Alloy steel material, preparation method, shaft assembly and electronic equipment
By preparing specific alloy steel materials and adopting metal injection molding technology, combining solid solution treatment and aging treatment, the problem of insufficient strength and toughness of existing alloy materials is solved, and the balance of high strength, high hardness and toughness is achieved, which is suitable for Folding machine shaft assembly and other applications.
Patent Information
- Application Number
- CN202310546560.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-15
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-05-15
AI Technical Summary
Existing alloy materials cannot meet the needs of higher strength and toughness, especially in folding machine shaft assembly, which is difficult to achieve both light and high strength.
By preparing a specific alloy steel material, its composition includes elements such as nickel Ni, molybdenum Mo, cobalt Co, carbon C and iron Fe, it is prepared by metal injection molding process, combined with solid solution treatment and aging treatment, martensite and Austenitic structure to improve the strength and toughness of the material.
The yield strength of alloy steel materials exceeds 2000MPa, tensile strength exceeds 2100MPa and hardness exceeds 600HV, meeting the needs of high strength, high hardness and toughness, while reducing the preparation cost.
Smart Images

Figure CN117702002B_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of composite materials, and in particular relates to alloy steel materials, preparation methods, shaft assemblies and electronic equipment. Background Art
[0002] In recent years, electronic devices have become an important part of people's lives. With the increasing demand for electronic devices, various forms of electronic products have emerged. Among them, the demand for folding devices is also increasing. For example, folding mobile phones, this new form of mobile phone has been favored by people and developed rapidly after it came out. Since folding machines are folded with two screens, the thinness of folding machines is crucial to improving consumer experience. Since the folding machine mainly connects the two screens through the folding machine shaft assembly, the structure and volume of the shaft assembly largely determine the thickness of the folding phone when it is in the folded form. Therefore, in order to achieve thinness and ensure that the folding machine shaft assembly has a reliable rotation function under the premise of continuously compressing the volume, the material for preparing the shaft assembly will put forward higher strength and toughness requirements. Therefore, it is urgent to develop a high-strength and high-toughness alloy material. Summary of the invention
[0003] In view of this, the present application provides an alloy steel material, a preparation method, a shaft assembly and an electronic device to solve the problem that existing alloy materials cannot meet the requirements of higher strength and toughness.
[0004] Some embodiments of the present application provide an alloy steel material. The present application is introduced from multiple aspects below, and the embodiments and beneficial effects of the following multiple aspects can be referenced to each other.
[0005] In a first aspect, the present application provides a kind of 1. alloy steel material, characterized in that the alloy steel material includes the following components, and the weight percentage of each component is: nickel Ni: 12wt%-16wt%; molybdenum Mo: 6.0wt%-10.0wt%; cobalt Co: 10.0wt%-16.0wt%; carbon C≤0.10wt%; the balance is iron Fe and unavoidable impurities.
[0006] Since the alloy steel material of the embodiment of the present application has the above-mentioned components and contents, its yield strength can reach above 2000 MPa; the material hardness (surface / core) can reach 700 HV.
[0007] As an embodiment of the first aspect of the present application, the weight percentages of the components are: nickel Ni: 12wt%-14wt%; molybdenum Mo: 6.5wt%-8.5wt%; cobalt Co: 13wt%-15wt%; carbon C≤0.05wt%; the remainder is iron Fe and unavoidable impurities.
[0008] As an embodiment of the first aspect of the present application, the alloy steel material further includes a component of niobium Nb, and the weight percentage of Nb is ≤1wt%. By increasing the component of niobium Nb, niobium Nb reacts with iron to form a Fe-Nb phase, which can refine the grain structure and produce a fine grain strengthening effect. Using a weight percentage of niobium Nb of ≤1wt% can effectively improve the material strength, such as yield strength and hardness, and toughness and plasticity, such as tensile strength.
[0009] As an embodiment of the first aspect of the present application, the weight percentage of each component is: nickel Ni: 13wt%; molybdenum Mo: 6.5wt%-8wt%; cobalt Co: 14wt%; carbon C: 0.01wt%; niobium Nb: 0.4%; the remainder is iron Fe and inevitable impurities. The alloy steel material with this composition and content has good comprehensive strength and toughness.
[0010] As an embodiment of the first aspect of the present application, the unavoidable impurities include components of manganese Mn and silicon Si, wherein the weight percentage of Mn is less than 0.5wt%, and the weight percentage of Si is less than 0.5wt%. By controlling the content of impurities, it is possible to avoid the impurities from affecting the formation of Mo-Fe phase, Mo-Ni strengthening phase and Fe-Nb phase, and to avoid the impurities from affecting the strength and toughness of the material.
[0011] As an embodiment of the first aspect of the present application, the alloy steel material has a martensite structure and an austenite structure.
[0012] As an embodiment of the first aspect of the present application, the yield strength of the alloy steel material is greater than 2000 MPa, and the tensile strength of the alloy steel material is greater than 2100 MPa.
[0013] As an embodiment of the first aspect of the present application, the hardness of the alloy steel material is greater than 600 HV.
[0014] In a second aspect, the present application also discloses a method for preparing an alloy steel material, comprising:
[0015] An alloy powder is provided, wherein the weight percentage of each component in the alloy powder is: nickel Ni: 12wt%-16wt%; molybdenum Mo: 6.0wt%-10.0wt%; cobalt Co: 10.0wt%-16.0wt%; carbon C≤0.10wt%; the remainder is iron Fe and unavoidable impurities;
[0016] The alloy powder is subjected to metal injection molding to obtain an alloy steel material.
[0017] According to the preparation method of the embodiment of the present application, the alloy steel material is prepared by using the alloy powder of the above components and the metal injection molding process in the preparation process, which has higher strength and toughness than the alloy steel material of the prior art. Moreover, the preparation process is simple, and a fine alloy steel material can be prepared, and the manufacturing cost is low.
[0018] As an embodiment of the second aspect of the present application, metal injection molding includes: mixing, injection molding, degreasing, sintering and heat treatment.
[0019] As an embodiment of the second aspect of the present application, the particle size diameter distribution of the alloy powder is D50: 5-12um, D90: 15-25um, and the tap density of the alloy powder is ≥4.20g / cm 3 . This particle size distribution is beneficial to improving the strength and toughness of alloy steel materials.
[0020] As an embodiment of the second aspect of the present application, the particle size diameter distribution of the alloy powder is D50: 7-9um, D90: 16-20um, and the tap density is ≥ 4.5g / cm 3 .
[0021] As an embodiment of the second aspect of the present application, mixing includes: pouring the alloy powder and the binder into a mixer in a volume ratio of (1.2-2.3):1, mixing at a mixing temperature of 160°C-210°C, and mixing for 1-4 hours to obtain a flexible adhesive. The alloy powder and the binder in this ratio are conducive to the agglomeration of the powder and improve the rheological properties of the feed.
[0022] As an embodiment of the second aspect of the present application, the volume ratio of alloy powder to binder is (1.27-1.78): 1. This ratio of alloy powder to binder is conducive to the agglomeration of powders, forming a flexible adhesive, further improving the rheological properties of the feed, and ensuring that the green body is smoothly separated from the mold.
[0023] As an embodiment of the second aspect of the present application, the binder is one or more of polyoxymethylene, high-density polyethylene, polypropylene, paraffin, ethylene-vinyl acetate copolymer, polymethyl methacrylate, stearic acid, and an antioxidant.
[0024] As an embodiment of the second aspect of the present application, injection molding includes: injecting a flexible binder at an injection temperature of 160°C-210°C to obtain a green embryo. This temperature is conducive to the molding of the alloy material, and can avoid the binder in the unmolded alloy material being removed due to excessively high temperature and causing cracks, bulges, deformation or collapse of the green embryo.
[0025] As an embodiment of the second aspect of the present application, degreasing includes: performing acid catalyst catalytic degreasing or solvent degreasing on the injection molded green body to remove the binder. The use of the catalytic medium can effectively remove the polymer binder in the green body, and the degreasing efficiency is high.
[0026] As an embodiment of the second aspect of the present application, the degreasing temperature is between 120-130° C., and the catalytic degreasing time is 1-10 h.
[0027] As an embodiment of the second aspect of the present application, the catalytic medium is nitric acid or oxalic acid.
[0028] As an embodiment of the second aspect of the present application, sintering includes: sintering the degreased green embryo in a vacuum atmosphere at a sintering temperature of 1200-1400° C. for a holding time of 1-6 hours to obtain a cooked embryo.
[0029] As an embodiment of the second aspect of the present application, the heat treatment includes:
[0030] Solution treatment: keep the sintered embryo at 850-1100℃ for 1-3h, and then use high-pressure inert gas to quickly cool the embryo; the pressure of the inert gas is >6bar;
[0031] Aging treatment: keep the solution treated embryo at 400-600℃ for 60-360 minutes.
[0032] Solution treatment and aging treatment are beneficial to the formation of martensite and austenite, so that the alloy steel material has stronger strength and toughness.
[0033] As an embodiment of the second aspect of the present application, the heat treatment includes:
[0034] Solution treatment: keep the sintered embryo at 1000-1100℃ for 1-1.5h, and then use high-pressure inert gas to quickly cool the embryo; the pressure of the inert gas is >8bar;
[0035] Cryogenic treatment: The cooked embryo that has undergone solution treatment is placed at a temperature below -180°C for a deep cooling time of more than 1 hour;
[0036] Aging treatment: Keep the deep-cold-treated embryo at 500-550℃ for 4-5h.
[0037] This method is beneficial to the formation of martensite and austenite, thereby making the alloy steel material have greater strength and toughness.
[0038] In a third aspect, the present application further discloses a shaft assembly, which is made of the alloy steel material as in the embodiment of the first aspect.
[0039] In a fourth aspect, an embodiment of the present application further discloses an electronic device, including:
[0040] The housing comprises a first frame and a second frame.
[0041] A folding screen, the folding screen comprises a first screen and a second screen, the first screen is arranged on the first frame, and the second screen is arranged on the second frame;
[0042] The shaft assembly is arranged in the shell, and the two ends are respectively connected to the first frame and the second frame, and is used to make the first screen and the second screen rotatably connected. The shaft assembly is the shaft assembly explained in the embodiment of the third aspect. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 A process flow chart of a method for preparing an alloy steel material in one embodiment;
[0044] Figure 2 A process flow chart of a method for preparing an alloy steel material in another embodiment;
[0045] Figure 3 This is a schematic diagram of the structure of a foldable screen mobile phone in different states according to an embodiment of the present application;
[0046] Figure 4 This is a flow chart of a method for preparing an alloy steel material according to an embodiment of the present application;
[0047] Figure 5 This is a flow chart of a method for preparing an alloy steel material by using a metal injection molding process according to an embodiment of the present application;
[0048] Figure 6 The metallographic structure diagram of the alloy steel material prepared in Example 8 of the present application;
[0049] Figure 7 This is the metallographic structure diagram of the alloy steel material prepared in Example 11 of the present application. DETAILED DESCRIPTION
[0050] The following will provide a clear and complete description of the various embodiments of the present application in conjunction with the accompanying drawings.
[0051] In order to facilitate understanding of the technical solution of the present application, the technical problem of the present application is first described below.
[0052] Since the shaft assembly of the folding machine has a complex and fine three-dimensional structure, in some schemes, the shaft assembly with a complex structure is prepared by using profiles and machining. This manufacturing method is costly and inefficient. In order to reduce costs and improve efficiency, in some schemes, the shaft assembly is prepared by metal powder injection molding. The metal powder injection molding method is a powder metallurgy method close to net molding, which can mass-produce metal parts with complex three-dimensional shapes. Therefore, the use of metal powder injection molding has attracted much attention.
[0053] refer to Figure 1 , Figure 1 A process flow chart of a method for preparing an alloy steel material in one embodiment is shown. Figure 1 As shown in the figure, the process includes powder making, mixing, injection molding, degreasing, sintering, shaping, heat treatment and surface treatment. This method mainly adopts the method of maraging steel powder injection molding + heat treatment. The problem is that the conventional maraging steel has low strength and yield strength of 1500-1850MPa, which cannot meet the needs of continuous thinning.
[0054] refer to Figure 2 , Figure 2 FIG. 2 shows a process flow chart of a method for preparing an alloy steel material in another embodiment. Figure 2 As shown in FIG. 1 , the flow chart mainly includes smelting, forging, cold drawing, CNC machining, heat treatment and surface treatment. This solution mainly adopts the method of maraging steel profile + cold drawing + CNC machining + heat treatment. The problems are high machining cost, low machining efficiency, difficulty in machining micro and three-dimensional complex structural parts, and the strength and toughness cannot meet the requirements.
[0055] In order to solve the problem of insufficient strength of stainless steel materials for metal injection molding in the above scheme and high cost of CNC machining of high-strength steel profiles, the present application provides an alloy steel material. By studying the components and contents in the material, a reasonable component and content are adopted, and the alloy steel material is obtained by combining the metal injection molding process. The alloy steel material has ultra-high yield strength, hardness and tensile strength, and can prepare complex product structures at low cost.
[0056] The following describes the preparation method of the alloy steel material according to the embodiment of the present application and the use of the alloy steel material in conjunction with the accompanying drawings.
[0057] According to an embodiment of the present application, an alloy steel material is provided, which includes the following components, and the weight percentage of each component is: nickel Ni: 12wt%-16wt%; molybdenum Mo: 6.0wt%-10.0wt%; cobalt Co: 10.0wt%-16.0wt%; carbon C≤0.10wt%; the balance is iron Fe and unavoidable impurities.
[0058] Among them, the role of nickel Ni in the preparation of alloy steel materials is to expand the austenite phase region, ensure the volume of lath martensite after solid solution rapid cooling, and improve the plasticity of the material.
[0059] Cobalt Co can indirectly improve the strengthening effect of alloy materials. It promotes the precipitation of Mo-Fe phase and Mo-Ni strengthening phase by reducing the solid solubility of Mo element in the lath martensite matrix. It also inhibits the recovery of martensite substructure during aging treatment and provides more nucleation sites for precipitation phase.
[0060] Molybdenum (Mo) is a strengthening alloy element. It reacts with Ni and Fe to disperse and precipitate Mo-Fe phase and Mo-Ni strengthening phase to improve the strength of the material.
[0061] In the embodiment of the present application, the sum of the content of molybdenum Mo and nickel Ni is in the range of 18%-26%. Within this range, the yield strength of the alloy steel material can be greater than 2000MPa, and the tensile strength can be greater than 2100MPa, and because the alloy steel material has good plasticity, the yield strength and tensile strength are positively correlated. If the sum of the Mo and Ni element contents is less than 18%, the yield strength of the material is less than 2000MPa; if the sum of the Mo and Ni element contents accounts for more than 26%, the yield strength and tensile strength are negatively correlated due to the low plasticity of the material, that is, the higher the yield strength, the lower the tensile strength. Therefore, the alloy steel material in the embodiment of the present application has high yield strength, tensile strength and hardness, and can meet the current demand for high strength and high hardness of the shaft assembly.
[0062] In one embodiment of the present application, the weight percentage of each component is: nickel Ni: 12wt%-14wt%; molybdenum Mo: 6.5wt%-8.5wt%; cobalt Co: 13wt%-15wt%; carbon C≤0.05; the remainder is iron Fe and inevitable impurities. The alloy steel material with this composition and content has better strength and toughness.
[0063] Due to the above components and contents, its yield strength can reach above 2000MPa; the material hardness (surface / core) can reach 700HV.
[0064] In one embodiment of the present application, the alloy steel material further includes a component of niobium Nb, and the weight percentage of Nb is ≤1%. Niobium Nb reacts with iron to form a Fe-Nb phase, which can refine the grain structure, produce a fine grain strengthening effect, and improve the material strength, such as yield strength and hardness, and toughness and plasticity, such as tensile strength.
[0065] In the embodiment of the present application, the unavoidable impurities include components of manganese Mn and silicon Si, wherein the weight percentage of Mn is less than 0.5wt%, and the weight percentage of Si is less than 0.5wt%. By controlling the content of impurities, it is possible to avoid the impurities from affecting the formation of Mo-Fe phase, Mo-Ni strengthening phase and Fe-Nb phase, and to avoid the impurities from affecting the strength and toughness of the material.
[0066] In the embodiments of the present application, the yield strength of the alloy steel material is greater than 2000 MPa, and the tensile strength of the alloy steel material is greater than 2100 MPa.
[0067] In the embodiment of the present application, the hardness of the alloy steel material is greater than 600 HV.
[0068] It should be noted that in some embodiments of the present application, in addition to the above-mentioned components, other ingredients may be added as needed, for example, rare earth elements, aluminum (Al) or titanium (Ti), etc., so as to meet the requirements of other material properties, such as the magnetism, luminescence or electrochemical properties of the material, on the basis of the improved strength (yield strength and hardness) and toughness (tensile strength) achieved in the above-mentioned embodiments of the present application.
[0069] The alloy steel material of the embodiment of the present application can be applied to electronic devices. For example, the alloy steel material is processed into a shaft assembly and applied to a foldable electronic device. For example, taking a folding screen mobile phone as an example, it can be used as a shaft assembly for realizing the unfolding or folding of two screens. The shaft assembly can be made more compact, and the strength and toughness of the shaft can be guaranteed to meet the requirements of the mobile phone being thin and light. It can also be used for other opening and closing devices, for example, clamshell electronic devices, such as laptop computers and other structural parts with opening and closing actions.
[0070] The following description will take a foldable screen mobile phone as an example of an electronic device.
[0071] refer to Figure 3 , Figure 3 The structure diagram of the folding screen mobile phone in the embodiment of the present application is shown. Figure 3 (a)- Figure 3 As shown in (c) in the figure, the folding screen mobile phone includes a shell, a folding screen and a hinge assembly 30.
[0072] Among them, Figure 3As shown in (c) in the figure, the housing includes a first frame body 11 and a second frame body 12. The folding screen includes a first screen 21 and a second screen 22, wherein the first screen 21 is disposed on the first frame body 11, and the second screen 22 is disposed on the second frame body 12. The hinge assembly 30 is disposed in the housing and fixed on the housing. The two ends of the hinge assembly 30 are respectively connected to the first frame body 11 and the second frame body 12. Since the hinge can be opened and closed, the hinge assembly 30 can realize the folding of the mobile phone screen. Figure 3 As shown in (a) of FIG. 1 , the mobile phone is in the unfolded state, and after the rotation of the shaft assembly 30, the mobile phone is in the unfolded state. Figure 3 The folding action of (b) in the figure is performed, thereby realizing the rotatable connection between the first screen 21 and the second screen 22. Since the hinge assembly 30 is made of the alloy steel material in the above embodiment, the hinge assembly can be made more compact and can ensure strength and toughness, the mobile phone as a whole can be thinner and lighter, and the service life will also be improved.
[0073] It should be noted that the structure of the above electronic device is only an exemplary description. In some embodiments, the hinge assembly may be arranged in the middle of a non-display screen, or one side of the hinge assembly may be connected to a frame on which a display screen is mounted, and the other side may be connected to a mobile phone cover, etc. The present application does not limit the specific application and structure of the hinge assembly.
[0074] According to the foldable electronic device of the embodiment of the present application, since the hinge assembly is made of the alloy steel material of the embodiment of the present application, the foldable electronic device can be light and thin. In addition, the hinge assembly has high strength and toughness, which is conducive to extending the service life of the electronic device.
[0075] In other embodiments of the present application, the alloy steel material can also be applied to other electronic devices, not only as a rotating shaft, but also as other components with high strength and toughness requirements. Among them, the electronic device can be a mobile phone, or a tablet computer, a mobile phone, an e-reader, a remote control, a personal computer (personal computer, PC), a laptop, a personal digital assistant (personal digital assistant, PDA), a vehicle-mounted device, an Internet TV, a wearable device, a TV, and other products with a display interface, as well as smart display wearable products such as smart watches and smart bracelets. The embodiments of the present application do not impose any special restrictions on the form of the above-mentioned electronic devices.
[0076] In addition, the alloy steel material of the embodiment of the present application can also be applied to other technical fields, such as photovoltaics, semiconductors, etc., for making other devices, for precision forging dies and plastic molds. The present application does not limit the application fields.
[0077] The preparation method of the alloy steel material in the embodiment of the present application is described below with reference to the accompanying drawings.
[0078] refer to Figure 4 , Figure 4 The flowchart of the method for preparing the alloy steel material of the embodiment of the present application is shown. Figure 4 As shown, the method includes S410 - S420 as explained below.
[0079] S410, preparing alloy powder.
[0080] Among the components of the alloy powder, the weight percentage of each component can be: nickel Ni: 12wt%-16wt%, for example, 13wt%, 14wt% or 15wt%, etc.; molybdenum Mo: 6.0wt%-10.0wt%, for example, 6.5wt%, 7wt%, 7.5wt%, 8wt%, 8.5wt% or 9wt%, etc.; cobalt Co: 10.0wt%-16.0wt%, for example, 11wt%, 12wt%, 13wt%, 14wt% or 15wt%, etc.; carbon C≤0.10wt%, for example, 0.01wt%, 0.02wt% or 0.05wt%, etc.; the remainder is iron Fe and unavoidable impurities. The alloy powder with this component and content has strong strength and toughness after preparing alloy steel material.
[0081] In some embodiments, the weight percentage of each component can be: nickel Ni: 12wt%-14wt%, for example, 12.5wt% or 13.5wt%; molybdenum Mo: 6.5wt%-8.5wt%; cobalt Co: 13wt%-15wt%; carbon C≤0.05wt%; the remainder is iron Fe and inevitable impurities. After the alloy steel material is prepared with the alloy powder of this component and content, its strength and toughness are significantly better than the alloy steel material of the prior art.
[0082] In some embodiments, the weight percentage of each component can be: nickel Ni: 12wt%-14wt%; molybdenum Mo: 6.5wt%-8.5wt%; cobalt Co: 13wt%-15wt%; niobium Nb≤1wt%; carbon C≤0.05wt%; the balance is iron Fe and inevitable impurities. By increasing the component niobium Nb, niobium Nb reacts with iron to form Fe-Nb phase, which can refine the grain structure and produce fine grain strengthening effect. Using niobium Nb weight percentage ≤1wt% can effectively improve material strength, such as yield strength and hardness, and toughness and plasticity, such as tensile strength.
[0083] The alloy steel material prepared by the above components has high yield strength, tensile strength and hardness, and can meet the current demand for high strength and high hardness of the shaft assembly.
[0084] In one embodiment of the present application, the alloy powder can be prepared by high-pressure water atomization / gas atomization. The particle size characteristic distribution of the alloy powder is D50: 5-12um, such as 6um, 7um, 8um, 9um, 10um or 11um, etc., D90: 15-25um, such as 17um, 19um, 21um, 22um or 24um. D50 represents 50% of the particle size, that is, the volume content of particles with a particle size below 5-12μm accounts for 50% of all particles. D90: 15-25um, the volume content of particles with a particle size below 15-25um accounts for 90% of all particles. The tap density of the alloy powder is ≥4.20g / cm 3 .
[0085] In some embodiments, the alloy powder has a powder size distribution of D50: 7-9 um, D90: 16-20 um, and a tap density of ≥ 4.5 g / cm 3 . This particle size distribution is beneficial to improving the strength and toughness of alloy steel materials.
[0086] S420, subjecting the alloy powder to a metal injection molding (MIM) process to obtain an alloy steel material (or an alloy steel material product).
[0087] According to the preparation method of the embodiment of the present application, the alloy steel material is prepared by using the alloy powder of the above components and the metal injection molding process in the preparation process, which has higher strength and toughness than the alloy steel material of the prior art. Moreover, the preparation process is simple, and a fine alloy steel material can be prepared, and the manufacturing cost is low.
[0088] In one embodiment of the present application, metal injection molding may include steps such as mixing, injection molding, debinding, sintering and heat treatment.
[0089] refer to Figure 5 , Figure 5 The flowchart of the method for preparing alloy steel material by metal injection molding process in the embodiment of the present application is shown. Figure 5 As shown, the flow chart includes S421-S425 as explained below. That is, the alloy powder prepared in S410 is sequentially subjected to mixing, injection molding, degreasing, sintering and heat treatment to obtain the alloy steel material (alloy steel material product).
[0090] The following describes the various steps of preparing the alloy steel material using the MIM process in the embodiments of the present application.
[0091] S421, mixing.
[0092] The alloy powder and the binder in S410 may be mixed in a volume ratio of (1.2-2.3):1, and poured into a mixer for mixing. The mixing temperature may be 160°C-210°C, and the mixing time may be 1 to 4 hours (1-4h).
[0093] In one embodiment of the present application, the volume ratio of alloy powder to binder may be (1.27-1.78): 1. This ratio of alloy powder to binder is conducive to the agglomeration of powders to form a flexible adhesive, and the addition of binder can improve the rheological properties of the feed material and ensure that the green body can be smoothly separated from the mold.
[0094] In one embodiment of the present application, the binder may be a polymer binder, and its composition may be at least one of polyoxymethylene, high-density polyethylene, polypropylene, paraffin, ethylene-vinyl acetate copolymer (EVA), polymethyl methacrylate (PMMA), stearic acid, and an antioxidant. The binder can effectively aggregate the alloy powder, change its rheological properties, and facilitate its release from the mold.
[0095] S422, injection molding.
[0096] In the embodiment of the present application, an injection molding machine can be used for injection molding, wherein the cavity of the injection molding mold is processed in advance into a shape that is close to or close to coupling with the structural product, so as to facilitate molding and obtain a green body. The injection temperature can be 160°C-210°C. This temperature is conducive to the molding of the alloy material, and can avoid the removal of the binder in the unmolded alloy material due to excessive temperature and the occurrence of cracks, bulges, deformation or collapse of the green body.
[0097] S423, degrease.
[0098] In one embodiment of the present application, the injection molded green body is degreased, for example, by acid catalyst catalytic degreasing or solvent degreasing to remove the polymer binder. In some embodiments, the degreasing temperature can be 120-130° C., the catalytic degreasing time can be 1 to 10 hours, and the catalytic medium can be nitric acid or oxalic acid. The use of the catalytic medium can effectively remove the polymer binder in the green body, and the degreasing efficiency is high.
[0099] S424, sintered.
[0100] The degreased green body is sintered in a vacuum atmosphere and an argon protective atmosphere to obtain a cooked body, wherein the sintering temperature may be 1200-1400°C, the holding time may be 1 to 6 hours, and the argon partial pressure may be 10-50 KPa.
[0101] In some embodiments, the sintering temperature may be 1320-1380° C., the holding time may be 2 to 5 hours, and the argon partial pressure may be 15-30 KPa.
[0102] S425, heat treated.
[0103] In one embodiment of the present application, the heat treatment may include two steps: solution treatment and aging treatment.
[0104] The temperature of the solution treatment may be 850-1100°C for 1 to 3 hours, and then the temperature in the furnace chamber is rapidly cooled to below 50°C using high-pressure inert gas, wherein the inert gas pressure is >6 bar.
[0105] After the solution treatment, an aging treatment is performed, wherein the aging treatment temperature may be 400-600°C and the holding time may be 1-6 hours.
[0106] The above process is conducive to the formation of martensite and austenite, so that the alloy steel material has stronger strength and toughness.
[0107] In another embodiment of the present application, the heat treatment may include three steps: solution treatment, cryogenic treatment and aging treatment.
[0108] The temperature of the solution treatment may be 1000-1100°C, the holding time may be 1-1.5 hours, and then the temperature in the furnace cavity is rapidly cooled to below 50°C using high-pressure inert gas, wherein the inert gas pressure is >8 bar.
[0109] Thereafter, a cryogenic treatment is performed at a temperature below -180°C and the cryogenic insulation time is greater than 1 hour.
[0110] After the deep cryogenic treatment, the ripe blank is subjected to aging treatment. The aging treatment temperature may be 500-550° C. and the insulation time may be 4-5 hours.
[0111] After the above steps, the alloy steel material or alloy steel material product of the embodiment of the present application is obtained, and its internal microstructure contains more martensite and austenite, and the material has higher strength and toughness.
[0112] The alloy steel material (product) prepared by the method of the embodiment of the present application can have a yield strength of more than 2000 MPa; the material hardness (surface / core) can reach 600-700 HV. Compared with the yield strength of 1800 MPa of the alloy steel material in the prior art, it is greatly improved. In addition, the metal injection molding process is adopted, the preparation process is simpler, the processing efficiency is high, and complex structural parts can be processed.
[0113] The alloy steel material and the preparation method thereof provided in the embodiments of the present application are described below through 13 specific embodiments and 2 comparative examples.
[0114] Example 1
[0115] 1) Preparation of alloy powder
[0116] The alloy powder is prepared by high-pressure water atomization and the powder raw materials are sieved by air flow classification. The powder composition and characteristics are as follows:
[0117] Chemical composition of powder: carbon (C): 0.02%; nickel (Ni): 12%; molybdenum (Mo): 7.5%; cobalt (Co): 10%; iron: balance.
[0118] Powder particle size specifications: laser particle size D50: 9μm, D90: 23μm.
[0119] 2) Feeding and mixing
[0120] The alloy powder and polyoxymethylene were poured into a Σ-type kneader at a volume ratio of 1.27:1 for mixing at a mixing temperature of 190°C for 1 hour. After mixing, the feed was poured into a mixing extruder for extrusion and granulation.
[0121] 3) Injection molding
[0122] The injection molding is performed using an injection molding machine, and the injection temperature is 190° C. The cavity of the injection molding mold used is pre-processed into a shape that is close to or close to coupling with the structural product.
[0123] 4) Remove the binder
[0124] The injection molded green body is degreased by acid catalyst to remove the polymer binder. The degreasing temperature is 120°C and the catalytic time is 2 hours. The catalytic medium is nitric acid and the protective atmosphere is nitrogen.
[0125] 5) Sintering
[0126] The sintering equipment is a vacuum batch furnace;
[0127] Sintering process: the maximum sintering temperature is 1360℃, and the temperature is kept for 180 minutes; the atmosphere is vacuum, the protective atmosphere is argon, and the argon partial pressure is 15KPa.
[0128] 6) Shaping: Cold shaping is performed on sintered products to ensure the accuracy of part size and shape.
[0129] 7) Heat treatment. Heat treatment is divided into three steps: solution treatment, cryogenic treatment, and aging treatment;
[0130] The solution treatment equipment is a vacuum high-pressure gas quenching furnace; heated to 1080°C and kept warm for 120 minutes; after the end of the insulation, the temperature in the furnace chamber is quickly cooled to below 30°C using high-pressure inert gas, which is nitrogen or argon with a pressure of 8 bar;
[0131] The cryogenic treatment uses a cryogenic treatment tank, the cryogenic treatment temperature is lower than -180℃, and the cryogenic insulation time is greater than 1h;
[0132] The aging treatment equipment is a vacuum heat treatment furnace, which is heated to 520°C and kept warm for 240 minutes; the atmosphere is vacuum.
[0133] Sample 1 of Example 1 was obtained.
[0134] Example 2
[0135] In Example 2, except for the following differences, other steps are the same as those in Example 1, except that:
[0136] Chemical composition of powder: carbon (C): 0.02%; nickel (Ni): 12%; molybdenum (Mo): 8.0%; cobalt (Co): 12%; iron: balance.
[0137] The sample 2 corresponding to Example 2 was obtained.
[0138] Example 3
[0139] In Example 3, except for the following differences, other steps are the same as those in Example 1, except that:
[0140] Chemical composition of powder: carbon (C): 0.02%; nickel (Ni): 13%; molybdenum (Mo): 8.5%; cobalt (Co): 14%; iron: balance.
[0141] The sample 3 corresponding to Example 3 was obtained.
[0142] Example 4
[0143] In Example 4, except for the following differences, other steps are the same as those in Example 1, except that:
[0144] Chemical composition of powder: carbon (C): 0.02%; nickel (Ni): 14%; molybdenum (Mo): 9.0%; cobalt (Co): 15%; iron: balance.
[0145] The sample 4 corresponding to Example 4 was obtained.
[0146] Example 5
[0147] In Example 5, except for the following differences, other steps are the same as those in Example 1, except that:
[0148] Chemical composition of powder: carbon (C): 0.01%; nickel (Ni): 14%; molybdenum (Mo): 9.5%; cobalt (Co): 15%; iron: balance.
[0149] The sample 5 corresponding to Example 5 was obtained.
[0150] Example 6
[0151] In Example 6, except for the following differences, the other steps are the same as those in Example 1, except that:
[0152] Chemical composition of powder: carbon (C): 0.01%; nickel (Ni): 14%; molybdenum (Mo): 10%; cobalt (Co): 15%; iron: balance.
[0153] The sample 6 corresponding to Example 6 was obtained.
[0154] Example 7
[0155] In Example 7, except for the following differences, other steps are the same as those in Example 1, except that:
[0156] Chemical composition of powder: carbon (C): 0.01%; nickel (Ni): 16%; molybdenum (Mo): 10.0%; cobalt (Co): 16%; iron: balance.
[0157] The sample 7 corresponding to Example 7 was obtained.
[0158] Example 8
[0159] In Example 8, except for the following differences, other steps are the same as those in Example 1, except that:
[0160] Chemical composition of the powder: carbon (C): 0.01%; nickel (Ni): 13%; molybdenum (Mo): 9.0%; cobalt (Co): 15%; niobium (Nb): 0.5%; iron: balance.
[0161] Powder particle size specifications: laser particle size D50: 8μm, D90: 18μm.
[0162] The sample 8 corresponding to the embodiment 8 was obtained.
[0163] Example 9
[0164] In Example 9, except for the following differences, the other steps are the same as those in Example 1, except that:
[0165] Chemical composition of the powder: carbon (C): 0.01%; nickel (Ni): 16%; molybdenum (Mo): 10%; cobalt (Co): 15%; niobium (Nb): 0.5%; iron: balance.
[0166] Powder particle size specifications: laser particle size D50: 7μm, D90: 17μm.
[0167] The sample 9 corresponding to Example 9 was obtained.
[0168] Example 10
[0169] In Example 10, except for the following differences, other steps are the same as those in Example 1, except that:
[0170] Chemical composition of the powder: carbon (C): 0.01%; nickel (Ni): 16%; molybdenum (Mo): 10.0%; cobalt (Co): 16%; niobium (Nb): 0.5%; iron: balance.
[0171] Powder particle size specifications: laser particle size D50: 7μm, D90: 17μm.
[0172] The sample 10 corresponding to the embodiment 10 is obtained.
[0173] Embodiment 11
[0174] In Example 11, except for the following differences, other steps are the same as those in Example 1, except that:
[0175] Chemical composition of the powder: carbon (C): 0.01%; nickel (Ni): 13%; molybdenum (Mo): 7.5%; cobalt (Co): 14%; niobium (Nb): 0.4%; iron: balance.
[0176] Powder particle size specifications: laser particle size D50: 8μm, D90: 20μm.
[0177] The sample 11 corresponding to Example 11 was obtained.
[0178] It should be noted that the components in the above embodiments contain inevitable impurities, and the weight percentages of Mn and Si are both less than 0.5wt%.
[0179] Example 12
[0180] In Example 11, except for the following differences, other steps are the same as those in Example 1, except that:
[0181] Chemical composition of the powder: carbon (C): 0.01%; nickel (Ni): 13%; molybdenum (Mo): 6.5%; cobalt (Co): 14%; niobium (Nb): 0.4%; iron: balance.
[0182] Powder particle size specifications: laser particle size D50: 8μm, D90: 20μm.
[0183] The sample 12 corresponding to Example 12 is obtained.
[0184] Embodiment 13
[0185] In Example 11, except for the following differences, other steps are the same as those in Example 1, except that:
[0186] Chemical composition of the powder: carbon (C): 0.01%; nickel (Ni): 13%; molybdenum (Mo): 6.0%; cobalt (Co): 14%; niobium (Nb): 0.4%; iron: balance.
[0187] Powder particle size specifications: laser particle size D50: 8μm, D90: 20μm.
[0188] The sample 13 corresponding to Example 13 was obtained.
[0189] Comparative Example 1
[0190] The powder components used are Ni, Co, Mo, and Fe in mass percentages of 18%, 13.5%, and 9%, respectively, with the remainder being Fe and unavoidable impurities. A premix is prepared by mixing atomized alloy powder with carbonyl alloy powder, and the powder particle size specification is not limited.
[0191] Except for the above differences, the other preparation processes are the same as those in Example 1.
[0192] A comparative sample 1 of comparative example 1 was obtained.
[0193] Comparative Example 2
[0194] The powder composition used is: nickel: 17% to 18%; cobalt: 8.5% to 9.5%; molybdenum: 4.5% to 5.0%; the balance is iron. Powder particle size specification: no limit.
[0195] Except for the above differences, the other preparation processes are the same as those in Example 1.
[0196] The room temperature mechanical properties of the samples of the 11 embodiments and 2 comparative examples were tested: yield strength, tensile strength, elongation and hardness. The results are shown in Table 1.
[0197] Table 1 Performance test results
[0198]
[0199] As can be seen from Table 1, the yield strength of the samples corresponding to the alloy steel materials prepared by the preparation method of the embodiment of the present application can reach more than 2000MPa, and can reach up to 2140MPa, which is much higher than the yield strength of the comparative example, i.e. 1880MPa, 1640MPa and 1350MPa. And the tensile strength of the samples of the embodiment of the present application can reach more than 2100MPa, and can reach up to 2280MPa, which is much higher than the tensile strength of the comparative example 1. The hardness can reach more than 602HV, and can reach up to 700HV, which is higher than the hardness corresponding to the comparative example sample. It can be seen that the strength and toughness of the alloy steel materials of the embodiment of the present application are much higher than the alloy steel materials of the prior art. In addition, the alloy steel materials of the embodiment of the present application can also have a good elongation while ensuring that the strength is large enough, and the elongation can be between 2% and 5%.
[0200] The microstructures of the alloy steel material samples of Example 8 and Example 11 are observed below in conjunction with the accompanying drawings.
[0201] refer to Figure 6 and Figure 7 , Figure 6 The metallographic structure diagram of the alloy steel material prepared in Example 8 of the present application is shown. Figure 7 The metallographic structure diagram of the alloy steel material prepared in Example 11 of the present application is shown. Figure 6 and Figure 7 As shown in the figure, it can be seen from the metallographic structure diagram that the structure is mainly divided into lath martensite and austenite. Among them, lath martensite has ultra-high strength, which improves the yield strength and hardness of alloy steel materials, while austenite has strong plasticity, which can improve the tensile strength of alloy steel materials.
[0202] In addition, the density of the product can reach more than 98%, and the diameter of the sintering pores is generally less than 20 microns, which will not affect the mechanical properties.
[0203] It should be noted that the materials, equipment and steps are not mentioned in the preparation method of the alloy steel material in the embodiment of the present application. The implementation method of the prior art can be referred to and will not be described in detail here.
[0204] Although the present application has been illustrated and described with reference to certain preferred embodiments thereof, it will be apparent to those skilled in the art that various changes in form and details may be made therein without departing from the spirit and scope of the present application.
Claims
1. An alloy steel material, characterized in that: The alloy steel material is composed of the following components, and the weight percentage of each component is: nickel Ni: 12wt%-14wt%; molybdenum Mo: 6.5wt%-8.5wt%; cobalt Co: 13wt%-15wt%; niobium Nb≤1wt%; carbon C≤0.05wt%; the remainder is iron Fe and inevitable impurities; the hardness of the alloy steel material is greater than 600HV, the yield strength of the alloy steel material is greater than 2000MPa, and the elongation range of the alloy steel material is 2%-5%.
2. The alloy steel material according to claim 1, characterized in that: The weight percentages of the components are: nickel Ni: 13wt%; molybdenum Mo: 6.5wt%-8wt%; cobalt Co: 14wt%; carbon C: 0.01wt%; niobium Nb: 0.4%; the remainder is iron Fe and unavoidable impurities.
3. The alloy steel material according to claim 1 or 2, characterized in that: The inevitable impurities include components of manganese Mn and silicon Si, wherein the weight percentage of Mn is less than 0.5wt%, and the weight percentage of Si is less than 0.5wt%.
4. The alloy steel material according to claim 1, characterized in that: The alloy steel material has a martensite structure and an austenite structure.
5. The alloy steel material according to claim 1, characterized in that: The tensile strength of the alloy steel material is greater than 2100 MPa.
6. A method for preparing an alloy steel material, characterized in that: include: An alloy powder is provided, wherein the weight percentage of each component in the alloy powder is: nickel Ni: 12wt%-14wt%; molybdenum Mo: 6.5wt%-8.5wt%; cobalt Co: 13wt%-15wt%; niobium Nb≤1wt%; carbon C≤0.05wt%; the remainder is iron Fe and unavoidable impurities; The alloy powder is subjected to metal injection molding to obtain the alloy steel material; wherein the metal injection molding includes: mixing, injection molding, degreasing, sintering and heat treatment; the heat treatment includes solution treatment, cryogenic treatment and aging treatment; The hardness of the alloy steel material is greater than 600 HV, the yield strength of the alloy steel material is greater than 2000 MPa, and the elongation range of the alloy steel material is 2%-5%.
7. The preparation method according to claim 6, characterized in that: The particle size distribution of the alloy powder is D50: 5-12um, D90: 15-25um, and the tap density of the alloy powder is ≥4.20g / cm 3 .
8. The preparation method according to claim 7, characterized in that: The particle size distribution of the alloy powder is D50: 7-9um, D90: 16-20um, and the tap density is ≥ 4.5g / cm 3 .
9. The preparation method according to claim 6, characterized in that: The mixing comprises: The alloy powder and the binder are poured into a mixer in a volume ratio of (1.2-2.3):1 and mixed at a mixing temperature of 160° C.-210° C. for 1-4 hours to obtain a flexible adhesive.
10. The preparation method according to claim 9, characterized in that: The volume ratio of the alloy powder to the binder is (1.27-1.78):
1.
11. The preparation method according to claim 9 or 10, characterized in that: The binder is one or more of polyoxymethylene, high-density polyethylene, polypropylene, paraffin, ethylene-vinyl acetate copolymer, polymethyl methacrylate, stearic acid, and antioxidant.
12. The preparation method according to claim 9, characterized in that: The injection molding comprises: The flexible adhesive is injection molded at an injection temperature of 160° C. to 210° C. to obtain a green embryo.
13. The preparation method according to claim 12, characterized in that: The degreasing comprises: The injection molded green body is subjected to acid catalyst degreasing or solvent degreasing to remove the binder.
14. The preparation method according to claim 13, characterized in that: The degreasing temperature is between 120-130° C., and the catalytic degreasing time is 1-10 hours.
15. The preparation method according to claim 13 or 14, characterized in that: The catalytic medium is nitric acid or oxalic acid.
16. The preparation method according to claim 13, characterized in that: The sintering comprises: sintering the degreased green embryo in a vacuum atmosphere, the sintering temperature is 1200-1400° C., the heat preservation time is 1-6 hours, and a cooked embryo is obtained.
17. The preparation method according to claim 16, characterized in that: The heat treatment comprises: Solution treatment: the sintered embryo is kept at a temperature of 1000-1100°C for 1-1.5 hours, and then the embryo is quickly cooled using high-pressure inert gas; wherein the pressure of the inert gas is >8 bar; Cryogenic treatment: the cooked embryo that has undergone the solution treatment is cryogenically cooled and kept warm for more than 1 hour at a temperature below -180°C; Aging treatment: The deep-cold treated cooked embryo is kept at a temperature of 500-550° C. for 4-5 hours.
18. A rotating shaft assembly, characterized in that: The shaft assembly is made of the alloy steel material as described in any one of claims 1-5.
19. An electronic device, characterized in that: include: The housing comprises a first frame and a second frame; A folding screen, the folding screen comprising a first screen and a second screen, the first screen being arranged on the first frame, and the second screen being arranged on the second frame; A shaft assembly is disposed in the shell, and two ends of the shaft assembly are respectively connected to the first frame and the second frame, and is used to enable the first screen and the second screen to be rotatably connected. The shaft assembly is the shaft assembly described in claim 18.
Citation Information
Patent Citations
Corrosion-resistant steel powder, ultrahigh-strength steel feed and corrosion-resistant steel complex part preparation process
CN111992704A
2600MPa-grade ultrahigh-strength steel and preparation method thereof
CN113604753A
Steel material, steel structural part, preparation method of steel structural part and terminal
CN114908300A
Titanium-free, nickel-containing maraging steel die block article and method of manufacture
US5482531A