A porous spherical silver powder material and its preparation method

Porous spherical silver powder was prepared by mixing alkanolamine and reducing agent solution under ultrasonic conditions, which solved the problems of incomplete reaction and soft agglomeration of silver powder, and achieved silver powder with high dispersibility and shape consistency, thus improving sintering activity and electrical conductivity.

CN117718470BActive Publication Date: 2026-11-17福建富轩科技有限公司
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410104196.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-25
Publication Date
2026-11-17
Estimated Expiration
2044-01-25

AI Technical Summary

Technical Problem

In existing technologies, the silver powder reaction is incomplete, the preparation steps are cumbersome, and soft agglomeration is prone to occur, making it difficult to achieve uniform shape and particle size of porous silver powder.

Method used

A solution of alcoholic amine and a solution of strong reducing agent are mixed under ultrasonic conditions. The temperature is controlled and the mixture is ultrasonically stirred to generate bubbles that serve as templates. The alcoholic amine decomposes and reduces silver ions at high temperature to prepare porous spherical silver powder, thus avoiding the need for additional pH adjusters.

Benefits of technology

High dispersion and shape consistency of silver particles were achieved, and monodisperse spherical porous silver powder was prepared, which improved sintering activity and electrical conductivity.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention relates to the field of silver powder preparation technology, and more particularly to a porous spherical silver powder material and its preparation method, comprising: S1, preparing a solution; S2, placing the beaker containing the reaction solution prepared in step S1 into an ultrasonic cleaner for ultrasonic cleaning while maintaining mechanical stirring for 0.5-1 h; S3, heating the reaction solution obtained in step S2 to between 40℃ and 90℃ under ultrasonic conditions while maintaining mechanical stirring for 0.5-1 h; S4, centrifuging and washing the suspension obtained in step S3, and then drying it to obtain silver powder. This invention uses ultrasonic conditions to ensure excellent dispersion of the prepared silver particles, generating bubbles to serve as templates for porous silver powder and ensuring sufficient nucleation, while simultaneously initiating the decomposition and reduction of alkanolamines to prepare monodisperse spherical porous silver powder; the addition of an alkanolamine solution to the reaction solution eliminates the need for additional regulators, and the alkanolamine begins to react after the temperature conditions are reached, further ensuring complete reduction of silver ions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of silver powder preparation technology, specifically to a porous spherical silver powder material and its preparation method. Background Technology

[0002] Silver powder is the conductive phase in front-side silver paste, accounting for 80-92% of the paste's mass. It significantly influences the paste's rheological properties and printability, and plays a decisive role in the photoelectric conversion efficiency of solar cells. Front-side silver paste plays a crucial role in solar cells, and silver powder is the dominant component within it. The electronics industry requires silver powder with high purity and good dispersibility. Currently, the market mainly relies on imported silver powder from DOWA in Japan. DOWA is the world's largest supplier of silver powder for solar conductive pastes, offering products with small particle size ranges, good surface organic coating, and excellent dispersibility. Furthermore, its porous silver powder has large pore sizes, superior specific surface area, and higher sintering activity. Currently, the main particle size distribution of silver powder used in front-side silver paste is 1-2 μm, which is prone to soft agglomeration. Solar front-side silver paste has even stricter requirements for the shape and particle size of the silver powder. Researching and developing porous silver powder with highly consistent shape and highly uniform particle size is crucial for improving the performance of solar front-side silver paste.

[0003] The patent with publication number CN106041123A uses a nanobubble generator to introduce a large number of nanobubbles. Using the nanobubbles as carriers, silver nitrate and gum arabic powder are adsorbed on their surface. Ascorbic acid solution is then added to prepare a highly active hollow silver powder for positive silver in solar cells. Before the reaction, nanobubbles are introduced using tools. The process is cumbersome and cannot guarantee that the silver powder generated in the subsequent reaction will be hollow.

[0004] The patent with publication number CN117047121A describes the preparation of silver powder under alkaline conditions. It utilizes two reducing agents to ensure the complete reaction of silver ions, resulting in mixed silver powder with particles of varying sizes. A silver solution is prepared by adding sodium hydroxide and ammonia. After washing, the silver powder is filtered and dispersed in solutions of different solvents. However, it is difficult to control the amount and timing of the pH adjuster and the second reducing agent. The surface treatment of the product is complex and difficult to achieve industrial production.

[0005] Therefore, the above technical solution has the following drawbacks:

[0006] 1. Incomplete reaction of silver powder. A reducing agent is prone to incomplete reaction under normal reaction conditions. This invention uses ultrasonic conditions to facilitate the nucleation of silver particles, and the addition of an alcoholic amine compound, which reacts upon reaching the designated temperature, further ensures the complete reduction of silver ions in the solution.

[0007] 2. The preparation of porous silver powder involves cumbersome steps. The solution preparation is simple and easy to operate. This invention involves reacting under ultrasonic conditions, which helps generate bubbles. No additional pH adjuster is needed; an alcoholic amine solution is used instead. All steps are completed in a single container, simplifying the operation.

[0008] 3. To address the issue of soft agglomeration that easily occurs in silver powder, the silver particles are evenly dispersed during the growth process under ultrasonic conditions, eliminating the need for additional treatment during the cleaning process and helping to ensure high consistency in shape and high uniformity in particle size during the growth process.

[0009] Therefore, a porous spherical silver powder material and its preparation method are proposed to address the above problems. Summary of the Invention

[0010] The purpose of this invention is to provide a porous spherical silver powder material and its preparation method, so as to solve the problems mentioned in the background art.

[0011] To achieve the above objectives, the present invention provides the following technical solution:

[0012] A porous spherical silver powder material includes silver powder, wherein each particle of the silver powder is composed of primary silver particles at the nanometer and submicrometer scale.

[0013] A porous spherical silver powder material and its preparation method, comprising the following steps:

[0014] S1. Prepare silver amine solution and strong reducing agent solution containing alcohol amine respectively;

[0015] S2. Under conditions of 0-20℃, rapidly mix the silver amine solution and strong reducing agent solution prepared in S1, and stir vigorously for 0.5-1h.

[0016] S3. Continue mechanical stirring of the reaction solution and introduce ultrasound, while raising the temperature of the reaction solution to 40-90℃ and maintaining the temperature while ultrasonically stirring for 1-12 hours.

[0017] S4. Separate and wash the precipitate in the suspension obtained in step S3, and dry it at a temperature of 40-200℃ to obtain silver powder.

[0018] Preferably, the silver source in the silver amine solution is any one or more of silver nitrate, silver oxide, silver chloride, silver carbonate, silver sulfate, silver fluoride, silver perchlorate, silver chlorate, and silver bicarbonate, with a molar concentration of silver between 0.001 and 1 mol / L; the amine is any one or more of ammonia, alkanolamine, and fatty acid ammonium, wherein the molar ratio of ammonium or amine group to silver is between 1:2 and 8:1.

[0019] Preferably, the amine compound is any one or more of ethanolamine, diethanolamine, triethanolamine, methyldiethanolamine, 3-propanolamine, isopropanolamine, diisopropanolamine, triisopropanolamine, N,N-dimethylethanolamine, and N,N-diethylethanolamine, wherein the molar ratio of the amine group to silver is between 1:2 and 8:1.

[0020] Preferably, the reducing agent is any one or more of formaldehyde, ascorbic acid, sodium borohydride, hydrazine hydrate, glucose, hydroquinone, ferrous sulfate, sodium citrate, acetaldehyde, propionaldehyde, glyoxal, formic acid, potassium formate, sodium formate, ammonium formate, ethyl formate, propyl formate, unsaturated alcohol, sodium hypophosphite, and sodium borohydride, wherein the molar ratio of the reducing agent to silver is between 1:1 and 8:1.

[0021] Preferably, the dispersant is any one or more of the following: polyvinylpyrrolidone, gum arabic, hexadecyl ammonium bromide, sodium dodecyl sulfate, oleic acid, methylcellulose, polyacrylic acid, trisodium citrate, gelatin, polyethylene glycol, benzotriazole, polyvinyl alcohol, polyvinyl butyral, polyacrylic acid, fatty alcohol polyoxyethylene ether, (2-hydroxy-3-alkoxy)propyl-carboxymethyl chitosan, polyoxyethylene stearate, dimethylaminomethacrylamide, acrylic acid copolymer, oleamide, polyacrylamide, sodium methylene dimethylnaphthalene sulfonate, polycarboxylic acid ammonium salt, sodium polycarboxylic acid salt type, sodium lignosulfonate, and 2-acrylamido-2-methylpropanesulfonic acid.

[0022] Preferably, in step S2, the ultrasonic frequency range is between 20-1200KHz, and the mechanical stirring speed is controlled between 50-600rpm.

[0023] Preferably, in step S1, the proportion of the silver source solution is controlled within the selected silver source solubility range; the amount of dispersant added is 0.01%-5% of the theoretical mass of synthesized silver powder.

[0024] Preferably, in step S4, the cleaning process involves repeatedly washing with anhydrous ethanol, acetone, and deionized water 2-10 times.

[0025] Compared with the prior art, the beneficial effects of the present invention are:

[0026] 1. The present invention conducts the reaction under ultrasonic conditions, which fully ensures the good dispersion of the prepared silver particles, generates bubbles to serve as templates for porous silver powder, and ensures sufficient nucleation. At the same time, it initiates the decomposition and reduction of alkanolamines to prepare monodisperse spherical porous silver powder.

[0027] 2. Add an alcoholic amine solution to the reaction solution. No additional regulator is needed. The alcoholic amine will start to react after the temperature conditions are met, which further ensures the complete reduction of silver ions. Detailed Implementation

[0028] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0029] This invention provides a technical solution:

[0030] A porous spherical silver powder material and its preparation method, comprising the following steps:

[0031] S1. Prepare silver amine solution and strong reducing agent solution containing alcohol amine respectively;

[0032] S2. Under conditions of 0-20℃, rapidly mix the silver amine solution and strong reducing agent solution prepared in S1, and stir vigorously for 0.5-1h.

[0033] S3. Continue mechanical stirring of the reaction solution and introduce ultrasound, while raising the temperature of the reaction solution to 40-90℃ and maintaining the temperature while ultrasonically stirring for 1-12 hours.

[0034] S4. Separate and wash the precipitate in the suspension obtained in step S3, and dry it at a temperature of 40-200℃ to obtain silver powder.

[0035] In this embodiment, the silver source in the silver amine solution is any one or more of silver nitrate, silver oxide, silver chloride, silver carbonate, silver sulfate, silver fluoride, silver perchlorate, silver chlorate, and silver bicarbonate, with a molar concentration of silver between 0.001 and 1 mol / L; the amine is any one or more of ammonia, alkanolamine, and fatty acid ammonium, wherein the molar ratio of ammonium or amine group to silver is between 1:2 and 8:1.

[0036] In this embodiment, the amine compound is any one or more of ethanolamine, diethanolamine, triethanolamine, methyldiethanolamine, 3-propanolamine, isopropanolamine, diisopropanolamine, triisopropanolamine, N,N-dimethylethanolamine, and N,N-diethylethanolamine, wherein the molar ratio of the amine group to silver is between 1:2 and 8:1.

[0037] In this embodiment, the reducing agent is any one or more of formaldehyde, ascorbic acid, sodium borohydride, hydrazine hydrate, glucose, hydroquinone, ferrous sulfate, sodium citrate, acetaldehyde, propionaldehyde, glyoxal, formic acid, potassium formate, sodium formate, ammonium formate, ethyl formate, propyl formate, unsaturated alcohol, sodium hypophosphite, and sodium borohydride, wherein the molar ratio of the reducing agent to silver is between 1:1 and 8:1.

[0038] In this embodiment, the dispersant is any one or more of the following: polyvinylpyrrolidone, gum arabic, hexadecyl ammonium bromide, sodium dodecyl sulfate, oleic acid, methylcellulose, polyacrylic acid, trisodium citrate, gelatin, polyethylene glycol, benzotriazole, polyvinyl alcohol, polyvinyl butyral, polyacrylic acid, fatty alcohol polyoxyethylene ether, (2-hydroxy-3-alkoxy)propyl-carboxymethyl chitosan, polyoxyethylene stearate, dimethylaminomethacrylamide, acrylic acid copolymer, oleamide, polyacrylamide, sodium methylene dimethylnaphthalene sulfonate, polycarboxylic acid ammonium salt, sodium polycarboxylic acid salt type, sodium lignosulfonate, and 2-acrylamido-2-methylpropanesulfonic acid.

[0039] In this implementation, in step S2, the ultrasonic frequency range is between 20-1200KHz, and the mechanical stirring speed is controlled between 50-600rpm.

[0040] In this embodiment, the proportion of the silver source solution in step S1 is controlled within the selected silver source solubility range; the amount of dispersant added is 0.01%-5% of the theoretically synthesized silver powder mass.

[0041] In this implementation, in step S4, anhydrous ethanol, acetone, and deionized water are used for repeated cleaning 2-10 times.

[0042] The present invention will be further described below with reference to specific embodiments;

[0043] Example 1

[0044] A porous spherical silver powder material and its preparation method, comprising the following steps:

[0045] S1. Prepare silver amine solution and strong reducing agent solution containing alcohol amine respectively;

[0046] S2. Under 20℃ conditions, the silver amine solution and strong reducing agent solution prepared in S1 are rapidly mixed and stirred vigorously for 6 hours to obtain a large number of fine seed crystals.

[0047] S3. Continue mechanical stirring of the reaction solution and introduce ultrasound. At the same time, raise the temperature of the reaction solution to 50°C and keep it at this temperature for 6 hours of ultrasonic stirring. On the one hand, the alcohol amine decomposes into a reducing agent, causing the fine seed crystals to agglomerate into large particles. On the other hand, the bubbles generated by ultrasound become the hollow cores of the agglomerates.

[0048] S4. Separate and wash the precipitate from the suspension obtained in step S3, and dry it at 100°C to obtain silver powder.

[0049] The silver particles prepared according to this method are spherical or near-spherical in shape, without obvious agglomeration, with a tap density ≥4.2g / cm3, a particle size distribution D50 of about 2.1μm, and a porous internal structure. The sintering activity is higher than that of solid silver powder, and the electrical conductivity after sintering is ≥1.78×107S / m.

[0050] Example 2

[0051] A porous spherical silver powder material and its preparation method, comprising the following steps:

[0052] S1. Prepare silver amine solution and strong reducing agent solution containing alcohol amine respectively;

[0053] S2. Under 10℃ conditions, the silver amine solution and strong reducing agent solution prepared in S1 are rapidly mixed and stirred vigorously for 6 hours to obtain a large number of fine seed crystals.

[0054] S3. Continue mechanical stirring of the reaction solution and introduce ultrasound. At the same time, raise the temperature of the reaction solution to 40°C and keep it at this temperature for 4 hours of ultrasonic stirring. On the one hand, the alcohol amine decomposes into a reducing agent, causing the fine seed crystals to agglomerate into large particles. On the other hand, the bubbles generated by ultrasound become the hollow cores of the agglomerates.

[0055] S4. Separate and wash the precipitate from the suspension obtained in step S3, and dry it at 150°C to obtain silver powder.

[0056] The silver particles prepared according to this method are spherical or near-spherical in shape, without obvious agglomeration, with a tap density ≥4.2g / cm3, a particle size distribution D50 of about 1.6μm, and a porous internal structure. The sintering activity is higher than that of solid silver powder, and the electrical conductivity after sintering is ≥1.78×107S / m.

[0057] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A method for preparing porous spherical silver powder material, characterized in that: Includes the following steps: S1. Prepare a silver amine solution and a strong reducing agent solution containing an alkanolamine, respectively. The silver source in the silver amine solution is any one or more of silver nitrate, silver oxide, silver chloride, silver carbonate, silver sulfate, silver fluoride, silver perchlorate, silver chlorate, and silver bicarbonate, with a molar concentration of silver between 0.001 and 1 mol / L. The amine is any one or more of ammonia, alkanolamine, and fatty acid ammonium, wherein the molar ratio of ammonium or amine group to silver is between 1:2 and 8:

1. The alkanolamine compound is any one or more of ethanolamine, diethanolamine, triethanolamine, methyldiethanolamine, 3-propanolamine, isopropanolamine, diisopropanolamine, triisopropanolamine, N,N-dimethylethanolamine, and N,N-diethylethanolamine. The reducing agent is any one or more of formaldehyde, ascorbic acid, hydrazine hydrate, glucose, hydroquinone, ferrous sulfate, sodium citrate, acetaldehyde, propionaldehyde, glyoxal, formic acid, potassium formate, sodium formate, ammonium formate, ethyl formate, propyl formate, unsaturated alcohol, sodium hypophosphite, and sodium borohydride, wherein the molar ratio of the reducing agent to silver is between 1:1 and 8:1; The proportion of the silver source solution is controlled within the selected silver source solubility range; the amount of dispersant added is 0.01%-5% of the theoretical mass of synthesized silver powder; S2. Under conditions of 0-20℃, rapidly mix the silver amine solution and strong reducing agent solution prepared in S1, and stir vigorously for 0.5-1h. S3. Continue mechanical stirring of the reaction solution and introduce ultrasound. At the same time, increase the temperature of the reaction solution to 40-90℃ and keep it warm while ultrasonic stirring for 1-12 hours. The ultrasonic frequency range is between 20-1200KHz, and the mechanical stirring speed is controlled between 50-600rpm. S4. Separate and wash the precipitate in the suspension obtained in step S3, and dry it at a temperature of 40-200℃ to obtain silver powder.

2. The method for preparing porous spherical silver powder material according to claim 1, characterized in that: The dispersant is any one or more of the following: polyvinylpyrrolidone, gum arabic, hexadecyl ammonium bromide, sodium dodecyl sulfate, oleic acid, methylcellulose, polyacrylic acid, trisodium citrate, gelatin, polyethylene glycol, benzotriazole, polyvinyl alcohol, polyvinyl butyral, fatty alcohol polyoxyethylene ether, (2-hydroxy-3-alkoxy)propyl-carboxymethyl chitosan, polyoxyethylene stearate, dimethylaminomethacrylamide, acrylic acid copolymer, oleamide, polyacrylamide, sodium methylene dimethylnaphthalene sulfonate, ammonium polycarboxylate, sodium polycarboxylate, sodium lignosulfonate, and 2-acrylamido-2-methylpropanesulfonic acid.

3. A porous spherical silver powder material, wherein the porous spherical silver powder material is prepared by the method for preparing porous spherical silver powder material according to any one of claims 1-2.

Citation Information

Patent Citations

  • High-activity hollow silver powder for front silver of solar cell and preparing method for high-activity hollow silver powder

    CN106041123A

  • Preparation method of silver powder

    CN117047121A

  • Method of preparing metal stephanoporate spherical aluminum powder

    CN101318225A

  • Ultrasonic-assisted silver powder preparation method, prepared silver powder and application

    CN116251961A