A sodium ion battery positive electrode composite material and its preparation method and application

By ball milling and sintering ferrous salt, sodium salt, sulfur source and MIL type MOF materials under reduced atmosphere, Na2Fe2-xMx(SO4)3/C positive electrode composite material was prepared, and the problem of insufficient performance of sodium ion battery material was solved, and the problem of High specific capacity and long cycle life, suitable for large-scale energy storage applications.

CN117747786BActive Publication Date: 2024-11-12HUBEI HONGRUN HIGH-TECH NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311755365.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-18
Publication Date
2024-11-12
Estimated Expiration
2043-12-18

Smart Images

  • Figure CN117747786B_ABST
    Figure CN117747786B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing a sodium ion battery positive electrode composite material, comprising the following steps: A) ball milling ferrous salt, sodium salt, sulfur source, carbon source and MIL type MOF material under reducing atmosphere to obtain a mixture; B) sintering the mixture under reducing atmosphere to obtain Na2Fe 2‑x M x (SO4)3 / C positive electrode composite material, wherein M is selected from Al or Cr, and x is in the range of 0.01 to 0.2. The preparation method of the positive electrode composite material for sodium ion batteries provided by the present invention is simple, and heterovalent metal doping and coating of mesoporous nano-network structure carbon materials are achieved in one step, so as to obtain a positive electrode composite material with less impurities, high specific capacity and long cycle life. The raw materials are simple and easy to obtain, the preparation process is simple to operate, the experimental reproducibility is good, and it is easy to realize industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of sodium ion batteries, and in particular relates to a sodium ion battery positive electrode composite material and a preparation method and application thereof. Background Art

[0002] Against the backdrop of increasing demand for energy, electrochemical energy storage is an important technology among all energy storage methods. Among electrochemical energy storage technologies, lithium-ion batteries are efficient, clean, and recyclable energy sources. However, due to the limited reserves of lithium, uneven distribution, and difficulty in mining, the raw materials for lithium-ion batteries are expensive and have large price fluctuations. Therefore, it is very necessary to develop new secondary batteries to achieve large-scale energy storage. Sodium and lithium are in the same main group of the periodic table and have similar physical and chemical properties. Compared with lithium resources, sodium is abundant in the earth's crust, evenly distributed, and inexpensive. Therefore, sodium-ion batteries are most likely to be used in large-scale power storage and low-speed transportation in the future.

[0003] The main characteristics of polyanionic compounds in sodium positive electrodes are high electrode potential, good long cycle life and strong framework structure. The various crystal structures of polyanionic compounds provide open channels for sodium ions. Due to the abundant reserves and low price of iron, iron-based polyanionic materials have great advantages in the competition for large-scale production, economical and environmentally friendly sodium ion battery positive electrode materials. 2+ / Fe 3+ The redox couple exhibits multiple discharge platforms in different types of polyanion materials. In addition, most iron-based polyanion materials have a high operating voltage of more than 3V, which shows great application prospects in industrial production. + The volume change is small during the intercalation and deintercalation process, and the activation energy of ion diffusion is low. It has the advantages of being able to regulate the potential by adjusting the environment in which the polyanion is located. In addition, sulfate has a strong inductive effect and high-potential materials are easy to obtain. It is a positive electrode material with great development potential.

[0004] Sodium ferrous sulfate (Na2Fe2(SO4)3) is a positive electrode material for iron-based sulfate polyanion sodium ion batteries. It has the advantages of high operating voltage, abundant raw materials, low cost, and environmental friendliness. However, there are still some problems that need to be solved, such as poor electronic conductivity, easy water absorption by sulfate, and easy oxidation of ferrous ions. Carbon coating, nano-sizing, and cation doping of Na2Fe2(SO4)3 are common methods to improve its performance, but ordinary synthesis methods easily lead to high impurity content in the synthesized materials, reduce the content of active materials, and reduce the specific capacity of the materials. Summary of the invention

[0005] In view of this, the technical problem to be solved by the present invention is to provide a sodium ion battery positive electrode composite material and a preparation method thereof. The preparation method of the sodium ion battery positive electrode composite material provided by the present invention is simple, has good repeatability, and is environmentally friendly. The prepared positive electrode composite material has few impurities, high specific capacity, and long cycle life.

[0006] The present invention provides a method for preparing a sodium ion battery positive electrode composite material, comprising the following steps:

[0007] A) ball milling ferrous salt, sodium salt, sulfur source, carbon source and MIL-based MOF material under reducing atmosphere to obtain a mixture;

[0008] B) sintering the mixture under reducing atmosphere to obtain Na2Fe 2-x M x (SO4)3 / C positive electrode composite material, wherein M is selected from Al or Cr, and x ranges from 0.01 to 0.2.

[0009] Preferably, the MIL-type MOF material is selected from at least one of MIL-53 (Al), MIL-53 (Cr), MIL-100 (Al) or MIL-100 (Cr).

[0010] Preferably, the ferrous salt includes any one or more of ferrous sulfate, ferrous chloride, ferrous carbonate, and ferrous oxalate; preferably ferrous sulfate; and / or

[0011] The sodium salt includes any one or more of sodium carbonate, sodium bicarbonate, sodium hydroxide, sodium citric acid, sodium ethoxide, sodium sulfate, sodium nitrate, sodium acetate, and sodium bisulfate; and / or

[0012] The sulfur source includes any one or more of ferrous sulfate, sodium sulfate, potassium sulfate, and calcium sulfate; and / or

[0013] The carbon source is selected from any one or more of glucose, sucrose, fructose, cellulose, starch, and ascorbic acid; more preferably, ascorbic acid.

[0014] Preferably, the molar ratio of the ferrous ions in the ferrous salt to the sodium ions in the sodium salt is 1:0.5-1;

[0015] The molar amount of the metal ions in the MIL-type MOF material is 0.5 to 10% of the molar amount of Fe in the ferrous salt;

[0016] The input amount of the carbon source is 5-15% of the mass of the positive electrode composite material.

[0017] Preferably, the ball milling step comprises:

[0018] Under reducing atmosphere conditions, ferrous salt, sodium salt, sulfur source, carbon source and MIL MOF material are mixed with acetone for ball milling; the ball-to-material ratio is 10-20:1, the reducing atmosphere is selected from argon-hydrogen mixed gas, the ball milling speed is 450-600rpm, and the ball milling time is 4-12h; and / or

[0019] The sintering step comprises:

[0020] 1~5℃min -1 The heating rate is 200-280℃ for 4-8h, then 1-5℃min -1 The heating rate is 300-400℃ and sintered for 10-24h.

[0021] The present invention also provides a sodium ion battery positive electrode composite material prepared by the above preparation method, wherein the sodium ion battery positive electrode composite material is Na2Fe 2-x M x (SO4)3 / C positive electrode composite material, wherein M is selected from Al or Cr, and x ranges from 0.01 to 0.2.

[0022] Preferably, the Na2Fe 2-x M x The first-week charging capacity of the (SO4)3 / C positive electrode composite material ranges from 86.8 to 96.2 mAh / g, the coulombic efficiency is greater than 99%, and the capacity retention rate after 100 weeks of constant current charge and discharge at a current density of 0.5C is ≥88%.

[0023] Preferably, the Na2Fe 2-x M x The crystal form of the (SO4)3 / C positive electrode composite material is sodium phosphate type; the particle size is 400-1000nm.

[0024] The present invention also provides a positive electrode plate, comprising the sodium ion battery positive electrode composite material prepared by the above preparation method, or comprising the above sodium ion battery positive electrode composite material.

[0025] The present invention also provides a secondary battery, comprising the above-mentioned positive electrode plate.

[0026] The present invention also provides an electrical device, comprising the secondary battery.

[0027] Compared with the prior art, the present invention provides a method for preparing a sodium ion battery positive electrode composite material, comprising the following steps: A) ball milling ferrous salt, sodium salt, sulfur source, carbon source and MIL type MOF material under reducing atmosphere to obtain a mixture; B) sintering the mixture under reducing atmosphere to obtain Na2Fe 2-x M x(SO4)3 / C positive electrode composite material. The preparation method of the positive electrode composite material for sodium ion batteries provided by the present invention is simple, and heterovalent metal doping and coating of mesoporous nano-network structure carbon materials are achieved in one step, so as to obtain a positive electrode composite material with less impurities, high specific capacity and long cycle life. The raw materials are simple and easy to obtain, the preparation process is simple to operate, the experimental reproducibility is good, and it is easy to realize industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 X-ray diffraction (XRD) patterns of the sodium ferrous sulfate positive electrode composite materials prepared in Example 1, Example 2 and Comparative Example 2.

[0029] Figure 2 This is a scanning electron microscope (SEM) image of the sodium ferrous sulfate positive electrode composite material prepared in Example 1.

[0030] Figure 3 This is a cycle life diagram of a CR2032 button battery assembled with the sodium ferrous sulfate positive electrode composite material prepared in Example 1.

[0031] Figure 4 The charge and discharge curves of the CR2032 button battery assembled with the sodium ferrous sulfate positive electrode composite material prepared in Example 1 at the 2nd, 10th, 50th and 100th cycles are shown.

[0032] Figure 5 This is a rate performance diagram of a CR2032 button battery assembled with the sodium ferrous sulfate positive electrode composite material prepared in Example 1.

[0033] Figure 6 This is a cyclic voltammetry test diagram of a CR2032 button battery assembled with the sodium ferrous sulfate positive electrode composite material prepared in Example 1. DETAILED DESCRIPTION

[0034] The present invention provides a method for preparing a sodium ion battery positive electrode composite material, comprising the following steps:

[0035] A) ball milling ferrous salt, sodium salt, sulfur source, carbon source and MIL-based MOF material under reducing atmosphere to obtain a mixture;

[0036] B) sintering the mixture under reducing atmosphere to obtain Na2Fe 2-x M x (SO4)3 / C positive electrode composite material, wherein M is selected from Al or Cr, and x ranges from 0.01 to 0.2.

[0037] The preparation method of the sodium ion battery positive electrode composite material provided by the present invention is a simple process, good repeatability, and environmentally friendly preparation method. The method mainly uses MIL-type metal organic framework (MOF) materials as templates to synthesize metal-doped and carbon-coated modified Na2Fe 2-x M x (SO4)3 / C cathode material. During the heat treatment, the metal organic framework is pyrolyzed to form a mesoporous nano-network carbon material and doped with Na2Fe 2-x M x Heterovalent metal ions at the iron position in (SO4)3 / C. During the synthesis process, MOF materials were used to achieve joint modification of metal ion doping and carbon coating.

[0038] The present invention firstly treats the hydrate of salt in the raw material to remove the crystal water. The present invention has no special limitation on the treatment method, and any method known to those skilled in the art can be used. For example, FeSO4·7H2O is sintered under the protection of argon-hydrogen mixed gas to obtain FeSO4.

[0039] Then, ferrous salt, sodium salt, sulfur source, carbon source and MIL-based MOF material are mixed.

[0040] Wherein, the ferrous salt includes any one or more of ferrous sulfate, ferrous chloride, ferrous carbonate, and ferrous oxalate; preferably ferrous sulfate;

[0041] The sodium salt includes any one or more of sodium carbonate, sodium bicarbonate, sodium hydroxide, sodium lemon, sodium ethoxide, sodium sulfate, sodium nitrate, sodium acetate, and sodium bisulfate, preferably sodium sulfate;

[0042] When the ferrous salt is not ferrous sulfate and / or the sodium salt is not sodium sulfate, a sulfur source needs to be added to the reaction system. The sulfur source includes any one or more of ferrous sulfate, sodium sulfate, ammonium sulfate, and sodium bisulfate.

[0043] The molar ratio of the ferrous ions in the ferrous salt to the sodium ions in the sodium salt is 1:1-2, preferably 1:1, 1:1.2, 1:1.4, 1:1.6, 1:1.8, 1:2, or any value between 1:1 and 2; more preferably 1:1.2.

[0044] The molar amount of the total sulfur source is 1.5 to 1.8 times the molar amount of ferrous ions.

[0045] The carbon source is selected from any one or more of glucose, sucrose, fructose, cellulose, starch, and ascorbic acid; more preferably, ascorbic acid, which has stronger reducing properties than other commonly used carbon sources, and can better reduce trivalent iron during the calcination process, and can also be used as a coating carbon to enhance the conductivity of the composite material after calcination. The input amount of the carbon source is 5% to 15% of the mass of the positive electrode composite material, preferably 5%, 10%, 15%, or any value between 5% and 15%.

[0046] The MIL-type MOF material is selected from one of MIL-53 (Al), MIL-53 (Cr), MIL-100 (Al), and MIL-100 (Cr).

[0047] The present invention has no particular restrictions on the source of the MIL-type MOF material, which can be a commercially available product or prepared by itself. In the present invention, the MIL-53 (Al) or MIL-53 (Cr) is prepared according to the following method:

[0048] Dissolving terephthalic acid and aluminum salt or chromium salt in water to obtain a mixed solution;

[0049] The mixed solution is subjected to a hydrothermal reaction, and after solid-liquid separation of the obtained reaction solution, the solid is washed and calcined to obtain MIL-53(Al) or MIL-53(Cr);

[0050] The MIL-100(Al) or MIL-100(Cr) is prepared according to the following method:

[0051] dissolving trimesic acid and aluminum salt or chromium salt in water to obtain a mixed solution;

[0052] The mixed solution is subjected to a hydrothermal reaction, and after the obtained reaction solution is solid-liquid separated, the solid is washed and then calcined to obtain MIL-100 (Al) or MIL-100 (Cr).

[0053] Wherein, the aluminum salt is selected from aluminum nitrate nonahydrate or aluminum chloride hexahydrate; the chromium salt is selected from chromium acetate, chromium nitrate nonahydrate or chromium chloride hexahydrate.

[0054] The molar amount of metal ions in the MIL MOF material is 0.5-10% of the molar amount of Fe in the ferrous salt, preferably 0.5%, 1%, 2%, 4%, 5%, 6%, 8%, 10%, or any value between 2% and 10%.

[0055] MIL MOF materials are aromatic carbon sources. Compared with compound carbon sources such as sugars and esters that need to be cracked to form four carbon groups and then aromatized during heating, they are easier to aromatize, resulting in a higher degree of carbonization at lower temperatures. Therefore, the conductivity of the mesoporous carbon coating is slightly higher than that of carbon coatings such as glucose and sucrose. The mesoporous carbon coating improves the electronic conductivity and the wettability of the electrolyte to the positive electrode material. In addition, the trivalent metal M replaces the divalent iron element. In order to maintain the charge balance in the crystal structure, Na2Fe 2-x M x Some vacancies are created in the (SO4)3 / C crystal structure, which increases the transmission rate of sodium ions in the crystal structure.

[0056] In the present invention, the ferrous salt, sodium salt, sulfur source, carbon source and MIL MOF material are preferably mixed by ball milling, and an appropriate amount of acetone is added during mixing. The ball-to-material ratio is 10 to 20:1, preferably 10:1, 15:1, 20:1, or any value between 10 and 20:1. The ball milling is carried out under reducing atmosphere conditions to obtain a mixture.

[0057] The reducing atmosphere is selected from argon-hydrogen mixed gas. The ball milling speed is 450-600 rpm, and the ball milling time is 4-12 hours.

[0058] Then, the mixture is dried. The present invention has no particular limitation on the drying method, and any drying method known to those skilled in the art may be used.

[0059] Finally, the dried mixture is sintered to obtain Na2Fe 2-x M x (SO4)3 / C positive electrode composite material.

[0060] Wherein, the sintering is carried out under reducing atmosphere conditions, and the reducing atmosphere is selected from argon-hydrogen mixed gas.

[0061] The sintering procedure is:

[0062] 1~5℃min -1 The heating rate is 200-280℃ for 4-8h, then 1-5℃min -1 The heating rate is 300-400℃ and sintered for 10-24h.

[0063] In some specific embodiments of the present invention, the sintering procedure is:

[0064] At 2℃min -1 Heating rate: pre-sinter at 200℃ for 6h, then at 2℃min -1 Heating rate: sintering at 400℃ for 10 to 24 hours.

[0065] The present invention also provides a sodium ion battery positive electrode composite material prepared by the above preparation method, wherein the sodium ion battery positive electrode composite material is Na2Fe 2-x M x (SO4)3 / C positive electrode composite material, wherein M is selected from Al or Cr, x ranges from 0.01 to 0.2, and the doping amount of the metal ion M is preferably 0.12.

[0066] The Na2Fe 2-x M x The first-week charging capacity of the (SO4)3 / C positive electrode composite material ranges from 86.8 to 96.2 mAh / g, the coulombic efficiency is greater than 99%, and the capacity retention rate after 100 weeks of constant current charge and discharge at a current density of 0.5C is ≥88%.

[0067] In the present invention, the Na2Fe 2-x M x The crystal form of the (SO4)3 / C positive electrode composite material is sodium phosphate type; the particle size is 400-1000nm.

[0068] The present invention also provides a positive electrode plate, comprising the sodium ion battery positive electrode composite material prepared by the above preparation method, or comprising the above sodium ion battery positive electrode composite material.

[0069] The present invention also provides a sodium ion battery, comprising the above-mentioned sodium ion battery positive electrode composite material.

[0070] The present invention also provides a secondary battery, comprising the above-mentioned positive electrode plate.

[0071] The present invention also provides an electrical device, comprising the secondary battery.

[0072] The present invention has the following beneficial effects:

[0073] (1) The present invention provides a one-step method for preparing low-cost, long-cycle Na2Fe 2-x M x The method of preparing (SO4)3 / C cathode composite material, through a simple ball milling method, strictly controlling the atmosphere during the reaction, regulating the sintering temperature and time, and adding an appropriate amount of MIL-type MOF material, can achieve heterovalent metal doping and coating of mesoporous nano-network structure carbon materials in one step, thereby obtaining a cathode composite material with less impurities, high specific capacity and long cycle life. The raw materials are simple and easy to obtain, the preparation process is simple to operate, the experimental reproducibility is good, and it is easy to realize industrial production;

[0074] (2) The metal organic framework used in the present invention is pyrolyzed to form a mesoporous nano-network structure carbon material and doped with Na2Fe 2-x M x(SO4)3 / C is an alivalent metal element in the iron position. During the synthesis process, MOF materials were used to achieve metal ion doping and carbon coating. MIL MOF materials are aromatic carbon sources, which are easier to aromatize and have a higher degree of carbonization at lower temperatures. The mesoporous carbon coating layer improves the electronic conductivity and the wettability of the electrolyte to the positive electrode material. In addition, the trivalent metal element replaces the divalent iron element. In order to maintain the charge balance in the crystal structure, Na2Fe 2-x M x Some vacancies are generated in the (SO4)3 / C crystal structure, which increases the transmission rate of sodium ions in the crystal structure, and some defects promote the formation of pure phase Na2Fe2(SO4)3;

[0075] (3) The sodium ferrous sulfate positive electrode material prepared by the method of the present invention has high specific capacity, high coulombic efficiency and high capacity retention rate, shows good cycle performance and rate performance, and the cost is greatly reduced compared with other positive electrode materials, which provides a bright prospect for the application of low-cost, high-safety secondary batteries in the field of large-scale energy storage.

[0076] In order to further understand the present invention, the sodium ion battery positive electrode composite material provided by the present invention, its preparation method and application are described below in conjunction with embodiments, and the protection scope of the present invention is not limited by the following embodiments.

[0077] In the following embodiments:

[0078] XRD test: The phase analysis of the sodium ferrous sulfate positive electrode material prepared in the example was carried out using a Rigaku-D / max-2550pc X-ray powder diffractometer from Hitachi, Japan, using Cu-k as the radiation source with a wavelength of A Ni filter was used, the tube current was 40 mA, the tube voltage was 40 KV, the scanning range was 10° to 90°, the scanning speed was 8° / min, and the step length was 0.02°; the identification of the phase and the crystal structure information were analyzed by JADE6.0 software;

[0079] SEM test: A scanning electron microscope S-4800 produced by HITACHI was used with an accelerating voltage of 20KV to observe the microstructure of the sodium ferrous sulfate cathode material prepared in the embodiment;

[0080] Assembly of CR2032 type button sodium ion battery: The sodium ferrous sulfate positive electrode material prepared in the embodiment, acetylene black and polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 75:15:10, and the mixed slurry is coated on aluminum foil, dried and cut into discs as the positive electrode; the metal sodium sheet is used as the negative electrode, and Whatman glass fiber (GF / D) is used as the diaphragm; the organic electrolyte is prepared by NaClO4, EC (ethylene carbonate), DEC (diethyl carbonate) and FEC (fluoroethylene carbonate), the NaClO4 concentration is 1.0 mol / L, the volume ratio of EC to DEC is 1:1, and the mass fraction of FEC in the electrolyte is 5%; CR2032 type button battery is assembled in an argon glove box.

[0081] Electrochemical performance test: The assembled CR2032 button batteries were tested using a Land battery tester produced by Wuhan Jinnuo Electronics Co., Ltd. The test voltage was 1.5V to 4.5V.

[0082] Synthesis of MIL-53(Al)MOF material: 4.3mmol of terephthalic acid and 8mmol of trivalent metal salt (aluminum nitrate nonahydrate) were mixed and dissolved in 80mL of deionized water. The solution was placed in a stainless steel reactor lined with polytetrafluoroethylene and heated at 220°C for 72 hours, and then cooled to room temperature. The white powder was centrifuged, washed with anhydrous ethanol and N,N dimethylformamide, respectively, and filtered to obtain a washed powder; the washed powder was washed three times. Finally, it was calcined in air at 300°C for 72 hours to remove the residual terephthalic acid and obtain the MIL-53(Al)MOF material.

[0083] Synthesis of MIL-53(Cr)MOF material: 4.3mmol of terephthalic acid and 8mmol of trivalent metal salt (chromium nitrate nonahydrate) were mixed and dissolved in 80mL of deionized water. The solution was placed in a stainless steel reactor lined with polytetrafluoroethylene and heated at 220℃ for 72 hours, and then cooled to room temperature. The white powder was centrifuged, washed with anhydrous ethanol and N,N dimethylformamide, respectively, and filtered to obtain a washed powder; the washed powder was washed three times. Finally, it was calcined in air at 300℃ for 72 hours to remove the residual terephthalic acid and obtain the MIL-53(Cr)MOF material.

[0084] Synthesis of MIL-100(Al)MOF material: 3mmol of trimethyl 1,3,5-benzene trihydroxy ester and 6mmol of trivalent metal salt (aluminum nitrate nonahydrate) were mixed and dissolved in 80mL of deionized water, and nitric acid was added to adjust the pH of the solution to between 0.5 and 0.7. The solution was placed in a stainless steel reactor lined with polytetrafluoroethylene and heated at 210°C for 72 hours, and then cooled to room temperature. The yellow powder was centrifuged, washed with anhydrous ethanol and N,N dimethylformamide, and filtered to obtain a washed powder; the washed powder was washed three times. Finally, it was calcined in air at 300°C for 72 hours to remove residual terephthalic acid and obtain MIL-100(Al)MOF material.

[0085] Synthesis of MIL-100(Cr)MOF material: 4mmol of trimesic acid and 8mmol of trivalent metal salt (chromium chloride hexahydrate) were mixed and dissolved in 80mL of deionized water, and nitric acid was added to adjust the pH of the solution to between 0.5 and 0.7. The solution was placed in a stainless steel reactor lined with polytetrafluoroethylene and heated at 210°C for 72 hours, and then cooled to room temperature. The white powder was centrifuged, washed with anhydrous ethanol and N,N dimethylformamide, and filtered to obtain a washed powder; the washed powder was washed three times. Finally, it was calcined in air at 300°C for 72 hours to remove residual terephthalic acid and obtain MIL-100(Cr)MOF material.

[0086] The volume content of hydrogen in the argon-hydrogen mixed gas is 10%.

[0087] Example 1

[0088] FeSO4·7H2O was heated in a tube furnace at 2℃min under the protection of argon-hydrogen mixed gas. -1 The heating rate was 200℃ and sintered for 12h to obtain FeSO4. 9.4gFeSO4, 5.64gNa2SO4, 0.782gascorbic acid and 0.8428gMIL-53(Al) were placed in a ball mill, and an appropriate amount of acetone was added. The ball mill was filled with argon-hydrogen mixed gas, and then ball milled at a speed of 550rpm for 10h. The ball-milled sample was placed in a tube furnace at 2℃min under the protection of argon-hydrogen mixed gas. -1 Heating rate: 200℃ pre-sintering for 6h. After pre-sintering, -1 Heating rate, sintering at 400℃ for 18h, Na2Fe 1.88 Al 0.12 (SO4)3 / C positive electrode composite material.

[0089] The positive electrode material prepared in this example was characterized, and the results were as follows:

[0090] Figure 1 The XRD spectrum of Example 1 in the embodiment is basically consistent with the PDF standard card of sodium ferrous sulfate, and all diffraction peaks belong to the monoclinic structure of the C2 / C space group, which belongs to the Pl space group, which is consistent with the NFS previously reported in the literature, indicating that the use of MIL-53 (Al) for Al doping and carbon coating does not change the crystal structure of NFS. In addition, compared with Example 1, the XRD spectrum of Example 2 has a miscellaneous peak located at about 46.1°, indicating that the by-product Al2O3 is produced in Example 2; the XRD spectrum of Comparative Example 2 has miscellaneous peaks located at about 46.1°, 21.4°, 32.9°, and 35.9°, indicating that the by-products Na6Fe(SO4)4, Fe2(SO4)3, and Fe2O3 are produced in Example 2. The above results show that adding an appropriate amount of MIL-type MOF material and using the method of ball milling protected by argon hydrogen atmosphere can obtain a material with higher purity.

[0091] Figure 2 This is a scanning electron microscope (SEM) image of the sodium ferrous sulfate positive electrode composite material prepared in Example 1. Figure 2 It can be seen that sodium ferrous sulfate is composed of nano-scale particles that form aggregates to form secondary particles. There are many micropores between the particles and the specific surface area is large, which increases the contact area between the material and the electrolyte and increases the reaction active sites.

[0092] The prepared sodium ferrous sulfate cathode material was assembled into a CR2032 button cell and the constant current charge and discharge performance test was carried out at a current density of 0.5C. The results are shown in Figure 3 .according to Figure 3 The data in the table show that after 500 consecutive cycles, the coulombic efficiency of each week is maintained at more than 99%, and the battery capacity retention rate is 87% after 200 cycles, and still has a capacity retention rate of 78.2% after 500 cycles; according to Figure 4 From the data, we can see that the charge and discharge curves of the 2nd, 10th, 50th and 100th weeks are stable and have little difference, and the initial specific capacity can reach 96.2mAh / g. It can be seen that the battery capacity decays slowly and has good cycle stability.

[0093] The prepared sodium ferrous sulfate cathode material was assembled into a CR2032 button battery, and the constant current charge and discharge performance was tested at different current densities of 0.1C, 0.2C, 0.5C, 1C, and 2C, and the cycle was repeated for 10 weeks at each current density. The results are shown in Figure 5 .according to Figure 5 From the data, we can see that at a current of 2C, the specific capacity is still 79.8mAh / g. This shows that the battery has good rate performance.

[0094] Figure 6 This is a cyclic voltammetry test diagram of a CR2032 button battery assembled with the sodium ferrous sulfate positive electrode composite material prepared in Example 1. Figure 6 It can be seen that the surface exhibits two pairs of redox peaks, corresponding to the Fe 2+ with Fe 3+ redox reaction.

[0095] Example 2

[0096] FeSO4·7H2O was heated in a tube furnace at 2℃min under the protection of argon-hydrogen mixed gas. -1 The heating rate was 200℃ and sintered for 12h to obtain FeSO4. 9g FeSO4, 5.64g Na2SO4, 0.782g ascorbic acid and 1.405g MIL-53(Al) were placed in a ball mill, and an appropriate amount of acetone was added. The ball mill ratio was 20:1. The ball mill was filled with argon-hydrogen mixed gas, and then ball milled at a speed of 550rpm for 10h. The ball-milled sample was placed in a tube furnace at 2℃min under the protection of argon-hydrogen mixed gas. -1 Heating rate: pre-sintering at 200℃ for 6h. After pre-sintering, heating rate is 2℃min -1 Heating rate, sintering at 400℃ for 18h, Na2Fe 1.8 Al 0.2 (SO4)3 / C positive electrode composite material.

[0097] The positive electrode material prepared in this example was characterized, and the results were as follows:

[0098] The XRD spectrum of the sodium ferrous sulfate positive electrode material prepared in this example is basically consistent with the PDF standard card of sodium ferrous sulfate. All diffraction peaks belong to the monoclinic structure of the C2 / C space group and the Pl space group, which is consistent with the NFS previously reported in the literature. However, additional impurity peaks of Al2O3 were observed in the spectrum, indicating that by-products were produced during the preparation process.

[0099] The prepared sodium ferrous sulfate cathode material was assembled into a CR2032 button battery, and the constant current charge and discharge performance test was carried out at a current density of 0.5C. The first week charging capacity was 86.8mAh / g, and the coulomb efficiency of each week was maintained above 99% after 100 consecutive cycles except for the initial few weeks. Moreover, the battery capacity retention rate after 100 weeks was 88%, and the specific capacity was 76.4mAh / g at this time. It can be seen that the battery capacity is slightly lower than the product with an Al doping amount of 0.12, but it still has good cycle stability.

[0100] Example 3

[0101] FeSO4·7H2O was heated in a tube furnace at 2℃min under the protection of argon-hydrogen mixed gas.-1 The heating rate was 200℃ and sintered for 12h to obtain FeSO4. 9g FeSO4, 5.64g Na2SO4, 0.782g ascorbic acid and 0.2g MIL-53(Al) were placed in a ball mill, and an appropriate amount of acetone was added. The ball mill ratio was 20:1. The ball mill was filled with argon-hydrogen mixed gas, and then ball milled at a speed of 550rpm for 10h. The ball-milled sample was placed in a tube furnace at 2℃min under the protection of argon-hydrogen mixed gas. -1 Heating rate: pre-sintering at 200℃ for 6h. After pre-sintering, heating rate is 2℃min -1 Heating rate, sintering at 400℃ for 18h, Na2Fe 1.99 Al 0.01 (SO4)3 / C positive electrode composite material.

[0102] The positive electrode material prepared in this example was characterized, and the results were as follows:

[0103] The XRD spectrum of the sodium ferrous sulfate positive electrode material prepared in this example is basically consistent with the PDF standard card of sodium ferrous sulfate. All diffraction peaks belong to the monoclinic structure of the C2 / C space group and the Pl space group, which is consistent with the NFS previously reported in the literature. However, additional impurity peaks of Al2O3 were observed in the spectrum, indicating that by-products were produced during the preparation process.

[0104] The prepared sodium ferrous sulfate positive electrode material was assembled into a CR2032 button battery, and the constant current charge and discharge performance test was carried out at a current density of 0.5C. The first week charging capacity was 86.9mAh / g, and the continuous cycle lasted for 100 weeks. Except for the initial few weeks, the coulomb efficiency of each week was maintained above 99%, and the battery capacity retention rate after 100 weeks was 88%, and the capacity was 76.7mAh / g at this time. It can be seen that the battery capacity is slightly lower than the product with an Al doping amount of 0.12, but it still has good cycle stability.

[0105] Example 4

[0106] FeSO4·7H2O was heated in a tube furnace at 2℃min under the protection of argon-hydrogen mixed gas. -1 The heating rate was 200℃ and sintered for 12h to obtain FeSO4. 10gFeSO4, 5.64gNa2SO4, 0.782gascorbic acid and 0.8813gMIL-53(Cr) were put into a ball mill, and an appropriate amount of acetone was added. The ball mill was filled with argon-hydrogen mixed gas, and then ball milled at a speed of 550rpm for 10h. The ball milled sample was placed in a tube furnace at 2℃min under the protection of argon-hydrogen mixed gas. -1 Heating rate: pre-sintering at 200℃ for 6h. After pre-sintering, heating rate is 2℃min -1Heating rate, sintering at 400℃ for 18h, Na2Fe 1.88 Cr 0.12 (SO4)3 / C positive electrode composite material.

[0107] The positive electrode material prepared in this example was characterized, and the results were as follows:

[0108] The XRD spectrum of the sodium ferrous sulfate cathode material prepared in this embodiment is basically consistent with the PDF standard card of sodium ferrous sulfate, and all diffraction peaks belong to the monoclinic structure of the C2 / C space group, which belongs to the Pl space group, which is consistent with the NFS previously reported in the literature, indicating that the use of MIL-53 (Cr) for Cr doping and carbon coating does not change the crystal structure of NFS. In addition, there are fewer impurity peaks in the XRD spectrum, indicating that the synthesis method can obtain a material with higher purity, which may be due to the use of argon hydrogen atmosphere protection during the ball milling process.

[0109] The prepared sodium ferrous sulfate cathode material was assembled into a CR2032 button battery, and the constant current charge and discharge performance test was carried out at a current density of 0.5C. The first week charging capacity was 94.5mAh / g, and the coulomb efficiency of each week was maintained above 99% after 100 consecutive cycles except for the initial weeks. Moreover, the battery capacity retention rate after 100 weeks was 87%, and the specific capacity was 82.22mAh / g at this time. It can be seen that the battery capacity decays slowly and has good cycle stability.

[0110] Example 5

[0111] FeSO4·7H2O was heated in a tube furnace at 2℃min under the protection of argon-hydrogen mixed gas. -1 The heating rate was 200℃ and sintered for 12h to obtain FeSO4. 10gFeSO4, 5.64gNa2SO4, 0.782gascorbic acid and 0.7819gMIL-100(Al) were placed in a ball mill, and an appropriate amount of acetone was added. The ball mill ratio was 20:1. The ball mill was filled with argon-hydrogen mixed gas, and then ball milled at a speed of 550rpm for 10h. The ball-milled sample was placed in a tube furnace at 2℃min under the protection of argon-hydrogen mixed gas. -1 Heating rate: 200℃ pre-sintering for 6h. After pre-sintering, -1 Heating rate, sintering at 400℃ for 18h, Na2Fe 1.88 Al 0.12 (SO4)3 / C positive electrode composite material.

[0112] The positive electrode material prepared in this example was characterized, and the results were as follows:

[0113] The XRD spectrum of the sodium ferrous sulfate cathode material prepared in this embodiment is basically consistent with the PDF standard card of sodium ferrous sulfate, and all diffraction peaks belong to the monoclinic structure of the C2 / C space group, which belongs to the Pl space group, which is consistent with the NFS previously reported in the literature, indicating that the use of MIL-100 (Al) for Al doping and carbon coating does not change the crystal structure of NFS. In addition, there are fewer impurity peaks in the XRD spectrum, indicating that the synthesis method can obtain a material with higher purity, which may be due to the use of argon hydrogen atmosphere protection during the ball milling process.

[0114] The prepared sodium ferrous sulfate cathode material was assembled into a CR2032 button battery, and the constant current charge and discharge performance test was carried out at a current density of 0.5C. The first week charging specific capacity was 90.3mAh / g, and the battery capacity retention rate after 100 weeks was 92%, at which time the specific capacity was 83.1mAh / g. It can be seen that the material has a high specific capacity and good cycle stability.

[0115] Example 6

[0116] FeSO4·7H2O was heated in a tube furnace at 2℃min under the protection of argon-hydrogen mixed gas. -1 The heating rate was 200℃ and sintered for 12h to obtain FeSO4. 10gFeSO4, 5.64gNa2SO4, 0.782gascorbic acid and 0.8872gMIL-100(Cr) were put into a ball mill, and an appropriate amount of acetone was added. The ball mill was filled with argon-hydrogen mixed gas, and then ball milled at a speed of 550rpm for 10h. The ball milled sample was placed in a tube furnace at 2℃min under the protection of argon-hydrogen mixed gas. -1 Heating rate: pre-sintering at 200℃ for 6h. After pre-sintering, heating rate is 2℃min -1 Heating rate, sintering at 400℃ for 18h, Na2Fe 1.88 Cr 0.12 (SO4)3 / C positive electrode composite material.

[0117] The positive electrode material prepared in this example was characterized, and the results were as follows:

[0118] The XRD spectrum of the sodium ferrous sulfate cathode material prepared in this embodiment is basically consistent with the PDF standard card of sodium ferrous sulfate, and all diffraction peaks belong to the monoclinic structure of the C2 / C space group, which belongs to the Pl space group, which is consistent with the NFS previously reported in the literature, indicating that the use of MIL-100 (Cr) for Cr doping and carbon coating does not change the crystal structure of NFS. In addition, there are fewer impurity peaks in the XRD spectrum, indicating that the synthesis method can obtain a material with higher purity, which may be due to the use of argon hydrogen atmosphere protection during the ball milling process.

[0119] The prepared sodium ferrous sulfate cathode material was assembled into a CR2032 button battery, and the constant current charge and discharge performance test was carried out at a current density of 0.5C. The first week charging specific capacity was 89.5mAh / g, and the battery capacity retention rate after 100 weeks was 92.3%, at which time the specific capacity was 82.6mAh / g. It can be seen that the battery capacity decays slowly and has good cycle stability.

[0120] Comparative Example 1

[0121] FeSO4·7H2O was heated in a tube furnace at 2℃min under the protection of argon-hydrogen mixed gas. -1 The heating rate was 200℃ and sintered for 12h to obtain FeSO4. 10gFeSO4, 5.64gNa2SO4, 0.782gascorbic acid and 0.846gAl(NO3)3 were put into a ball mill, and an appropriate amount of acetone was added. The ball mill ratio was 20:1. The ball mill was filled with argon-hydrogen mixed gas, and then ball milled at a speed of 550rpm for 10h. The ball-milled sample was placed in a tube furnace at 2℃min under the protection of argon-hydrogen mixed gas. -1 Heating rate: 200℃ pre-sintering for 6h. After pre-sintering, -1 Heating rate, sintering at 400℃ for 18h, Na2Fe 1.88 Al 0.12 (SO4)3 / C positive electrode composite material.

[0122] The positive electrode material prepared in this comparative example was characterized, and the results were as follows:

[0123] The XRD spectrum of the sodium ferrous sulfate positive electrode material prepared in this comparative example is basically consistent with the PDF standard card of sodium ferrous sulfate. All diffraction peaks belong to the monoclinic structure of the C2 / C space group and the Pl space group, which is consistent with the NFS previously reported in the literature. However, additional impurity peaks of Al2O3 were observed in the spectrum, indicating that by-products were produced during the preparation process.

[0124] The prepared sodium ferrous sulfate positive electrode material was assembled into a CR2032 button battery, and the constant current charge and discharge performance test was carried out at a current density of 0.5C. The first week charging specific capacity was 79.7mAh / g, and the continuous cycle lasted for 100 weeks. Except for the initial few weeks, the coulomb efficiency of each week was maintained above 99%. The battery capacity retention rate after 100 weeks was 82.6%, and the specific capacity was 65.8mAh / g. It can be seen that the battery capacity is relatively low, only 82.8% of the experimental group using MIL-53 (Al) as the Al doping source, and the capacity decay is fast, and the cycle stability is poor.

[0125] Comparative Example 2

[0126] FeSO4·7H2O was heated in a tube furnace at 2℃min under the protection of argon-hydrogen mixed gas. -1 The heating rate was 200℃ and sintered for 12h to obtain FeSO4. 10gFeSO4, 5.64gNa2SO4, 0.782g ascorbic acid and 0.8428g glucose were placed in a ball mill, and an appropriate amount of acetone was added. The ball mill ratio was 20:1. The ball mill was filled with argon-hydrogen mixed gas, and then ball milled at a speed of 550rpm for 10h. The ball-milled sample was placed in a tube furnace at 2℃min under the protection of argon-hydrogen mixed gas. -1 Heating rate: pre-sintering at 200℃ for 6h. After pre-sintering, heating rate is 2℃min -1 The heating rate was increased to 400℃ and sintered for 18h to obtain the Na2Fe2(SO4)3 / C positive electrode composite material.

[0127] The positive electrode material prepared in this comparative example was characterized, and the results were as follows:

[0128] The XRD spectrum of the sodium ferrous sulfate positive electrode material prepared in this comparative example is basically consistent with the PDF standard card of sodium ferrous sulfate. All diffraction peaks belong to the monoclinic structure of the C2 / C space group and the Pl space group, which is consistent with the NFS previously reported in the literature. However, additional impurity peaks are observed in the spectrum, indicating that by-products such as Na6Fe(SO4)4 and Fe2(SO4)3 are produced during the preparation process.

[0129] The prepared sodium ferrous sulfate cathode material was assembled into a CR2032 button battery, and the constant current charge and discharge performance test was carried out at a current density of 0.5C. The first week charging capacity was 88mAh / g, and the continuous cycle lasted for 100 weeks. Except for the initial few weeks, the coulomb efficiency of each week was maintained above 99%, and the battery capacity retention rate after 100 weeks was 84.6%, and the specific capacity was 74.45mAh / g. It can be seen that the effect of using glucose as a carbon source is poor, indicating that the MIL MOF material is an aromatic carbon source, which is easier to aromatize and has a higher degree of carbonization at a lower temperature.

[0130] Comparative Example 3

[0131] FeSO4·7H2O was heated in a tube furnace at 2℃min under the protection of argon-hydrogen mixed gas. -1 The heating rate was 200℃ and sintered for 12h to obtain FeSO4. 10gFeSO4, 5.64gNa2SO4 and 1.625gg of glucose were put into a ball mill, and an appropriate amount of acetone was added. The ball mill ratio was 20:1. The ball mill was filled with argon-hydrogen mixed gas, and then ball milled at a speed of 550rpm for 10h. The ball-milled sample was placed in a tube furnace at 2℃min under the protection of argon-hydrogen mixed gas. -1 Heating rate: pre-sintering at 200℃ for 6h. After pre-sintering, heating rate is 2℃min-1 The heating rate was 400°C and sintered for 18 hours to obtain a Na2Fe2(SO4)3 / C cathode composite material. The cathode material prepared in this comparative example was characterized, and the results were as follows:

[0132] The XRD spectrum of the sodium ferrous sulfate positive electrode material prepared in this comparative example is basically consistent with the PDF standard card of sodium ferrous sulfate. All diffraction peaks belong to the monoclinic structure of the C2 / C space group and the Pl space group, which is consistent with the NFS previously reported in the literature. However, additional impurity peaks are observed in the spectrum, indicating that by-products such as Fe2O3, Na6Fe(SO4)4 and Fe2(SO4)3 are produced during the preparation process.

[0133] The prepared sodium ferrous sulfate cathode material was assembled into a CR2032 button cell, and constant current charge and discharge performance was tested at a current density of 0.5C. The first week charging capacity was 73.04mAh / g, and the cycle was continuous for 100 weeks. Except for the initial few weeks, the coulomb efficiency of each week was maintained above 99%. The battery capacity retention rate after 100 weeks was 89.7%, and the specific capacity was 65.52mAh / g. It can be seen that the comparison sample using only glucose as a reducing agent and supplementing the carbon source has poor performance, which may be due to the weak reducibility of glucose and the high required carbonization temperature.

[0134] From the above experimental results, it can be seen that the metal organic framework used in the present invention is pyrolyzed to form a mesoporous nano-network structure carbon material and a Na2Fe 2-x M x (SO4)3 / C is an alivalent metal element in the iron position. During the synthesis process, MOF materials are used to achieve joint modification of metal ion doping and carbon coating. MIL-type MOF materials are aromatic carbon sources, which are easier to aromatize and have a higher degree of carbonization at lower temperatures. The mesoporous carbon coating layer improves the electronic conductivity and the wettability of the electrolyte to the positive electrode material. The sodium ferrous sulfate positive electrode material prepared by the method of the present invention has high specific capacity, high coulombic efficiency and high capacity retention rate, and exhibits good cycle performance and rate performance.

[0135] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a sodium ion battery positive electrode composite material, characterized in that: The following steps are involved: A) ball milling ferrous salt, sodium salt, sulfur source, carbon source and MIL-type MOF material under reducing atmosphere to obtain a mixture; The molar ratio of the ferrous ions in the ferrous salt to the sodium ions in the sodium salt is 1:0.5-1; The molar amount of the metal ions in the MIL-type MOF material is 0.5-10% of the molar amount of Fe in the ferrous salt; The input amount of the carbon source is 5-15% of the mass of the positive electrode composite material; B) sintering the mixture under reducing atmosphere to obtain Na2Fe 2-x M x (SO4)3 / C cathode composite material, wherein M is selected from Al or Cr, and x is in the range of 0.01 to 0.2; The sintering step comprises: 1~5℃min -1 The heating rate is 200~280℃ for 4~8h, then 1~5℃min -1 The heating rate is 300~400℃ and sintered for 10~24h.

2. The preparation method according to claim 1, characterized in that: The MIL-type MOF material is selected from at least one of MIL-53 (Al), MIL-53 (Cr), MIL-100 (Al) or MIL-100 (Cr).

3. The preparation method according to claim 2, characterized in that: The ferrous salt includes any one or more of ferrous sulfate, ferrous chloride, ferrous carbonate, and ferrous oxalate; and / or The sodium salt includes any one or more of sodium carbonate, sodium bicarbonate, sodium hydroxide, sodium ethoxide, sodium sulfate, sodium nitrate, sodium acetate, and sodium bisulfate; and / or The sulfur source includes any one or more of ferrous sulfate, sodium sulfate, potassium sulfate, and calcium sulfate; and / or The carbon source is selected from any one or more of glucose, sucrose, fructose, cellulose, starch and ascorbic acid.

4. The preparation method according to claim 3, characterized in that: The ferrous salt is ferrous sulfate; and the carbon source is ascorbic acid.

5. The preparation method according to any one of claims 1 to 4, characterized in that The ball milling step comprises: Under reducing atmosphere conditions, ferrous salt, sodium salt, sulfur source, carbon source and MIL-type MOF material are mixed with acetone for ball milling; the ball-to-material ratio is 10-20:1, the reducing atmosphere is selected from argon-hydrogen mixed gas, the ball milling speed is 450-600rpm, and the ball milling time is 4-12h.

6. A sodium ion battery positive electrode composite material prepared by the preparation method according to any one of claims 1 to 5, characterized in that: The sodium ion battery positive electrode composite material is Na2Fe 2-x M x (SO4)3 / C positive electrode composite material, wherein M is selected from Al or Cr, and x ranges from 0.01 to 0.

2.

7. The sodium ion battery positive electrode composite material according to claim 6, characterized in that: The Na2Fe 2-x M x The first-week charging capacity of the (SO4)3 / C cathode composite material ranges from 86.8 to 96.2 mAh / g, the coulombic efficiency is greater than 99%, and the capacity retention rate is ≥88% after 100 weeks of constant current charge and discharge at a current density of 0.5C.

8. A positive electrode sheet, characterized in that: A sodium ion battery positive electrode composite material prepared by the preparation method according to any one of claims 1 to 5, or a sodium ion battery positive electrode composite material according to any one of claims 6 or 7.

9. A secondary battery, characterized in that: Including the positive electrode sheet as described in claim 8.