A calcium-based MOF material synergistic with flame-retardant epoxy resin composite material and its preparation method
By synergistically modifying epoxy resin with calcium-based MOF materials and phosphorus-nitrogen compound flame retardants, the compatibility problem between flame retardants and matrix was solved, achieving a balance between high-efficiency flame retardant performance and mechanical properties, and preparing low-smoke, low-toxicity, and halogen-free epoxy resin composite materials.
Patent Information
- Application Number
- CN202311690332.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-11
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-12-11
AI Technical Summary
In the existing technology, adding flame retardants alone has certain limitations in improving the flame retardant effect of epoxy resin, and the compatibility problem between phosphorus and nitrogen compound flame retardants and epoxy resin matrix leads to a decrease in mechanical properties.
Epoxy resin was synergistically modified with calcium-based MOF materials and phosphorus-nitrogen compound flame retardants. A high-efficiency, low-smoke, low-toxicity, and halogen-free flame-retardant epoxy resin composite material was prepared by using a compound flame retardant composed of aluminum diethylphosphonate and melamine polyphosphate, combined with amine, imidazole, or acid anhydride curing agents.
It significantly improves the limiting oxygen index and vertical combustion rating of epoxy resin at low addition levels, reduces the heat release rate and flue gas emission during combustion, while maintaining the mechanical properties of the material.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure HDA0004598971420000011
Abstract
Description
Technical Field
[0001] This invention belongs to the field of flame retardant materials technology, specifically relating to a calcium-based MOF material synergistically flame-retardant epoxy resin composite material and its preparation method. Background Technology
[0002] Epoxy resins generally refer to a class of low-molecular-weight prepolymers containing at least two or more reactive epoxy groups and with aromatic, aliphatic, or alicyclic carbon chains as their backbone. Due to their excellent mechanical strength, electrical insulation, chemical stability, corrosion resistance, and superior adhesive properties, they are widely used in various aspects of daily life, especially in engineering construction, electronics, coatings, medical, and aerospace fields. However, epoxy resins are highly flammable, easily causing fires and releasing large amounts of smoke and toxic gases, which can easily lead to asphyxiation and death, posing significant challenges to rescue personnel. Therefore, flame-retardant modification of epoxy resins is an urgent priority to improve their application safety.
[0003] Studies have found that adding a single flame retardant has limitations in improving the flame retardant effect of epoxy resins. Synergistic flame retardancy, as an important method to address the low efficiency of single flame retardants, is increasingly being applied to epoxy resin flame retardancy. Among these, phosphorus-nitrogen flame retardants, when used in combination, exhibit excellent flame retardant effects with minimal environmental impact. However, as additive flame retardants, phosphorus-nitrogen compound flame retardants are essentially filler-like auxiliaries, and compatibility issues exist between them and the epoxy resin matrix. Therefore, while improving the flame retardant performance of epoxy resins, phosphorus-nitrogen compound flame retardants often negatively impact the mechanical properties of the epoxy resin. Summary of the Invention
[0004] The purpose of this invention is to provide a method for modifying epoxy resin with calcium-based MOF and a phosphorus-nitrogen compound flame retardant, successfully preparing a high-efficiency, low-smoke, low-toxicity, and halogen-free flame-retardant epoxy resin. This compound flame-retardant system can not only effectively improve the flame-retardant performance of epoxy resin materials, but also reduce the release of toxic gases during epoxy resin combustion without affecting the excellent mechanical properties of the epoxy resin material itself, achieving green and environmentally friendly flame-retardant modification of epoxy resin.
[0005] The objective of this invention is achieved through the following technical solution: The flame-retardant epoxy resin provided by this invention is an epoxy resin composite material modified by calcium-based MOF and phosphorus-nitrogen compound flame retardant. In the composite material, the amount of compound flame retardant added is 5-20% of the mass of epoxy resin, the amount of calcium-based MOF material added is 1-5% of the mass of epoxy resin, and the amount of curing agent added is 20% of the mass of epoxy resin.
[0006] The compound flame retardant is composed of aluminum diethylphosphinate and melamine polyphosphate.
[0007] The epoxy resin is one or more of bisphenol A type epoxy resin, bisphenol S type epoxy resin, and bisphenol F type epoxy resin.
[0008] In compound flame retardants, the weight ratio of aluminum diethylphosphonate and melamine polyphosphate is 1.5 to 3.
[0009] The calcium-based MOF material is calcium terephthalate.
[0010] The curing agent is selected from one or more of amine curing agents, imidazole curing agents, or acid anhydride curing agents.
[0011] This invention also provides a method for preparing the above-mentioned flame-retardant epoxy resin. (1) Dry the epoxy resin in an oven at 100℃ for 30~60min, and dry the flame retardant and calcium-based MOF in an oven at 60℃ for 4~6h.
[0012] (2) Weigh each component by weight percentage, form a premix of flame retardant and calcium-based MOF, and uniformly disperse it in epoxy resin at 60°C with ultrasonic assistance; then add curing agent to form a uniform mixture. Pour the above mixture into a template preheated at 100°C, and after curing reaction, obtain flame-retardant epoxy resin composite material.
[0013] The curing reaction involves curing at 80~100℃ for 1.5~2 hours, followed by curing at 120~150℃ for another 1.5~2 hours. Beneficial effects
[0014] The method for modifying epoxy resin with calcium-based MOF synergistic phosphorus and nitrogen flame retardants provided by the present invention can significantly improve the limiting oxygen index and vertical burning rating of epoxy resin under low addition conditions, effectively reduce the heat release, smoke release rate and heat release, and smoke release amount of epoxy numerical material combustion, while taking into account the mechanical properties of the material. Attached Figure Description
[0015] Figure 1 Scanning electron microscope image of calcium terephthalate.
[0016] Figure 2 Scanning electron microscope images of cross sections of epoxy resin composite materials: (a) Example 1, (b) Example 2, (c) Example 3, (d) Example 4.
[0017] Figure 3 Thermogravimetric analysis of aluminum diethylphosphonate, melamine polyphosphate, and calcium terephthalate under nitrogen conditions.
[0018] Figure 4 Graphs showing the bending strength and impact strength of the examples and comparative samples. Detailed Implementation
[0019] The technical solutions in the embodiments of the present invention will be clearly and completely described below. The described embodiments are only a part of the embodiments of the present invention, and not all of them. Based on the embodiments of the present invention, all other implementation methods obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Example 1
[0020] The epoxy resin was dried in an oven at 100℃ for 60 min, and the aluminum diethylphosphonate, melamine polyphosphate, and calcium terephthalate were dried in an oven at 60℃ for 4 h. 80 g of epoxy resin E44 was weighed and preheated at 60℃. Under ultrasonic assistance, 2.67 g of aluminum diethylphosphonate, 1.33 g of melamine polyphosphate, and 0.8 g of calcium terephthalate were premixed and added to the epoxy resin. After thorough dispersion, 20 g of curing agent 4,4'-diaminodiphenylmethane was added to obtain a homogeneous mixture. The mixture was poured into a mold preheated at 100℃, and the curing temperature and time were 80℃ / 2 h and 120℃ / 2 h, respectively. After natural cooling and demolding, the flame-retardant epoxy resin composite material was obtained. Example 2
[0021] The epoxy resin was dried in an oven at 100℃ for 60 min, and the aluminum diethylphosphonate, melamine polyphosphate, and calcium terephthalate were dried in an oven at 60℃ for 4 h. 80 g of epoxy resin E44 was weighed and preheated at 60℃. Under ultrasonic assistance, 2.67 g of aluminum diethylphosphonate, 1.33 g of melamine polyphosphate, and 1.6 g of calcium terephthalate were premixed and added to the epoxy resin. After thorough dispersion, 20 g of curing agent 4,4'-diaminodiphenylmethane was added to obtain a homogeneous mixture. The mixture was poured into a mold preheated at 100℃, and the curing temperature and time were 80℃ / 2 h and 120℃ / 2 h, respectively. After natural cooling and demolding, the flame-retardant epoxy resin composite material was obtained. Example 3
[0022] The epoxy resin was dried in an oven at 100℃ for 60 min, and the aluminum diethylphosphonate, melamine polyphosphate, and calcium terephthalate were dried in an oven at 60℃ for 4 h. 80 g of epoxy resin E44 was weighed and preheated at 60℃. Under ultrasonic assistance, 2.67 g of aluminum diethylphosphonate, 1.33 g of melamine polyphosphate, and 2.4 g of calcium terephthalate were premixed and added to the epoxy resin. After thorough dispersion, 20 g of curing agent 4,4'-diaminodiphenylmethane was added to obtain a homogeneous mixture. The mixture was poured into a mold preheated at 100℃, and the curing temperature and time were 80℃ / 2 h and 120℃ / 2 h, respectively. After natural cooling and demolding, the flame-retardant epoxy resin composite material was obtained. Example 4
[0023] The epoxy resin was dried in an oven at 100℃ for 60 min, and the aluminum diethylphosphonate, melamine polyphosphate, and calcium terephthalate were dried in an oven at 60℃ for 4 h. 80 g of epoxy resin E44 was weighed and preheated at 60℃. Under ultrasonic assistance, 2.67 g of aluminum diethylphosphonate, 1.33 g of melamine polyphosphate, and 3.2 g of calcium terephthalate were premixed and added to the epoxy resin. After thorough dispersion, 20 g of curing agent 4,4'-diaminodiphenylmethane was added to obtain a homogeneous mixture. The mixture was poured into a mold preheated at 100℃, and the curing temperature and time were 80℃ / 2 h and 120℃ / 2 h, respectively. After natural cooling and demolding, the flame-retardant epoxy resin composite material was obtained. Example 5
[0024] The epoxy resin was dried in an oven at 100℃ for 60 min, and the aluminum diethylphosphonate, melamine polyphosphate, and calcium terephthalate were dried in an oven at 60℃ for 4 h. 80 g of epoxy resin E44 was weighed and preheated at 60℃. Under ultrasonic assistance, 2.67 g of aluminum diethylphosphonate, 1.33 g of melamine polyphosphate, and 4 g of calcium terephthalate were premixed and added to the epoxy resin. After thorough dispersion, 20 g of curing agent 4,4'-diaminodiphenylmethane was added to obtain a homogeneous mixture. The mixture was poured into a mold preheated at 100℃, and the curing temperature and time were 80℃ / 2 h and 120℃ / 2 h, respectively. After natural cooling and demolding, the flame-retardant epoxy resin composite material was obtained. Example 6
[0025] The epoxy resin was dried in an oven at 100℃ for 60 min, and the aluminum diethylphosphonate, melamine polyphosphate, and calcium terephthalate were dried in an oven at 60℃ for 4 h. 80 g of epoxy resin E44 was weighed and preheated at 60℃. Under ultrasonic assistance, 5.34 g of aluminum diethylphosphonate, 2.66 g of melamine polyphosphate, and 2.4 g of calcium terephthalate were premixed and added to the epoxy resin. After thorough dispersion, 20 g of curing agent 4,4'-diaminodiphenylmethane was added to obtain a homogeneous mixture. The mixture was poured into a mold preheated at 100℃, and the curing temperature and time were 80℃ / 2 h and 120℃ / 2 h, respectively. After natural cooling and demolding, the flame-retardant epoxy resin composite material was obtained. Example 7
[0026] The epoxy resin was dried in an oven at 100℃ for 60 min, and the aluminum diethylphosphonate, melamine polyphosphate, and calcium terephthalate were dried in an oven at 60℃ for 4 h. 80 g of epoxy resin E44 was weighed and preheated at 60℃. Under ultrasonic assistance, 10.68 g of aluminum diethylphosphonate, 5.32 g of melamine polyphosphate, and 2.4 g of calcium terephthalate were premixed and added to the epoxy resin. After thorough dispersion, 20 g of curing agent 4,4'-diaminodiphenylmethane was added to obtain a homogeneous mixture. The mixture was poured into a mold preheated at 100℃, and the curing temperature and time were 80℃ / 2 h and 120℃ / 2 h, respectively. After natural cooling and demolding, the flame-retardant epoxy resin composite material was obtained. Example 8
[0027] Preparation of flame-retardant epoxy resin composite material: Epoxy resin was dried in an oven at 100℃ for 60 min. Diethylphosphonate aluminum, melamine polyphosphate, and calcium terephthalate were dried in an oven at 60℃ for 4 h. 80 g of epoxy resin E44 was weighed and preheated at 60℃. Under ultrasonic assistance, 2.4 g of diethylphosphonate aluminum, 1.6 g of melamine polyphosphate, and 2.4 g of calcium terephthalate were premixed and added to the epoxy resin. After thorough dispersion, 20 g of curing agent 4,4'-diaminodiphenylmethane was added to obtain a homogeneous mixture. The mixture was poured into a mold preheated at 100℃, and the curing temperature and time were 80℃ / 2 h and 120℃ / 2 h, respectively. After natural cooling and demolding, the flame-retardant epoxy resin composite material was obtained. Example 9
[0028] The epoxy resin was dried in an oven at 100℃ for 60 min, and the aluminum diethylphosphonate, melamine polyphosphate, and calcium terephthalate were dried in an oven at 60℃ for 4 h. 80 g of epoxy resin E44 was weighed and preheated at 60℃. Under ultrasonic assistance, 3 g of aluminum diethylphosphonate, 1 g of melamine polyphosphate, and 2.4 g of calcium terephthalate were premixed and added to the epoxy resin. After thorough dispersion, 20 g of curing agent 4,4'-diaminodiphenylmethane was added to obtain a homogeneous mixture. The mixture was poured into a mold preheated at 100℃, and the curing temperature and time were 80℃ / 2 h and 120℃ / 2 h, respectively. After natural cooling and demolding, the flame-retardant epoxy resin composite material was obtained. Comparative Example 1
[0029] The epoxy resin was dried in an oven at 100℃ for 60 minutes, and the aluminum diethylphosphonate and melamine polyphosphate were dried in an oven at 60℃ for 4 hours. 80g of epoxy resin E44 was weighed and preheated at 60℃. Under ultrasonic assistance, 4.27g of aluminum diethylphosphonate and 2.13g of melamine polyphosphate were premixed and added to the epoxy resin. After thorough dispersion, 20g of curing agent 4,4'-diaminodiphenylmethane was added to obtain a homogeneous mixture. The mixture was poured into a mold preheated at 100℃, and the curing temperature and time were 80℃ / 2h and 120℃ / 2h, respectively. After natural cooling and demolding, the flame-retardant epoxy resin composite material was obtained. Comparative Example 2
[0030] The epoxy resin was dried in an oven at 100℃ for 60 minutes, and the ammonium polyphosphate, pentaerythritol, and calcium terephthalate were dried in an oven at 60℃ for 4 hours. 80g of epoxy resin E44 was weighed and preheated at 60℃. Under ultrasonic assistance, 2.67g of ammonium polyphosphate, 1.33g of pentaerythritol, and 2.4g of calcium terephthalate were premixed and added to the epoxy resin. After thorough dispersion, 20g of curing agent 4,4'-diaminodiphenylmethane was added to obtain a homogeneous mixture. The mixture was poured into a mold preheated at 100℃, and the curing temperature and time were 80℃ / 2h and 120℃ / 2h, respectively. After natural cooling and demolding, the flame-retardant epoxy resin composite material was obtained.
[0031] Table 1. Formulation table of the examples and comparative samples.
[0032]
[0033] Each group of flame-retardant epoxy resin composite materials was subjected to limiting oxygen index (LOI), UL-94 vertical burning test, cone calorimetry test, and mechanical test. The test results are shown in Table 2.
[0034] Table 2 Flame retardant and mechanical properties of samples in each embodiment and comparative example
[0035] As shown in Table 2, compared with the comparative example, the limiting oxygen index of the examples with added calcium terephthalate was significantly improved compared with that of the comparative example 1 without added calcium terephthalate, and the vertical burning rating reached V-0. Cone calorimetry results showed that the material combustion parameters of the examples—maximum heat release rate (pHRR), total heat release (THR), and smoke production rate (SPR)—were significantly lower than those of the comparative example, indicating that the addition of calcium terephthalate can further improve the flame retardant properties of epoxy resin and enhance the fire safety performance of the material application. Mechanical property test results indicate that the calcium terephthalate synergistic phosphorus-nitrogen compound flame retardant system can improve the flame retardant properties of epoxy resin while maintaining the mechanical properties of the material.
[0036] The specific embodiments described above are only a part of the implementation methods of the present invention. Without departing from the content of the present invention, improvements and modifications can be made to the methods of the present invention, and these improvements and modifications should also be considered within the protection scope of the present invention.
Claims
1. A calcium-based MOF material synergistic with flame-retardant epoxy resin composite material, characterized in that, In the composite material, the amount of the compounded flame retardant added is 5-20% of the epoxy resin mass, the amount of the calcium-based MOF material added is 1-5% of the epoxy resin mass, and the amount of the curing agent added is 20% of the epoxy resin mass; the calcium-based MOF material is calcium terephthalate; the compounded flame retardant is a compounded flame retardant composed of aluminum diethylphosphinate and melamine polyphosphate.
2. The flame-retardant epoxy resin composite material according to claim 1, characterized in that, In the compound flame retardant, the weight ratio of aluminum diethylphosphonate and melamine polyphosphate is 1.5~3:
1.
3. The flame-retardant epoxy resin composite material according to claim 1, characterized in that, The epoxy resin is one or more of bisphenol A type epoxy resin, bisphenol S type epoxy resin, and bisphenol F type epoxy resin.
4. The flame-retardant epoxy resin composite material according to claim 1, characterized in that, The curing agent is selected from one or more of amine curing agents, imidazole curing agents, or acid anhydride curing agents.
5. The method for preparing the flame-retardant epoxy resin composite material according to claim 1, characterized in that, The preparation method includes the following steps: (1) Raw material pretreatment: Dry the epoxy resin in an oven at 100℃ for 30~60min, and dry the aluminum diethylphosphonate, melamine polyphosphate and calcium terephthalate in an oven at 60℃ for 4~6h; (2) Weigh each component by mass percentage, stir and premix aluminum diethylphosphonate, melamine polyphosphate and calcium terephthalate, and then ultrasonically disperse them uniformly in epoxy resin at 60°C; then add curing agent to form a uniform mixture. (3) Pour the mixture from step (2) into a template preheated at 100°C and allow it to cure to obtain a flame-retardant epoxy resin composite material.
6. The method for preparing the flame-retardant epoxy resin composite material according to claim 5, characterized in that, The curing reaction is carried out at 80~100℃ for 1.5~2 hours, and then the temperature is raised to 120~150℃ for 1.5~2 hours.
Citation Information
Patent Citations
Flame retardant catalyst of metal organic frame complex and preparation method thereof
CN106046389A