rapid cross-linking and curing process of the sealant, which increases the cross-linking density and ensures that the cured sealant can maintain good corrosion resistance and high-pressure resistance in a petroleum immersion environment.

[0027] Mica enhances its lubrication performance, and plasticizers, reinforcing agents, etc. make the thread sealant have a certain elasticity after curing, which makes up for the disadvantage of volume shrinkage caused by polymer materials after polymerization, so that it can adapt to bending or distortion caused by stress changes in threaded connection parts; after the prepared thread sealant is applied to the thread surface, the high temperature and anaerobic environment generated by the buckle will promote the curing of the sealant to form a polymer with resilience and sealing properties and a layer of dense sealing ring, which can not only meet the sealing and lubrication properties under ordinary well conditions, but also maintain good sealing properties in high-pressure gas wells and higher temperature conditions. At the same time, because this layer of sealing ring has resilience, the sealing ring can adapt to small-scale deformation caused by bending and stress changes in threaded connection parts.

[0028] The thread sealant provided by the present invention does not contain heavy metal components, grease and other non-biodegradable materials, and is an environmentally friendly oil casing thread sealant. It can effectively prevent the thread end from loosening when evenly applied to the oil casing thread; after the thread is tightened, it solidifies into a solid cross-linked polymer to form an elastic sealing ring, thereby effectively blocking the thread leakage channel and the thread matching gap, and preventing the invasion and overflow of high-pressure fluid and gas; it will not age and degenerate when exposed to high temperature conditions for a long time, and has excellent high temperature resistance; it will not leak at a maximum pressure higher than the designed maximum pressure of the oil and gas well, and will not be corroded by highly corrosive chemical media, thereby ensuring the service life of the oil casing; at the same time, it has good air sealing performance, and can replace most specifications and high-cost special oil casing in oil and gas mixed wells, gas wells, deep wells, ultra-deep wells and when the connection strength of the oil casing joints is met, thereby greatly reducing the cost of use. DETAILED DESCRIPTION

[0029] The technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Preparation of hydroxylated graphene: Weigh 0.5 g of graphene and add it to a reaction bottle with 500 mL of deionized water, stir and disperse it evenly, add 0.334 g of Fenton catalyst (model JK-FDCH), continue stirring, then add 25 mL of H2O2 with a mass fraction of 25%. After ultrasonic treatment for 30 minutes, the product is first filtered through a 0.45 μm water-based microporous filtration membrane, and the filtrate is filtered again through a 50 nm water-based microporous filtration membrane. The retentate on the secondary filter membrane is the prepared hydroxylated graphene.

[0031] Example 1

[0032] (1) Tetrahydrofuran, 100 parts by weight of dichlorodimethylsilane and 290 parts by weight of 1-hydroxy-1,3-dihydrobenzo[c][1,2]oxaborole-5-carboxylic acid were added to a reaction flask, reacted at 70° C. for 1.5 h under a nitrogen atmosphere, cooled, filtered, washed with acetone, and dried to obtain a dicarboxyl organosilicon borane.

[0033] (2) Add 100 parts by weight of dicarboxyl organosilicon borane and N,N-dimethylformamide to a reaction flask, stir evenly, then add 40 parts of 3-butene-1-ol, 5 parts of 4-dimethylaminopyridine and 180 parts of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, react at 30° C. for 20 hours under a nitrogen atmosphere, then add ethyl acetate and deionized water for extraction, concentrate the organic phase, separate by column chromatography, and dry to obtain the diolefin organosilicon borane.

[0034] (3) Add 100 parts by weight of hydroxylated graphene and deionized water to a reaction flask, stir evenly, add 100 parts of dicarboxyl organosilicon borane, 8 parts of 4-dimethylaminopyridine and 220 parts of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, react at 35° C. for 9 hours, filter, wash with ethanol and deionized water, and dry to obtain carboxyl organosilicon boron modified graphene.

[0035] (4) Four components A, B, C, and D were prepared. The weight percentage of the components in component A was: 70% ethylene glycol, 25% water, and 5% EDTA; the weight percentage of the components in component B was: 60% ethyl methacrylate, 5% p-benzoquinone, and 35% propylene glycol adipate; the weight percentage of the components in component C was: 50% hydroxypropyl methacrylate, 30% tetraethylene glycol diisooctanoate, 15% glycidyl methacrylate, and 5% of the structural formula The components of component D are as follows according to weight percentage: 25% dibutyl ester, 30% mica powder, 30% carboxyl organic silicon boron modified graphene, 10% carbon fiber, 1% initiator cumene hydroperoxide, and 4% fumed silica. 9 parts of component A and 1 part of component B by weight are added to a reaction bottle, mixed and stirred evenly at room temperature, and then 200 parts of component C are added, stirred and dispersed, and finally 320 parts of component D are added and stirred evenly to obtain a cured high temperature and high pressure resistant thread sealant.

[0036] Example 2

[0037] (1) Tetrahydrofuran, 100 parts by weight of dichlorodimethylsilane and 310 parts by weight of 1-hydroxy-1,3-dihydrobenzo[c][1,2]oxaborole-5-carboxylic acid were added to a reaction flask, reacted at 65° C. for 2 h under a nitrogen atmosphere, cooled, filtered, washed with acetone, and dried to obtain a dicarboxyl organosilicon borane.

[0038] (2) Add 100 parts by weight of dicarboxyl organosilicon borane and N,N-dimethylformamide to a reaction flask, stir evenly, add 45 parts of 3-butene-1-ol, 3 parts of 4-dimethylaminopyridine and 190 parts of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, react at 20° C. for 24 hours under a nitrogen atmosphere, add ethyl acetate and deionized water for extraction, concentrate the organic phase, separate by column chromatography, and dry to obtain the diolefin organosilicon borane.

[0039] (3) Add 100 parts by weight of hydroxylated graphene and deionized water to a reaction flask, stir evenly, add 80 parts of dicarboxyl organosilicon borane, 10 parts of 4-dimethylaminopyridine and 210 parts of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, react at 40° C. for 5 h, filter, wash with ethanol and deionized water, and dry to obtain carboxyl organosilicon boron modified graphene.

[0040] (4) Four components A, B, C, and D were prepared. The weight percentage of the components in component A was: 84% ethylene glycol, 15% water, and 1% EDTA; the weight percentage of the components in component B was: 78% ethyl methacrylate, 2% p-benzoquinone, and 20% propylene glycol adipate; the weight percentage of the components in component C was: 35% hydroxypropyl methacrylate, 35% tetraethylene glycol diisooctanoate, 20% glycidyl methacrylate, and 10% of the structural formula The components of component D are as follows according to weight percentage: 20% dibutyl ester, 26% mica powder, 35% carboxyl organic silicon boron modified graphene, 10% carbon fiber, 2% initiator diisopropylbenzene hydroperoxide, and 7% fumed silica. 10 parts of component A and 1 part of component B by weight are added to a reaction bottle, mixed and stirred evenly at room temperature, and then 200 parts of component C are added and stirred and dispersed, and finally 300 parts of component D are added and stirred evenly to obtain a cured high temperature and high pressure resistant thread sealant.

[0041] Example 3

[0042] (1) Tetrahydrofuran, 100 parts by weight of dichlorodimethylsilane and 255 parts by weight of 1-hydroxy-1,3-dihydrobenzo[c][1,2]oxaborole-5-carboxylic acid were added to a reaction flask, reacted at 75° C. for 1 hour under a nitrogen atmosphere, cooled, filtered, washed with acetone, and dried to obtain a dicarboxyl organosilicon borane.

[0043] (2) Add 100 parts by weight of dicarboxyl organosilicon borane and N,N-dimethylformamide to a reaction flask, stir evenly, add 35 parts of 3-butene-1-ol, 6 parts of 4-dimethylaminopyridine and 140 parts of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, react at 35° C. for 12 hours under a nitrogen atmosphere, add ethyl acetate and deionized water for extraction, concentrate the organic phase, separate by column chromatography, and dry to obtain the diolefin organosilicon borane.

[0044] (3) Add 100 parts by weight of hydroxylated graphene and deionized water to a reaction flask, stir evenly, add 150 parts of dicarboxyl organosilicon borane, 5 parts of 4-dimethylaminopyridine and 240 parts of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, react at 25° C. for 10 h, filter, wash with ethanol and deionized water, and dry to obtain carboxyl organosilicon boron modified graphene.

[0045] (4) Four components A, B, C, and D were prepared. The weight percentage of the components in component A was: 60% ethylene glycol, 30% water, and 10% EDTA; the weight percentage of the components in component B was: 40% ethyl methacrylate, 10% p-benzoquinone, and 50% propylene glycol adipate; the weight percentage of the components in component C was: 25% hydroxypropyl methacrylate, 35% tetraethylene glycol diisooctanoate, 25% glycidyl methacrylate, and 15% of the structural formula The components of component D are as follows according to weight percentage: 20% dibutyl ester, 22% mica powder, 40% carboxyl organic silicon boron modified graphene, 12.5% ​​carbon fiber, 0.5% dilauroyl peroxide, and 5% fumed silica. 5 parts of component A and 1 part of component B by weight are added to a reaction bottle, mixed and stirred evenly at room temperature, and then 200 parts of component C are added and stirred and dispersed, and finally 350 parts of component D are added and stirred evenly to obtain a cured high temperature and high pressure resistant thread sealant.

[0046] Example 4

[0047] (1) Tetrahydrofuran, 100 parts by weight of dichlorodimethylsilane and 285 parts by weight of 1-hydroxy-1,3-dihydrobenzo[c][1,2]oxaborole-5-carboxylic acid were added to a reaction flask, reacted at 70° C. for 2 h under a nitrogen atmosphere, cooled, filtered, washed with acetone, and dried to obtain a dicarboxyl organosilicon borane.

[0048] (2) Add 100 parts by weight of dicarboxyl organosilicon borane and N,N-dimethylformamide to a reaction flask, stir evenly, add 42 parts of 3-butene-1-ol, 4 parts of 4-dimethylaminopyridine and 165 parts of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, react at 25° C. for 16 hours under a nitrogen atmosphere, add ethyl acetate and deionized water for extraction, concentrate the organic phase, separate by column chromatography, and dry to obtain the diolefin organosilicon borane.

[0049] (3) Add 100 parts by weight of hydroxylated graphene and deionized water to a reaction flask, stir evenly, add 130 parts of dicarboxyl organosilicon borane, 8 parts of 4-dimethylaminopyridine and 225 parts of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, react at 30° C. for 7 hours, filter, wash with ethanol and deionized water, and dry to obtain carboxyl organosilicon boron modified graphene.

[0050] (4) Four components A, B, C, and D were prepared. The weight percentage of the components in component A was: 75% ethylene glycol, 22% water, and 3% EDTA; the weight percentage of the components in component B was: 50% ethyl methacrylate, 5% p-benzoquinone, and 45% propylene glycol adipate; the weight percentage of the components in component C was: 20% hydroxypropyl methacrylate, 30% tetraethylene glycol diisooctanoate, 30% glycidyl methacrylate, and 20% of the structural formula The components of component D are as follows according to weight percentage: 21% dibutyl ester, 25% mica powder, 45% carboxyl organic silicon boron modified graphene, 5% carbon fiber, 1% initiator dibenzoyl peroxide, and 3% fumed silica. 70 parts of component A and 1 part of component B by weight are added to a reaction bottle, mixed and stirred evenly at room temperature, and then 200 parts of component C are added, stirred and dispersed, and finally 330 parts of component D are added and stirred evenly to obtain a cured high temperature and high pressure resistant thread sealant.

[0051] Comparative Example 1

[0052] The difference between Comparative Example 1 and Example 1 is that component C does not contain a compound having the structural formula Diolefin organosilicon borane.

[0053] Prepare four components A, B, C and D, wherein the weight percentage of each component in component A is: 70% ethylene glycol, 25% water, 5% EDTA; the weight percentage of each component in component B is: 60% ethyl methacrylate, 5% p-benzoquinone, 35% propylene glycol adipate; the weight percentage of each component in component C is: 55% hydroxypropyl methacrylate, 30% tetraethylene glycol diisooctanoate, 15% glycidyl methacrylate; the weight percentage of each component in component D is: 25% dibutyl ester, 30% mica powder, 30% carboxyl organic silicon boron modified graphene, 10% carbon fiber, 1% initiator isopropyl hydroperoxide, 4% fumed silica, add 9 parts of component A and 1 part of component B by weight into a reaction bottle, mix and stir evenly at room temperature, then add 200 parts of component C, stir and disperse, and finally add 320 parts of component D and stir evenly to obtain a curing thread sealant.

[0054] Comparative Example 2

[0055] The difference between Comparative Example 2 and Example 1 is that: no carboxyl organic silicon boron modified graphene is added to component D, and an equal mass of hydroxylated graphene is added.

[0056] Four components A, B, C and D are configured. The weight percentage of each component in component A is: 70% ethylene glycol, 25% water, 5% EDTA; the weight percentage of each component in component B is: 60% ethyl methacrylate, 5% p-benzoquinone, 35% propylene glycol adipate; the weight percentage of each component in component C is: 50% hydroxypropyl methacrylate, 30% tetraethylene glycol diisooctanoate, 15% glycidyl methacrylate, 5% structural formula The components of component D are as follows according to weight percentage: 25% dibutyl ester, 30% mica powder, 30% hydroxylated graphene, 10% carbon fiber, 1% initiator cumene hydroperoxide, and 4% fumed silica. 9 parts of component A and 1 part of component B by weight are added to a reaction bottle, mixed and stirred evenly at room temperature, and then 200 parts of component C are added, stirred and dispersed, and finally 320 parts of component D are added and stirred evenly to obtain a curing thread sealant.

[0057] Comparative Example 3

[0058] The difference between Comparative Example 3 and Example 1 is that glycidyl methacrylate is not added to the C component.

[0059] Four components A, B, C, and D are configured. The weight percentage of each component in component A is: 70% ethylene glycol, 25% water, and 5% EDTA; the weight percentage of each component in component B is: 60% ethyl methacrylate, 5% p-benzoquinone, and 35% propylene glycol adipate; the weight percentage of each component in component C is: 60% hydroxypropyl methacrylate, 35% tetraethylene glycol diisooctanoate, and 5% of the structural formula The components of component D are as follows according to weight percentage: 25% dibutyl ester, 30% mica powder, 30% carboxyl organic silicon boron modified graphene, 10% carbon fiber, 1% initiator cumene hydroperoxide, and 4% fumed silica. 9 parts of component A and 1 part of component B by weight are added to a reaction bottle, mixed and stirred evenly at room temperature, and then 200 parts of component C are added, stirred and dispersed, and finally 320 parts of component D are added and stirred evenly to obtain a curing thread sealant.

[0060] Macroscopic weight loss test: The thread sealant is cured at 80°C in a nitrogen atmosphere for 4 hours, then a certain mass of the cured thread sealant is weighed and placed in an alumina crucible, and heat treated in an air atmosphere in a muffle furnace at 200°C and 350°C for 12 hours, respectively. Finally, the thread sealant is taken out and weighed, and the mass loss rate is calculated.

[0061]

[0062]

[0063] It can be seen from the test data in the above table that the mass loss rate of the curing thread sealant increases with the increase of temperature. After heat treatment at 200°C and 350°C for 12 hours, the mass loss rate of Example 4 is 2.3% and 3.8%. The main reason for the increase in mass loss of the sample after heat treatment in the muffle furnace is that the polymer material of the thread sealant contains some solvents and other small molecular components. As the temperature increases, some solvents and small molecular components are lost, resulting in mass loss, but the loss rate is small. This is because the BO bond and Si-O bond in the synthesized diene organosilicon borane are both high-energy chemical bonds, and there is a conjugation effect in the structure, which has excellent high temperature resistance. At the same time, glycidyl methacrylate can undergo dual cross-linking with carboxyl organosilicon boron-modified graphene and diene organosilicon borane monomers, and has good quality stability under high temperature environment.

[0064] Comparative Example 1 does not contain diene organosilicon borane, and its mass loss rate at 200°C is 6.3%, and its mass loss rate at 350°C is 8.7%, and its high temperature resistance is poor; Comparative Example 2 does not contain carboxyl organosilicon boron modified graphene, but contains hydroxylated graphene, and does not form a cross-linked structure with glycidyl methacrylate, and its mass loss rate at 350°C is 9.7%, and its high temperature resistance needs to be further improved; Comparative Example 3 does not contain glycidyl methacrylate, and cannot undergo double cross-linking with carboxyl organosilicon boron modified graphene and diene organosilicon borane monomers, resulting in poor dispersion of graphene in the matrix, which in turn affects the high temperature resistance of the thread sealant.

[0065] Destructive torque test: Take an appropriate amount of thread sealant and evenly apply it on bolts and nuts with specifications of M10×30, place them at 80℃ for 6 hours, and then place them in a muffle furnace at 200℃ and heat treat them in a nitrogen atmosphere for 24 hours. After taking them out, use a torque wrench to measure the maximum value of the destructive torque to judge the thread sealant's curing ability and ability to seal thread gaps under high temperature conditions.

[0066] Breaking torque value (N·m) Example 1 5.3 Example 2 6.5 Example 3 7.2 Example 4 7.1 Comparative Example 1 4.1 Comparative Example 2 4.8 Comparative Example 3 4.9

[0067] The sealing principle of the curing type high temperature resistant thread agent is to use the curing reaction after the thread agent is threaded, and then block the leakage channel to play a sealing role; from the test data in the above table, it can be seen that with the increase of the content of diene organosilicon borane in the sealant, its breaking torque value gradually increases. After curing, at 200°C, the maximum breaking torque value reaches 7.2N·m. There is no softening or powdering phenomenon due to excessive temperature. After the thread is tightened, it solidifies into a solid cross-linked polymer to form an elastic sealing ring, thereby effectively blocking the thread leakage channel and the thread matching gap, preventing the invasion or overflow of high-pressure fluid and gas, and providing the possibility of sealing the thread leakage gap under high temperature conditions. It has good sealing performance and can be used with API threaded joint casing, replacing the special threaded joint casing originally prepared for use, which not only meets the sealing requirements but also greatly reduces the drilling and production costs.

[0068] Corrosion resistance test: cure the thread sealant in a nitrogen atmosphere at 80°C for 4 hours, soak a certain amount of the cured thread sealant in petroleum for 6 hours, and then age it in a constant temperature box at 200°C for 24 hours. Take it out and weigh it, and calculate its mass loss rate.

[0069]

[0070]

[0071] It can be seen from the measured data in the above table that after the thread sealant is immersed in petroleum for 6 hours and then aged in a constant temperature box at 200°C for 24 hours, its mass loss rate is relatively low, and the mass loss rate of Example 3 is 1.57%, showing better corrosion resistance. This is because the unsaturated double bonds in the sealant are highly active, and a three-dimensional network structure is formed during the rapid cross-linking and curing process of the sealant, which increases the cross-linking density and ensures that the cured sealant can maintain good corrosion resistance and bonding properties in a petroleum immersion environment.

[0072] High-pressure resistance test: Take an appropriate amount of thread sealant and apply it evenly on the bolts and nuts with specifications of M10×30. Curing it at a temperature of 25℃ and a relative humidity of 50% for 24 hours. After complete curing, keep it at a pressure of 35MPa for 24 hours. After taking it out, use a torque wrench to measure the maximum value of its breaking torque, compare it with the breaking torque measured at normal pressure, and calculate the change rate of the breaking torque.

[0073] Breaking torque change rate (%) Example 1 1.23 Example 2 1.10 Example 3 0.96 Example 4 0.87 Comparative Example 1 4.65 Comparative Example 2 3.16 Comparative Example 3 3.31

[0074] After the thread sealant is kept under a pressure of 35MPa for 24 hours, the change rate of its breaking torque does not exceed 1.5%, showing good high-pressure resistance. Glycidyl methacrylate can undergo dual cross-linking with carboxyl organic silicon boron modified graphene and diene organic silicon borane monomers, and still has good sealing performance under high temperature, high pressure and strong corrosion environment. At the same time, mica enhances its lubrication performance. The addition of carboxyl organic silicon boron modified graphene makes the thread sealant have a certain elasticity after curing, which makes up for the disadvantage of volume shrinkage after the polymerization of polymer materials, so that it can adapt to the bending or distortion caused by stress changes at the threaded connection part, and has excellent high-pressure resistance.

[0075] Obviously, the specific implementation of the present invention is not limited to the above-mentioned methods. As long as various non-substantial improvements are made using the method concept and technical solution of the present invention, or the concept and technical solution of the present invention are directly applied to other occasions without improvement, they are all within the protection scope of the present invention.

Claims

1. A method for preparing a curing high temperature and high pressure resistant thread sealant, characterized in that: The curing type high temperature and high pressure resistant thread sealant comprises the following components in parts by weight: 5-10 parts of component A, 1 part of component B, 200 parts of component C, and 300-350 parts of component D; the component A comprises the following components in parts by weight: 60-84% ethylene glycol, 15-30% water, and 1-10% EDTA; the component B comprises the following components in parts by weight: 40-78% ethyl methacrylate, 2-10% para-benzoquinone, and 20-50% propylene glycol adipate; The C component includes the following ingredients in weight ratio: 20-50% hydroxypropyl methacrylate, 30-35% tetraethylene glycol diisooctanoate, 15-30% glycidyl methacrylate, 5-20% of the structural formula Diolefin organosilicon borane; The D component includes the following ingredients in weight proportion: 20-25% dibutyl ester, 22-26% mica powder, 30-45% carboxyl organic silicon boron modified graphene, 5-12.5% ​​carbon fiber, 0.5-2% initiator, and 3-7% fumed silica; The preparation method of the bis-alkenyl organosilicon borane is as follows: (1) Add tetrahydrofuran, dichlorodimethylsilane and 1-hydroxy-1,3-dihydrobenzo[c][1,2]oxaborole-5-carboxylic acid into a reaction flask, react at 65-75° C. for 1-2 h under a nitrogen atmosphere, cool, filter, wash with acetone, and dry to obtain a dicarboxyl organosilicon borane; (2) Add dicarboxyl organosilicon borane and N,N-dimethylformamide to a reaction flask, stir evenly, then add 3-butene-1-ol, 4-dimethylaminopyridine and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, and stir the reaction under a nitrogen atmosphere. After the reaction is completed, add ethyl acetate and deionized water for extraction, concentrate the organic phase, separate by column chromatography, and dry to obtain the diolefin organosilicon borane; The preparation method of the curing type high temperature and high pressure resistant thread sealant is as follows: adding component A and component B into a reaction bottle according to the ratio of the above formula, mixing and stirring evenly at room temperature, then adding component C, stirring and dispersing, and finally adding component D and stirring evenly to obtain the curing type high temperature and high pressure resistant thread sealant.

2. The method for preparing a curing high temperature and high pressure resistant thread sealant according to claim 1, characterized in that: The initiator is any one of cumene hydroperoxide, dicumyl hydroperoxide, dilauroyl peroxide and dibenzoyl peroxide.

3. The method for preparing a curing high temperature and high pressure resistant thread sealant according to claim 1, characterized in that: In the step (1), the amount of dichlorodimethylsilane is 100 parts by weight, and the amount of 1-hydroxy-1,3-dihydrobenzo[c][1,2]oxaborole-5-carboxylic acid is 255-310 parts by weight.

4. The method for preparing a curing high temperature and high pressure resistant thread sealant according to claim 1, characterized in that: In the step (2), by weight, the dicarboxyl organosilicon borane is 100 parts, 3-butene-1-ol is 35-45 parts, 4-dimethylaminopyridine is 3-6 parts, and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride is 140-190 parts.

5. The method for preparing a curable high temperature and high pressure resistant thread sealant according to claim 1, characterized in that: In the step (2), the reaction temperature is 20-35° C. and the reaction time is 12-24 h.

6. The method for preparing a curing high temperature and high pressure resistant thread sealant according to claim 1, characterized in that: The preparation method of the carboxyl organic silicon boron modified graphene is as follows: hydroxylated graphene and deionized water are added into a reaction flask, stirred evenly, dicarboxyl organic silicon borane, 4-dimethylaminopyridine and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride are added, reacted at 25-40° C. for 5-10 hours, filtered, washed with ethanol and deionized water, and dried to obtain the carboxyl organic silicon boron modified graphene.

7. The method for preparing a curable high temperature and high pressure resistant thread sealant according to claim 6, characterized in that: In parts by weight, the hydroxylated graphene is 100 parts, the dicarboxyl organosilicon borane is 80-150 parts, the 4-dimethylaminopyridine is 5-10 parts, and the 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride is 210-240 parts.

Citation Information

Patent Citations

  • High-airtight thread sealing grease

    CN101775265A

  • High-gas-barrier-property composite silicone sealant and preparation method thereof

    CN106281205A

  • Composite silicone sealant having high gas barrier property and preparation method therefor