Rare earth sintered magnet, method for producing rare earth sintered magnet, rotor and rotating machine
By introducing elements such as Cu, Al or Ga into Nd-Fe-B magnets, the distribution of Sm and element M is optimized to form a specific crystal structure, and the magnetic characteristics of Nd-Fe-B magnets are solved. Problem, high residual magnetic flux density and coercivity are achieved, and the consumption of heavy rare earth elements is reduced.
Patent Information
- Application Number
- CN202180101117.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-08-04
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-08-04
AI Technical Summary
The magnetic characteristics of the existing Nd-Fe-B system sintered magnets decrease when the temperature rises, and the consumption of heavy rare earth elements increases, resulting in increased costs and procurement risks. It is difficult for the existing technology to improve the magnetic characteristics of room temperature while suppressing the magnetic properties caused by temperature rise. Decreased characteristics.
Using rare earth sintered magnets of the general formula (Nd, La, Sm)-Fe-B-M, the main phase and oxide sub-phase of the R2Fe14B crystal structure are formed by introducing elements such as Cu, Al or Ga into the Nd-Fe-B magnet. The concentration distribution of Sm and element M is optimized to improve magnetic properties and coercivity.
It is achieved while suppressing the use of Nd and heavy rare earth elements, and the magnetic characteristics of room temperature are improved and the reduction of magnetic characteristics brought about by temperature rise, meeting the demand of industrial motors for high residual magnetic flux density and coercivity.
Smart Images

Figure CN117751414B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a rare earth sintered magnet, which is a permanent magnet obtained by sintering a material containing a rare earth element, and a method for producing the rare earth sintered magnet, a rotor, and a rotating machine. Background Art
[0002] It is known that the tetragonal R2T 14 RTB permanent magnets with B intermetallic compound as the main phase. Among them, element R is a rare earth element, element T is a transition metal element such as Fe (iron) or Fe in which a part is replaced by Co (cobalt), and B is boron. RTB permanent magnets are used in various high value-added components, mainly industrial motors. In particular, Nd-Fe-B sintered magnets with element R being Nd (neodymium) have excellent magnetic properties and are therefore used in various components. In addition, industrial motors are often used in high-temperature environments exceeding 100°C, so attempts have been made to increase the coercive force by adding heavy rare earth elements such as Dy (dysprosium) to Nd-TB permanent magnets.
[0003] In recent years, the production of Nd-Fe-B system sintered magnets has been expanding, and the consumption of Nd and heavy rare earth elements such as Dy and Tb (terbium) has been increasing. However, the price of Nd and heavy rare earth elements is high, and the regional heterogeneity is high, which poses a procurement risk. Therefore, as a countermeasure to reduce the consumption of Nd and heavy rare earth elements, it is considered to use other rare earth elements such as Ce (cerium), La (lanthanum), Sm (samarium), Sc (scandium), Gd (gadolinium), Y (yttrium) and Lu (lutetium) in element R. However, it is known that when all or part of Nd is replaced by these elements, the magnetic properties are significantly reduced. Therefore, so far, attempts have been made to develop a technology that can suppress the reduction in magnetic properties associated with temperature rise when these elements are used in the manufacture of Nd-Fe-B system sintered magnets.
[0004] For example, Patent Document 1 discloses a rare earth magnet alloy having: 14 B crystal structure, a main phase with one or more elements selected from Nd, La and Sm and Fe and B as main constituent elements; a crystalline subphase with one or more elements selected from Nd, La and Sm and O (oxygen) as main constituent elements. In the rare earth magnet alloy described in Patent Document 1, La is segregated in the crystalline subphase, and Sm is dispersed in the crystalline subphase of the main phase without segregation. In the rare earth magnet alloy described in Patent Document 1, by forming the above-mentioned organizational form, the reduction of magnetic properties associated with temperature rise is suppressed.
[0005] Patent Document 2 discloses a rare earth magnet comprising: a T bThe first phase of the compound represented by X; the concentration of element R existing at the grain boundary of the first phase is greater than R a T b X high grain boundary phase; and S c M d The second phase is composed of a single crystal of a compound represented by. Among them, the element R is one or more rare earth elements including Nd, the element T is one or more transition metal elements including Fe, and the element X is one or more elements selected from B and C (carbon). The element S is one or more rare earth elements including Sm, and the element M is one or more transition metal elements including Co. According to the technology described in Patent Document 2, a rare earth magnet having sufficient magnetic properties even at high temperatures is obtained.
[0006] Patent document 3 discloses an RTB-based sintered magnet having: a first main phase composed of grains of an RTB-based alloy containing a light rare earth element as an element R, a second main phase composed of grains of an RTB-based alloy containing a heavy rare earth element as an element R, a surface phase surrounding the surfaces of the grains constituting the first main phase and the second main phase, and a grain boundary alloy phase existing at a triple point of grain boundaries. Among them, element T is a product of replacing Fe or a part of Fe with Co. In the RTB-based sintered magnet described in Patent document 3, the concentration of heavy rare earth elements is lower in the first main phase and the grain boundary alloy phase than in the second main phase and the surface phase. According to the technology described in Patent document 3, it is possible to effectively increase the coercive force using rare earth elements that impart high coercive force.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: International Publication No. 2021 / 048916
[0010] Patent Document 2: Japanese Patent Application Publication No. 2021-9862
[0011] Patent Document 3: Japanese Patent Application Publication No. 2018-174205 Summary of the invention
[0012] Problems to be solved by the invention
[0013] However, as for the rare earth magnet alloy described in Patent Document 1, since Sm is uniformly dispersed in the main phase and the subphase in the rare earth magnet alloy, even if the reduction of magnetic properties associated with the temperature rise can be suppressed, it may not contribute to the improvement of magnetic properties at room temperature. In addition, as for the rare earth magnet described in Patent Document 2, the second phase is composed of a single crystal, and there is no concentration difference in the elements present in the second phase. That is, the second phase is distributed in the rare earth magnet, but has the same composition at any position and is formed by a compound with a uniform concentration distribution. Therefore, even in the rare earth magnet described in Patent Document 2, the improvement of magnetic properties at room temperature has not yet become the best organization. That is, there is a problem that there is room for further improvement of magnetic properties. In addition, in the RTB-based sintered magnet described in Patent Document 3, although a high coercive force is obtained due to the formation of a structure that must contain heavy rare earth elements, the residual magnetic flux density required for industrial motors, etc. cannot be obtained, and there is a problem of reduced magnetic properties. As described above, there is a demand for a rare earth sintered magnet that achieves both improvement of magnetic properties at room temperature and suppression of degradation of magnetic properties associated with temperature rise.
[0014] The present disclosure has been made in view of the above circumstances, and an object of the present disclosure is to obtain a rare earth sintered magnet capable of improving magnetic properties at room temperature and suppressing a decrease in magnetic properties associated with a temperature rise while suppressing the use of Nd and heavy rare earth elements.
[0015] Means for solving problems
[0016] In order to solve the above problems and achieve the purpose, the present invention discloses a rare earth sintered magnet in which the element M is one or more elements selected from Cu, Al and Ga and satisfies the general formula (Nd, La, Sm)-Fe-BM, and has: 14 A main phase of crystal grains having a basic B crystal structure, a crystalline first subphase mainly composed of an oxide phase represented by (Nd, La, Sm)-O, and a crystalline second subphase mainly composed of an oxide phase represented by (Nd, La)-O. The first subphase has a higher Sm concentration than the second subphase, and the second subphase has a higher element M concentration than the first subphase.
[0017] Effects of the Invention
[0018] According to the present disclosure, it is possible to achieve an effect of improving magnetic properties at room temperature and suppressing a decrease in magnetic properties associated with a temperature rise while suppressing the use of Nd and heavy rare earth elements. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a diagram schematically showing an example of the structure of the rare earth sintered magnet in the sintered state according to the first embodiment.
[0020] Figure 2 To represent tetragonal Nd2Fe 14 B Diagram of the atomic sites in the crystal structure.
[0021] Figure 3 This is a flowchart showing an example of steps of a method for producing a rare earth magnet alloy according to the second embodiment.
[0022] Figure 4 This is a diagram schematically showing a method for producing a rare earth magnet alloy according to the second embodiment.
[0023] Figure 5 This is a flowchart showing an example of the steps of the method for producing a rare earth sintered magnet according to the second embodiment.
[0024] Figure 6 It is a cross-sectional view schematically showing an example of the structure of a rotor equipped with a rare earth sintered magnet according to the third embodiment.
[0025] Figure 7 It is a cross-sectional view schematically showing an example of the structure of a rotating machine according to the fourth embodiment.
[0026] Figure 8 These are composition images obtained by analyzing the cross sections of the rare earth sintered magnets according to Examples 1 to 8 using FE-EPMA.
[0027] Fig. 9 This is the elemental mapping of Nd obtained by analyzing the cross sections of the rare earth sintered magnets according to Examples 1 to 8 using FE-EPMA.
[0028] Fig.10 The elemental surface distribution of O is obtained by analyzing the cross section of the rare earth sintered magnet according to Examples 1 to 8 using FE-EPMA.
[0029] Fig.11 The elemental planar distribution of La was obtained by analyzing the cross sections of the rare earth sintered magnets according to Examples 1 to 8 using FE-EPMA.
[0030] Fig.12 The elemental surface distribution of Sm is obtained by analyzing the cross sections of the rare earth sintered magnets according to Examples 1 to 8 using FE-EPMA.
[0031] Fig.13 The elemental surface distribution of Cu was obtained by analyzing the cross sections of the rare earth sintered magnets according to Examples 1 to 8 using FE-EPMA.
[0032] Fig.14 The elemental surface distribution of Al was obtained by analyzing the cross sections of the rare earth sintered magnets according to Examples 1 to 8 using FE-EPMA.
[0033] Fig.15 The elemental surface distribution of Ga was obtained by analyzing the cross sections of the rare earth sintered magnets according to Examples 1 to 8 using FE-EPMA. DETAILED DESCRIPTION
[0034] Hereinafter, a rare earth sintered magnet, a method for producing a rare earth sintered magnet, a rotor, and a rotating machine according to an embodiment of the present disclosure will be described in detail with reference to the drawings.
[0035] Implementation method 1.
[0036] Figure 1 FIG. 1 is a diagram schematically showing an example of the structure of a sintered rare earth sintered magnet according to Embodiment 1. The permanent magnet according to Embodiment 1 is a rare earth sintered magnet 1 satisfying the general formula (Nd, La, Sm)-Fe-BM, and having a structure containing R2Fe 14 A rare earth sintered magnet 1 having a main phase 10 of crystal grains having a basic B crystal structure, and a sub-phase 20. The sub-phase 20 has a crystalline first sub-phase 21 having an oxide phase represented by (Nd, La, Sm)-O as a main component, and a crystalline second sub-phase 22 having an oxide phase represented by (Nd, La)-O as a main component. The element M represents one or more elements selected from Cu (copper), Al (aluminum) and Ga (gallium).
[0037] The main phase 10 has a tetragonal R2Fe2O3 phase in which the elements R are Nd, La and Sm. 14 B crystal structure. That is, the main phase 10 has (Nd, La, Sm)2Fe 14 The composition formula of B. Make R2Fe with tetragonal crystal 14 The reason why the element R of the rare earth sintered magnet 1 having the B crystal structure is a rare earth element composed of Nd, La and Sm is that, according to the calculation result of the magnetic interaction energy using the molecular orbital method, by forming a composition in which La and Sm are added to Nd, a practical rare earth sintered magnet 1 capable of suppressing the deterioration of magnetic properties accompanying a temperature rise is obtained. In addition, by intentionally segregating La and Sm also at the grain boundary as an example of the sub-phase 20 and relatively diffusing Nd in the main phase 10, the crystal magnetic anisotropy of the main phase 10 can be improved. As a result, a quasi-core-shell structure in which a portion with high magnetic anisotropy and a portion with low magnetic anisotropy exist is formed in the main phase 10. As a result, the effect of suppressing the deterioration of magnetic properties accompanying a temperature rise is further improved.
[0038] It should be noted that if the added amount of La and Sm is too much, the amount of Nd, an element with high magnetic anisotropy constant and saturation magnetic polarization, will decrease, leading to a decrease in magnetic properties. Therefore, when the composition ratios of Nd, La and Sm are set to a, b and c respectively, it is preferably a>(b+c).
[0039] The average grain size of the crystal grains of the main phase 10 is preferably 100 μm or less, and more preferably 0.1 μm or more and 50 μm or less in order to improve the magnetic properties.
[0040] The crystalline subphase 20 is a general term for the crystalline first subphase 21 and the second subphase 22, and exists between the main phase 10. The crystalline first subphase 21 is represented by (Nd, La, Sm)-O as described above, and the crystalline second subphase 22 is represented by (Nd, La)-O as described above. (Nd, La, Sm) represented here means that part of Nd is replaced by La and Sm. It should be noted that the elements of the main components are recorded in parentheses here, so the first subphase 21 and the second subphase 22 may also contain trace amounts of other components. In one example, the second subphase 22 represented by (Nd, La)-O contains a very small amount of Sm.
[0041] In the rare earth sintered magnet 1 according to the first embodiment, the first subphase 21 has a higher concentration of Sm than the second subphase 22, and the second subphase 22 has a higher concentration of element M than the first subphase 21. In other words, Sm and element M are segregated in different subphases 20. Since Sm exists in a high concentration in the first subphase 21, Nd of the Nd-rich phase is relatively diffused into the main phase 10, thereby improving the crystal magnetic anisotropy of the main phase 10. Furthermore, since Sm also exists in the crystal grains of the main phase 10, it contributes to the improvement of the residual magnetic flux density by combining with Fe, which is a ferromagnetic body, in the same magnetization direction. Since element M exists in a high concentration in the second subphase 22, it forms a non-magnetic phase that magnetically separates the main phases 10, thereby contributing to the improvement of magnetic properties. Since Sm and the element M exist at high concentrations in different subphases 20 , it is possible to improve both the residual magnetic flux density and the coercive force.
[0042] In the rare earth sintered magnet 1 according to the first embodiment, there is a difference in the concentration of La and Sm between the main phase 10 and the sub-phase 20, the sum of the concentrations of La in the first sub-phase 21 and the second sub-phase 22 is greater than the concentration of La in the main phase 10, and the sum of the concentrations of Sm in the first sub-phase 21 and the second sub-phase 22 is greater than the concentration of Sm in the main phase 10. Specifically, the concentrations of La and Sm in the sub-phase 20 are greater than the concentrations of La and Sm in the main phase 10. Furthermore, there is a difference in the concentration of La between the first sub-phase 21 and the second sub-phase 22, and the concentration of La in the first sub-phase 21 is greater than the concentration of La in the second sub-phase 22.
[0043] Among them, when the La concentration contained in the main phase 10 is set to X, the La concentration contained in the first subphase 21 is set to X1, the La concentration contained in the second subphase 22 is set to X2, the Sm concentration contained in the main phase 10 is set to Y, the Sm concentration contained in the first subphase 21 is set to Y1, and the Sm concentration contained in the second subphase 22 is set to Y2, the relationship of the following formula (1) is satisfied.
[0044] 1<(Y1+Y2) / Y<(X1+X2) / X · · · (1)
[0045] As for La, since it exists at a high concentration in the grain boundary during the manufacturing process, especially the heat treatment process, Nd is relatively diffused into the main phase 10. As a result, in the rare earth sintered magnet 1 in the first embodiment, Nd of the main phase 10 is not consumed at the grain boundary, and the crystal magnetic anisotropy is improved. As for Sm, since it exists at a high concentration in the sub-phase 20, especially the first sub-phase 21, compared with the main phase 10, similarly to La, Nd is relatively diffused into the main phase 10, and the crystal magnetic anisotropy is improved.
[0046] The rare earth sintered magnet 1 according to the first embodiment may contain an additive element N for improving magnetic properties. The additive element N is one or more elements selected from Co, Zr (zirconium), Ti (titanium), Pr (praseodymium), Nb (niobium), Dy, Tb, Mn (manganese), Gd, and Ho (holmium).
[0047] Therefore, in the rare earth sintered magnet 1 according to the first embodiment, the general formula is (Nd a La b Sm c )Fe d B e M f N g It indicates that the added element N is one or more elements selected from Co, Zr, Ti, Pr, Nb, Dy, Tb, Mn, Gd and Ho. a, b, c, d, e, f and g preferably satisfy the following relationship.
[0048] 5≤a≤20
[0049] 0<b+c<a
[0050] 70≤d≤90
[0051] 0.5≤e≤10
[0052] 0≤f≤5
[0053] 0≤g≤5
[0054] a+b+c+d+e+f+g=100 atomic %
[0055] Secondly, for La and Sm in tetragonal R2Fe 14 Explain which atomic site in the crystal structure of B is replaced. Figure 2 To represent tetragonal Nd2Fe 14 B is a diagram of the atomic sites in the crystal structure. Figure 2 The crystal structure shown in is described in, for example, the following reference 1 Figure 1 The stabilization energy of the replaced site is calculated by band calculation and molecular field approximation of the Heisenberg model, and the judgment is made based on the value of the energy.
[0056] (Reference 1) JFHerbs et al. "Relationships between crys tal s tructureand magnet ic properties in Nd2Fe 14 B". PHYSICAL REVIEW B. 1984, Vol. 29, No. 7, pp. 4176-4178.
[0057] First, the calculation method of the stabilization energy in La is described. The stabilization energy in La can be calculated using Nd8Fe 56 B4 unit cell, through (Nd7La1)Fe 56 B4+Nd and Nd8(Fe 55 The energy difference between La1)B4+Fe is calculated. The smaller the energy value, the more stable it is when the atom is replaced at that site. That is, for La, the atomic site with the smallest energy is easily replaced. In this calculation, it is considered that when La is replaced with the original atom, the tetragonal R2Fe 14 The lattice constant in the B crystal structure does not change due to the difference in atomic radius. Table 1 is a table showing the stabilization energy of La at each substitution site when the ambient temperature is changed.
[0058] [Table 1]
[0059] (Table 1)
[0060]
[0061] Unit: eV
[0062] According to Table 1, the stable substitution site of La is the Nd(f) site at a temperature above 1000K, and is the Fe(c) site at a temperature of 293K and 500K. According to the rare earth sintered magnet 1 of Embodiment 1, as described later, the raw material of the rare earth sintered magnet 1 is heated to a temperature above 1000K and melted, and then rapidly cooled. Therefore, it is considered that the raw material of the rare earth sintered magnet 1 is maintained at a temperature above 1000K, that is, above 727°C, preferably around 1300K, that is, 1027°C. At this time, it is considered that La is substituted at the Nd(f) site or the Nd(g) site. Among them, it is considered that the energetically stable Nd(f) site is preferentially substituted with La, and among the substitution sites of La, substitution to the Nd(g) site with a small energy difference can also be performed. Therefore, the Nd(g) site can also be listed as a candidate for the substitution site of La.
[0063] Furthermore, when the rare earth sintered magnet 1 is manufactured by the manufacturing method described below, although the temperature is 1000K or more during sintering, the Fe(c) site described in Table 1 is maintained in the energy-stable temperature range by passing through the first aging step, the second aging step, and the cooling step. In other words, the substitution of La at the Nd site of the main phase 10 is maintained in an unstable energy state. That is, in the raw material stage of the rare earth sintered magnet 1, La is mainly substituted at the Nd site of the main phase 10, but in the rare earth sintered magnet 1 manufactured by the manufacturing method described below, it can be said that the Nd site of the main phase 10 is maintained in an unstable energy state temperature range, thereby releasing a certain amount of La from the Nd site of the main phase 10, and as a result, La is segregated in the sub-phase 20.
[0064] Next, the calculation method of the stabilization energy in Sm is described. The stabilization energy of Sm can be calculated by (Nd7Sm1)Fe 56 B4+Nd and Nd8(Fe 55 The energy difference of Sm1)B4+Fe is calculated. 14 The lattice constant in the B crystal structure does not change, which is the same as the case of La. Table 2 is a table showing the stabilization energy of Sm at each substitution site when the ambient temperature is changed.
[0065] [Table 2]
[0066] (Table 2)
[0067]
[0068] Unit:eV
[0069] According to Table 2, the stable substitution site of Sm is Nd(g) site at any temperature, unlike La. Although it is believed that Sm preferentially substitutes at the energetically stable Nd(g) site, it may also substitute at the Nd(f) site with a small energy difference among the substitution sites of Sm.
[0070] When the rare earth sintered magnet 1 is manufactured by the manufacturing method described later, the substitution at the Nd(g) site of the main phase 10 is most stable in terms of energy. However, as described above, since the temperature range where the substitution at the Nd site of the main phase 10 becomes unstable in La is maintained, a part of Sm is also released from the Nd site of the main phase 10 together with La, and segregates in the sub-phase 20. As a result, there is a concentration difference between La and Sm in the main phase 10 and the sub-phase 20, and the sum of the La concentrations in the first sub-phase 21 and the second sub-phase 22 is greater than the La concentration in the main phase 10, and the sum of the Sm concentrations in the first sub-phase 21 and the second sub-phase 22 is greater than the Sm concentration in the main phase 10. That is, it can be said that La and Sm are segregated in the sub-phase 20. Furthermore, since La is segregated in the sub-phase 20 together with Sm, it can be said that the La concentration in the first sub-phase 21 is greater than the La concentration in the second sub-phase 22, similarly to the Sm concentration.
[0071] In addition, when comparing La and Sm, it is found that La maintained in a temperature region of an unstable energy state tends to be overwhelmingly segregated in the subphase 20 from an energy point of view. Therefore, in the case of the rare earth sintered magnet 1 prepared with La and Sm concentrations being the same, the La segregation ratio in the subphase 20 is large relative to the La and Sm present in the rare earth sintered magnet 1, that is, the relationship of the above formula (1) is satisfied.
[0072] Furthermore, the element M, that is, the element such as Cu, Al and Ga, which forms a non-magnetic phase at the grain boundary and contributes to the high coercivity, also originally exists in the subphase 20. However, as described above, La and Sm are segregated in the same subphase 20 by undergoing the aging process and the cooling process, and as a result, the element M mainly exists in the subphase 20 different from La and Sm. That is, each element is not uniformly present, but the concentration of the element M including Cu, Al and Ga is higher in the second subphase 22 than in the first subphase 21. As a result, the rare earth sintered magnet 1 having the following characteristics is obtained: the concentration of Sm is higher in the first subphase 21 than in the second subphase 22, the concentration of the element M is higher in the second subphase 22 than in the first subphase 21, and the concentration of Sm and the element M is higher in the subphase 20 of different types.
[0073] As described above, the rare earth sintered magnet 1 of the first embodiment is a rare earth sintered magnet 1 in which the element M is one or more elements selected from Cu, Al and Ga and satisfies the general formula (Nd, La, Sm)-Fe-BM, and has a structure including R2Fe 14 The present invention comprises a main phase 10 having crystal grains based on a B crystal structure, a crystalline first subphase 21 having an oxide phase represented by (Nd, La, Sm)-O as a main component, and a crystalline second subphase 22 having an oxide phase represented by (Nd, La)-O as a main component. In the rare earth sintered magnet 1 of the first embodiment, the concentration of Sm in the first subphase 21 is increased compared to the second subphase 22, and the concentration of element M in the second subphase 22 is increased compared to the first subphase 21. That is, the concentration of Sm and the concentration of element M in the subphase 20 are different. As a result, since Sm exists in the first subphase 21 at a high concentration, Nd is relatively diffused into the main phase 10, thereby improving the crystal magnetic anisotropy of the main phase 10. Furthermore, since Sm also exists in the crystal grains of the main phase 10, it contributes to the improvement of the residual magnetic flux density by combining with Fe, which is a ferromagnetic body, in the same magnetization direction. Since the element M exists in the second subphase 22 at a high concentration, it forms a non-magnetic phase that magnetically separates the main phases 10, contributing to the improvement of magnetic properties. Since Sm and the element M exist in different subphases 20 at high concentrations, the residual magnetic flux density and the coercive force can be improved at the same time.
[0074] Furthermore, the main phase 10 has a tetragonal R2Fe2O3 phase in which the elements R are Nd, La and Sm. 14 B crystal structure, thus becoming a rare earth sintered magnet 1 capable of suppressing the deterioration of magnetic properties associated with temperature rise. As a result, compared with a rare earth sintered magnet satisfying Nd—Fe—B, a rare earth sintered magnet 1 capable of achieving improvement of magnetic properties at room temperature and suppression of deterioration of magnetic properties associated with temperature rise while suppressing the use of Nd and heavy rare earth elements can be obtained.
[0075] Implementation method 2.
[0076] In the second embodiment, the method for manufacturing the rare earth sintered magnet 1 described in the first embodiment is described separately as a method for manufacturing a rare earth magnet alloy that is a raw material of the rare earth sintered magnet 1 and a method for manufacturing the rare earth sintered magnet 1 using the rare earth magnet alloy.
[0077] Figure 3 This is a flowchart showing an example of steps of a method for producing a rare earth magnet alloy according to the second embodiment. Figure 4 This is a diagram schematically showing a method for producing a rare earth magnet alloy according to the second embodiment.
[0078] First, if Figure 3As shown in, the method for manufacturing a rare earth magnet alloy includes: a melting process (step S1) of heating a raw material of a rare earth magnet alloy containing elements constituting a rare earth sintered magnet 1 to a temperature of 1000K or more to melt the raw material; a first cooling process (step S2) of cooling the raw material in a molten state on a rotating body to obtain a solidified alloy; and a second cooling process (step S3) of further cooling the solidified alloy in a container. Each process is described below.
[0079] In the melting process of step S1, Figure 4 As shown in the figure, in an atmosphere containing an inert gas such as Ar (argon) or in a vacuum, the raw material of the rare earth magnet alloy is heated to a temperature of 1000K or more in a crucible 31 and melted. Thus, a molten alloy 32 of molten rare earth magnet alloy is prepared. As a raw material, a product of a combination of Nd, La, Sm, Fe, B, and one or more elements M selected from Al, Cu and Ga can be used. At this time, one or more elements selected from Co, Zr, Ti, Pr, Nb, Dy, Tb, Mn, Gd and Ho may also be included in the raw material as an added element N.
[0080] Secondly, in the first cooling process of step S2, Figure 4 As shown in the figure, the molten alloy 32 prepared in the melting step flows into the tundish 33, and then flows into the single roller 34 which is a rotating body rotating in the direction of the arrow. As a result, the molten alloy 32 is rapidly cooled on the single roller 34, and a solidified alloy 35 having a thickness thinner than that of the ingot alloy is prepared on the single roller 34 from the molten alloy 32. Here, as the rotating body that rotates, a single roller 34 is used, but it is not limited to this, and it can be contacted with a double roller, a rotating disk, a rotating cylindrical mold, etc. to be rapidly cooled. From the viewpoint of efficiently obtaining a thin solidified alloy 35, the cooling rate in the first cooling step is preferably not less than 10°C / second and not less than 10°C / second. 7 ℃ / sec or less, more preferably 10 3 ℃ / sec or more and 10 4 The thickness of the solidified alloy 35 is within a range of 0.03 mm to 10 mm. The molten alloy 32 solidifies from the portion in contact with the single roller 34 and crystals grow in a columnar or needle shape in the thickness direction from the contact surface with the single roller 34 .
[0081] Then, in the second cooling process of step S3, Figure 4As shown in the figure, the thin solidified alloy 35 prepared in the first cooling process is placed in a tray container 36 for cooling. The thin solidified alloy 35 is broken when entering the tray container 36, and becomes a scaly rare earth magnet alloy 37 and is cooled. Depending on the cooling rate, a strip-shaped rare earth magnet alloy 37 is sometimes obtained, and it is not limited to a scaly shape. From the perspective of obtaining a rare earth magnet alloy 37 with a good temperature characteristic of magnetic properties, the cooling rate in the second cooling process is preferably 10 -2 ℃ / sec or more and 10 5 ℃ / sec or less, more preferably 10 -1 ℃ / sec or more and 10 2 ℃ / second or less.
[0082] The rare earth magnet alloy 37 obtained through these steps has a fine crystalline structure including a (Nd, La, Sm)-Fe-B crystal phase having a minor axis dimension of 3 μm or more and 10 μm or less and a major axis dimension of 10 μm or more and 300 μm or less and a crystalline subphase 20 of an oxide represented by (Nd, La, Sm)-O. Hereinafter, the crystalline subphase 20 of an oxide represented by (Nd, La, Sm)-O is referred to as the (Nd, La, Sm)-O phase. The (Nd, La, Sm)-O phase is a non-magnetic phase composed of an oxide having a relatively high concentration of rare earth elements. The thickness of the (Nd, La, Sm)-O phase is equivalent to the width of the grain boundary and is less than 10 μm. As for the rare earth magnet alloy 37 manufactured by the above manufacturing method, since it undergoes a rapid cooling process, the structure is refined and the grain diameter is small compared with the rare earth magnet alloy obtained by the mold casting method.
[0083] Figure 5 FIG. 1 is a flow chart showing an example of the steps of the method for producing a rare earth sintered magnet according to Embodiment 2. Figure 5 As shown in, the manufacturing method of the rare earth sintered magnet 1 includes: a crushing process (step S21) of crushing the rare earth magnet alloy 37 satisfying (Nd, La, Sm)-Fe-BM; a molding process (step S22) of preparing a molded body by molding the powder of the crushed rare earth magnet alloy 37; a sintering process (step S23) of obtaining a sintered body by sintering the molded body; an aging process (step S24) of aging the sintered body; and a cooling process (step S25) of cooling the aged sintered body.
[0084] In the crushing process of step S21, Figure 3The rare earth magnet alloy 37 manufactured by the manufacturing method of the rare earth magnet alloy 37, that is, the rare earth magnet alloy 37 having the (Nd, La, Sm)-Fe-B crystal phase and the (Nd, La, Sm)-O phase, is crushed to obtain a rare earth magnet alloy powder having a particle size of less than 200 μm, preferably more than 0.5 μm and less than 100 μm. It is to be noted that, in the crushed rare earth magnet alloy 37, as described above, it contains one or more elements M selected from Al, Cu and Ga. As for the crushing of the rare earth magnet alloy 37, for example, an agate mortar, a pounding mill, a jaw crusher or a jet mill is used. In particular, in the case of reducing the particle size of the powder, it is preferred to crush the rare earth magnet alloy 37 in an atmosphere containing an inert gas. By crushing the rare earth magnet alloy 37 in an atmosphere containing an inert gas, the mixing of oxygen into the powder can be suppressed. However, in the case where the atmosphere during the crushing has no effect on the magnetic properties of the magnet, the crushing of the rare earth magnet alloy 37 can be carried out in the air.
[0085] In the molding process of step S22, the powder of the rare earth magnet alloy 37 is compression molded in a mold with a magnetic field applied to prepare a molded body. The applied magnetic field can be set to 2 T in one example. It should be noted that molding can be performed without a magnetic field and without applying a magnetic field.
[0086] In the sintering process of step S23, a sintered body is prepared by keeping the compression-molded molded body at a sintering temperature in the range of 900° C. to 1300° C. for a time in the range of 0.1 hours to 10 hours. As for sintering, in order to suppress oxidation, it is preferably carried out in an atmosphere containing an inert gas or in a vacuum. Sintering can be carried out while applying a magnetic field. In addition, in the sintering process, in order to improve the magnetic properties, that is, the anisotropy of the magnetic field or the coercive force, a heating process or an aging treatment process may also be added. Furthermore, a process of infiltrating a compound containing Cu, Al, a heavy rare earth element, etc. into the boundary between the main phases 10, that is, the grain boundary, may be added.
[0087] The aging process of step S24 includes a first aging process of step S24-1 and a second aging process of step S24-2. As for the conditions of the first aging process of step S24-1, the sintered body is kept at a temperature lower than the sintering temperature, i.e., the first aging temperature, specifically, at a temperature in the range of 700° C. to less than 900° C., for a period of 0.1 hour to 10 hours.
[0088] Regarding the conditions of the second aging process in step S24-2, after the first aging process, the sintered body is maintained at a temperature lower than the first aging temperature, i.e., the second aging temperature, specifically, at a temperature in the range of 450°C to less than 700°C, for a period of 0.1 hour to 10 hours.
[0089] In the cooling process of step S25, the sintered body is kept at a temperature lower than the second aging temperature, specifically, at a temperature in the range of 200°C to less than 450°C, for 0.1 to 5 hours. Then, the rare earth sintered magnet 1 is completed by cooling to room temperature.
[0090] In the above sintering step, aging step and cooling step, by controlling the temperature and time as described above, it is possible to manufacture the rare earth sintered magnet 1 in which the first subphase 21 has a higher concentration of Sm than the second subphase 22, and the second subphase 22 has a higher concentration of one or more elements M selected from Cu, Al and Ga than the first subphase 21. That is, in the aging step and cooling step, the crystalline first subphase 21 having an oxide phase represented by (Nd, La, Sm)-O as a main component and the crystalline second subphase 22 having an oxide phase represented by (Nd, La)-O as a main component are generated from the (Nd, La, Sm)-O phase, in one example, according to the concentration of the element M. It is to be noted that the second subphase 22 may contain a trace amount of Sm.
[0091] In the second embodiment, the rare earth magnet alloy powder obtained by crushing the rare earth magnet alloy 37 having the (Nd, La, Sm)-Fe-B crystal phase and the (Nd, La, Sm)-O phase is molded, the molded body is sintered to form a sintered body, and the sintered body is aged and cooled to manufacture the rare earth sintered magnet 1. Thus, the rare earth sintered magnet 1 according to the first embodiment can be manufactured. In addition, in the first aging step, the sintered body is maintained at a temperature lower than the sintering temperature, specifically, at a first aging temperature in a range of 700° C. to less than 900° C., for a period of 0.1 hour to 10 hours. In the second aging step, after the first aging step, the sintered body is maintained at a second aging temperature lower than the first aging temperature, specifically, at a temperature in a range of 450° C. to less than 700° C., for a period of 0.1 hour to 10 hours. In the cooling step, the sintered body is maintained at a temperature lower than the second aging temperature, specifically, at a temperature in a range of 200° C. to less than 450° C., for a period of 0.1 hour to 5 hours, and is cooled to room temperature. Thus, the rare earth sintered magnet 1 can be manufactured in which the first subphase 21 has a higher Sm concentration than the second subphase 22 , and the second subphase 22 has a higher concentration of one or more elements M selected from Cu, Al and Ga than the first subphase 21 .
[0092] Furthermore, through the above-mentioned manufacturing process, the following rare earth sintered magnet 1 can be manufactured: the sum of the La concentrations in the first subphase 21 and the second subphase 22 is equal to or higher than the La concentration in the main phase 10, the sum of the Sm concentrations in the first subphase 21 and the second subphase 22 is equal to or higher than the Sm concentration in the main phase 10, and the La concentration in the first subphase 21 is equal to or higher than the La concentration in the second subphase 22. In addition, the rare earth sintered magnet 1 can be manufactured in which the La concentration and the Sm concentration contained in the main phase 10, the La concentration and the Sm concentration contained in the first subphase 21, and the La concentration and the Sm concentration contained in the second subphase 22 satisfy the above-mentioned formula (1).
[0093] Implementation method 3.
[0094] Next, a rotor on which the rare earth sintered magnet 1 according to the first embodiment is mounted will be described. Figure 6 This is a cross-sectional view schematically showing an example of the structure of a rotor equipped with a rare earth sintered magnet according to Embodiment 3. Figure 6 , a cross section in a direction perpendicular to the rotation axis RA of the rotor 100 is shown.
[0095] The rotor 100 is rotatable about a rotation axis RA. The rotor 100 includes a rotor core 101 and a rare earth sintered magnet 1 inserted into a magnet insertion hole 102 provided in the rotor core 101 along the circumferential direction of the rotor 100. Figure 6 In the embodiment, four rare earth sintered magnets 1 are used, but the number of rare earth sintered magnets 1 is not limited thereto and can be changed according to the design of the rotor 100. Figure 6 , an example is shown in which four magnet insertion holes 102 are provided in the rotor core 101 and four rare earth sintered magnets 1 are inserted into the magnet insertion holes 102, but the number of magnet insertion holes 102 and the number of rare earth sintered magnets 1 can be changed according to the design of the rotor 100. The rotor core 101 is formed by stacking a plurality of disk-shaped electromagnetic steel sheets in the axial direction of the rotation axis RA.
[0096] The rare earth sintered magnet 1 has the structure described in the first embodiment and is manufactured according to the manufacturing method described in the second embodiment. The four rare earth sintered magnets 1 are inserted into the corresponding magnet insertion holes 102. The four rare earth sintered magnets 1 are magnetized in a manner different from that of the adjacent rare earth sintered magnets 1 in the radially outer side of the rotor 100.
[0097] Thus, the rotor 100 according to the third embodiment includes the rare earth sintered magnet 1 according to the first embodiment, which can achieve improvement of magnetic properties at room temperature and suppression of degradation of magnetic properties associated with temperature rise. Thus, since the rare earth sintered magnet 1 can suppress degradation of magnetic properties associated with temperature rise while maintaining high residual magnetic flux density and coercive force, degradation of magnetic properties is suppressed even in a high temperature environment exceeding 100°C. As a result, the operation of the rotor 100 can be stabilized even in a high temperature environment exceeding 100°C.
[0098] Implementation method 4.
[0099] Next, a rotating machine equipped with the rotor 100 according to the fourth embodiment will be described. Figure 7 FIG. 1 is a cross-sectional view schematically showing an example of the structure of a rotating machine according to Embodiment 4. Figure 7 , a cross section in a direction perpendicular to the rotation axis RA of the rotor 100 is shown.
[0100] The rotating machine 120 includes: the rotor 100 described in Embodiment 3, which is rotatable around the rotation axis RA; and an annular stator 130, which is coaxially arranged with the rotor 100 and arranged opposite to the rotor 100. The stator 130 is formed by stacking a plurality of electromagnetic steel sheets in the axial direction of the rotation axis RA. The structure of the stator 130 is not limited to this, and an existing structure can be adopted. As for the stator 130, the tooth portion 131 protruding on the rotor 100 side is arranged along the inner surface of the stator 130. The winding 132 is arranged on the tooth portion 131. The winding method of the winding 132 is not limited to concentrated winding, but can also be distributed winding. The number of magnetic poles of the rotor 100 located in the rotating machine 120 can be more than 2 poles, that is, the number of rare earth sintered magnets 1 can be more than 2. In addition, in Figure 7 In the embodiment, a magnet embedded type rotor 100 is used, but a surface magnet type in which the rare earth sintered magnet 1 is fixed to the outer periphery with an adhesive may be used.
[0101] Thus, the rotating machine 120 according to the fourth embodiment includes the rare earth sintered magnet 1 according to the first embodiment, which can achieve improvement of magnetic properties at room temperature and suppression of reduction of magnetic properties associated with temperature rise. Thus, since the rare earth sintered magnet 1 can suppress reduction of magnetic properties associated with temperature rise while maintaining high residual magnetic flux density and coercive force, reduction of magnetic properties is suppressed even in a high temperature environment exceeding 100°C. As a result, even in a high temperature environment exceeding 100°C, the rotor 100 can be stably driven, and the operation of the rotating machine 120 can be stabilized.
[0102] Example
[0103] The rare earth sintered magnet 1 of the present disclosure will be described in detail below using examples and comparative examples.
[0104] In Examples 1 to 8 and Comparative Examples 1 to 6, a rare earth sintered magnet 1 was manufactured by the method shown in Embodiment 2 using a plurality of samples represented by R-Fe-BMN of rare earth magnet alloys 37 having different compositions of the main phase 10. In the samples according to Examples 1 to 8 and Comparative Examples 1 to 6, the portion of the element R was changed.
[0105] In Examples 1 to 8 and Comparative Examples 5 and 6, the rare earth magnet alloy 37 in which the contents of Nd, La and Sm in the element R were changed was used to produce the rare earth sintered magnet 1. However, in Examples 1 to 7, the rare earth magnet alloy 37 containing no additive element N and to which one or more elements M selected from Cu, Al and Ga were added was used. In addition, in Example 8, the rare earth magnet alloy 37 to which the element M and one or more additive elements N selected from Co, Zr, Ti, Pr, Nb, Dy, Tb, Mn, Gd and Ho were added was used.
[0106] In Comparative Examples 1 and 3, a rare earth magnet alloy 37 in which the element R is Nd is used. However, in Comparative Example 1, the element M and the additive element N are not contained, and in Comparative Example 3, the additive element N is not contained.
[0107] In Comparative Examples 2 and 4, a rare earth magnet alloy 37 in which the element R includes Nd and Dy as a heavy rare earth element is used. However, in Comparative Example 2, the element M and the additive element N are not contained, and in Comparative Example 4, the additive element N is not contained.
[0108] Table 3 is a table showing the general formula of the rare earth sintered magnet according to the examples and comparative examples, the content of the elements constituting the element R, the analysis results of the organizational morphology, and the determination results of the magnetic properties. Table 3 shows the general formula of the main phase 10 of each sample of the rare earth sintered magnet 1 of Examples 1 to 8 and Comparative Examples 1 to 6. In addition, in Table 3, only the presence or absence of addition of the element M and the added element N is shown. It should be noted that in Examples 1 to 8 and Comparative Examples 3 and 4, as the element M, the case where all of Cu, Al, and Ga are included is given as an example.
[0109]
[0110] Next, the method for analyzing the structure of the rare earth sintered magnet 1 of Examples 1 to 8 and Comparative Examples 1 to 6 is described. The structure morphology of the rare earth sintered magnet 1 is determined by elemental analysis using a scanning electron microscope (Scanning Electron Microscope: SEM) and an electron probe micro analyzer (Electron Probe Micro Analyzer: EPMA). Among them, as SEM and EPMA, a field emission electron probe micro analyzer (manufactured by JEOL Ltd., product name: JXA-8530F) is used. As for the conditions of elemental analysis, the acceleration voltage is 15.0 kV, the irradiation current is 22.71 nA, the irradiation time is 130 ms, the number of pixels is 512 pixels × 512 pixels, the magnification is 5000 times, and the number of accumulations is 1 time.
[0111] Next, the evaluation method of the magnetic properties of the rare earth sintered magnet 1 according to Examples 1 to 8 and Comparative Examples 1 to 6 is described. The evaluation of the magnetic properties is performed by measuring the coercive force of a plurality of samples using a pulse excitation type BH tracker. The maximum applied magnetic field using the BH tracker is 6T or more, which makes the rare earth sintered magnet 1 completely magnetized. In addition to the pulse excitation type BH tracker, a DC self-recording fluxmeter, a vibrating sample magnetometer (Vibrating Sample Magnetometer: VSM), a magnetic property measuring device (Magnetic Property Measurement System: MPMS), a physical property measuring device (Physical Property Measurement System: PPMS), etc., which are also called DC type BH trackers, can also be used as long as they can generate a maximum applied magnetic field of 6T or more. The measurement is performed in an atmosphere containing an inert gas such as nitrogen. The magnetic properties of each sample are measured at each temperature of a first measurement temperature T1 and a second measurement temperature T2 that are different from each other. The temperature coefficient α [% / °C] of the residual magnetic flux density is the value obtained by dividing the difference between the residual magnetic flux density at the first measurement temperature T1 and the residual magnetic flux density at the second measurement temperature T2 to the ratio of the residual magnetic flux density at the first measurement temperature T1 by the temperature difference (T2-T1). In addition, the temperature coefficient β [% / °C] of the coercive force is the value obtained by dividing the difference between the coercive force at the first measurement temperature T1 and the coercive force at the second measurement temperature T2 to the ratio of the coercive force at the first measurement temperature T1 by the temperature difference (T2-T1). Therefore, the smaller the absolute values of the temperature coefficients of the magnetic properties |α| and |β|, the more the decrease in the magnetic properties of the magnet due to the increase in temperature is suppressed.
[0112] First, the analysis results of the samples according to Examples 1 to 8 and Comparative Examples 1 to 6 will be described. Figure 8 These are composition images obtained by analyzing the cross sections of the rare earth sintered magnets according to Examples 1 to 8 using a field emission electron probe microanalyzer (FE-EPMA). Figures 9 to 15 The element surface distribution is obtained by analyzing the cross section of the rare earth sintered magnet according to Examples 1 to 8 using FE-EPMA. Fig. 9 is the element surface distribution of Nd, Fig.10 is the element surface distribution of O, Fig.11 is the element surface distribution of La, Fig.12 is the element surface distribution of Sm, Fig.13 is the element surface distribution of Cu, Fig.14 is the element surface distribution of Al, Fig.15 is the element surface distribution of Ga. Figures 9 to 15 for Figure 8 The element surface distribution in the region shown in FIG. 1 is shown in FIG. 1 . In addition, the rare earth sintered magnets 1 according to Examples 1 to 8 all show the same results. Figures 8 to 15 In the embodiment 1 to the embodiment 8, a representative embodiment is shown. Figure 1 The same components are denoted by the same reference numerals.
[0113] like Figures 8 to 12 As shown, in each sample of Examples 1 to 8, it can be confirmed that R2Fe 14 The main phase 10 is a crystal grain having a basic B crystal structure, a crystalline first subphase 21 having an oxide phase represented by (Nd, La, Sm)-O as a main component, and a crystalline second subphase 22 having an oxide phase represented by (Nd, La)-O as a main component. In each of the samples of Examples 1 to 8, Fig.12 As shown in , it can be confirmed that the concentration of Sm in the first subphase 21 is higher than that in the second subphase 22. Figures 13 to 15 As shown in , it can be confirmed that the concentration of one or more elements M selected from Cu, Al, and Ga is higher in the second subphase 22 than in the first subphase 21 .
[0114] In Table 3, the case where the first subphase 21 has a higher Sm concentration than the second subphase 22 is indicated in the item "Sm concentration first subphase>second subphase" of the structure morphology, and the case where the second subphase 22 has a higher element M concentration than the first subphase 21 is indicated in the item "element M concentration first subphase<second subphase" of the structure morphology. For Examples 1 to 8 and Comparative Examples 1 to 6, samples where these conditions could be confirmed are indicated by "○", and samples where these conditions could not be confirmed are indicated by "×".
[0115] In addition, from the intensity ratio of the element surface distribution obtained by the FE-EPMA analysis, it can be confirmed that the sum of the La concentrations in the first subphase 21 and the second subphase 22 is greater than the La concentration in the main phase 10, and the sum of the Sm concentrations in the first subphase 21 and the second subphase 22 is greater than the Sm concentration in the main phase 10. Furthermore, it can also be confirmed that the La concentration in the first subphase 21 is greater than the La concentration in the second subphase 22.
[0116] Among them, by using FE-EPMA to measure the La concentration contained in the main phase 10, the first subphase 21 and the second subphase 22 and the Sm concentration contained in the main phase 10, the first subphase 21 and the second subphase 22, the intensity ratio of the element surface distribution can be confirmed: the relationship between the La concentration contained in the main phase 10, the first subphase 21 and the second subphase 22 and the Sm concentration contained in the main phase 10, the first subphase 21 and the second subphase 22 satisfies the above-mentioned formula (1).
[0117] Next, the measurement results of magnetic properties in each sample according to Examples 1 to 8 and Comparative Examples 1 to 6 are described. The shape of each sample for magnetic measurement is a block with a length, width and height of 7 mm. The first measurement temperature T1 is 23°C, and the second measurement temperature T2 is 200°C. 23°C is room temperature. 200°C is a temperature that can occur as an environment when an automobile motor or an industrial motor is operating.
[0118] First, the residual magnetic flux density and coercive force in each sample according to Examples 1 to 8 and Comparative Examples 2 to 6 were judged in comparison with Comparative Example 1. The residual magnetic flux density and coercive force values of each sample at 23°C were compared with the values in Comparative Example 1, and when the values were within 1% of the measurement error, they were judged as "same", when the values were higher than 1%, they were judged as "good", and when the values were lower than 1%, they were judged as "bad".
[0119] Next, the temperature coefficient α of the residual magnetic flux density was calculated using the residual magnetic flux density at 23°C of the first measurement temperature T1 and the residual magnetic flux density at 200°C of the second measurement temperature T2. In addition, the temperature coefficient β of the coercive force was calculated using the coercive force at 23°C of the first measurement temperature T1 and the coercive force at 200°C of the second measurement temperature T2. The temperature coefficient of the residual magnetic flux density and the temperature coefficient of the coercive force in each sample according to Examples 1 to 8 and Comparative Examples 2 to 6 were determined by comparison with Comparative Example 1. For each sample, when compared with the absolute value of the temperature coefficient of the residual magnetic flux density |α| and the absolute value of the temperature coefficient of the coercive force |β| in the sample according to Comparative Example 1, if a value that can be considered to be within ±1% of the measurement error is shown, it is judged as "same", if a value lower than -1% is shown, it is judged as "good", and if a value higher than +1% is shown, it is judged as "bad". The samples judged as "good" have a smaller temperature coefficient, so that the reduction in magnetic properties accompanying the temperature rise is suppressed and the rare earth sintered magnet 1 having stable magnetic properties even in a high temperature environment can be provided.
[0120] Table 3 shows the results of determination of the above residual magnetic flux density, coercive force, temperature coefficient of residual magnetic flux density, and temperature coefficient of coercive force.
[0121] Comparative Example 1 is a sample of a rare earth sintered magnet 1 produced by the manufacturing method of Embodiment 2 using Nd, Fe and FeB as raw materials so as to form Nd-Fe-B. When the microstructure of the sample is observed by the above method, since Sm is not added, it cannot be confirmed that the first subphase 21 is higher than the second subphase 22 in terms of Sm concentration. Furthermore, since the element M is not added, it cannot be confirmed that the second subphase 22 is higher than the first subphase 21 in terms of element M concentration. In addition, the magnetic properties of the sample were evaluated by the above method, and the residual magnetic flux density was 1.3T and the coercive force was 1000kA / m. The temperature coefficients of the residual magnetic flux density and the coercive force were |α|=0.191% / °C and |β|=0.460% / °C, respectively. These values of Comparative Example 1 were used as references.
[0122] Comparative Example 2 is a sample of a rare earth sintered magnet 1 produced by the manufacturing method of Embodiment 2 using Nd, Dy, Fe and FeB as raw materials in a manner of (Nd, Dy)-Fe-B. When the microstructure of the sample is observed in the above-mentioned method, since Sm is not added, it cannot be confirmed that the first subphase 21 has a higher Sm concentration than the second subphase 22. Furthermore, since the element M is not added, it cannot be confirmed that the second subphase 22 has a higher concentration than the first subphase 21. In addition, the magnetic properties of the sample are evaluated in the above-mentioned method, and the residual magnetic flux density is "poor", the coercive force is "good", the temperature coefficient of the residual magnetic flux density is "same", and the temperature coefficient of the coercive force is "same". This reflects the following results: the coercive force is improved by replacing Dy with a part of Nd, which has a high crystal magnetic anisotropy.
[0123] Comparative Example 3 is a sample of a rare earth sintered magnet 1 produced by the manufacturing method of Embodiment 2 using Nd, Fe and FeB and further element M as raw materials so as to form Nd-Fe-BM. When the microstructure of this sample is observed by the above method, since Sm is not added, it cannot be confirmed that the first subphase 21 is higher than the second subphase 22 in terms of Sm concentration. In addition, although the element M is added, since Sm is not present, the first subphase 21 and the second subphase 22 are not formed, and it cannot be confirmed that the second subphase 22 is higher than the first subphase 21 in terms of element M concentration. The magnetic properties of this sample are evaluated by the above method, and the residual magnetic flux density is "same", the coercive force is "good", the temperature coefficient of the residual magnetic flux density is "same", and the temperature coefficient of the coercive force is "same". This reflects the fact that although the grain boundary is nonmagnetized by the element M and the coercive force is improved, the concentration of Sm and the concentration of the element M in the subphase 20 are not appropriate structural forms due to the absence of La and Sm.
[0124] Comparative Example 4 is a sample of a rare earth sintered magnet 1 produced by the production method of Embodiment 2 using Nd, Dy, Fe and FeB and further element M as raw materials so as to form (Nd, Dy)-Fe-BM. When the microstructure of this sample is observed by the above method, since Sm is not added, it cannot be confirmed that the first subphase 21 is higher than the second subphase 22 in terms of Sm concentration. In addition, although the element M is added, since Sm is not present, the first subphase 21 and the second subphase 22 are not formed, and it cannot be confirmed that the second subphase 22 is higher than the first subphase 21 in terms of element M concentration. In addition, when the magnetic properties of this sample are evaluated by the above method, the residual magnetic flux density is "poor", the coercive force is "good", the temperature coefficient of the residual magnetic flux density is "same", and the temperature coefficient of the coercive force is "same". This formation reflects the following structure: although the coercivity is improved by replacing part of Dy and Nd with high crystal magnetic anisotropy and making the grain boundary nonmagnetic by M, the concentration of Sm and the concentration of element M in the subphase 20 are not appropriate organizational forms due to the absence of La and Sm.
[0125] Comparative Example 5 is a sample of a rare earth sintered magnet 1 produced by the production method of Embodiment 2 using Nd, La, Sm, Fe and FeB as raw materials so as to become (Nd, La, Sm)-Fe-B. When the microstructure of this sample is observed by the above method, although Sm is added, two sub-phases 20, namely the first sub-phase 21 and the second sub-phase 22, cannot be confirmed because M is not added, and the Sm concentration is uniformly dispersed in the main phase 10 and the sub-phase 20. Furthermore, since the two sub-phases 20 do not exist, it cannot be confirmed that the first sub-phase 21 has a higher Sm concentration than the second sub-phase 22. Furthermore, since the element M is not added, it cannot be confirmed that the second sub-phase 22 has a higher concentration than the first sub-phase 21. In addition, when the magnetic properties of this sample are evaluated by the above method, the residual magnetic flux density is "poor", the coercive force is "poor", the temperature coefficient of the residual magnetic flux density is "good", and the temperature coefficient of the coercive force is "good". This reflects the following results: since La and Sm exist in the main phase 10 or the subphase 20, the temperature coefficient of the magnetic properties shows good results, but the two subphases 20 do not exist, and the concentration of Sm and the concentration of element M in these subphases 20 are not appropriate organizational forms.
[0126] Comparative Example 6 is a sample of a rare earth sintered magnet 1 produced by the production method of Embodiment 2 using Nd, La, Sm, Fe and FeB and one or more additional elements N selected from Co, Zr, Ti, Pr, Nb, Dy, Tb, Mn, Gd and Ho as raw materials so as to become (Nd, La, Sm)-Fe-BN. When the microstructure of this sample is observed by the above method, although Sm is added, since the element M is not added, two types of sub-phases 20, namely the first sub-phase 21 and the second sub-phase 22, cannot be confirmed, and the Sm concentration is uniformly dispersed in the main phase 10 and the sub-phase 20. Furthermore, since the two types of sub-phases 20 do not exist, it cannot be confirmed that the first sub-phase 21 has a higher Sm concentration than the second sub-phase 22. Furthermore, since the element M is not added, it cannot be confirmed that the second sub-phase 22 has a higher concentration than the first sub-phase 21. In addition, the magnetic properties of the sample were evaluated according to the above method, and the residual magnetic flux density was "good", the coercive force was "poor", the temperature coefficient of the residual magnetic flux density was "good", and the temperature coefficient of the coercive force was "good". Since La and Sm exist in the main phase 10 or the sub-phase 20, the temperature coefficient of the magnetic properties shows a good result. In addition, due to the effect of adding elements N such as Co as a magnetic body, the magnetic flux density is improved. However, the formation reflects the following results: the two sub-phases 20 do not exist, and the concentration of Sm and the concentration of element M in these sub-phases 20 are not appropriate organizational forms.
[0127] Examples 1 to 7 are samples of rare earth sintered magnets 1 produced by the production method of Embodiment 2 using Nd, La, Sm, Fe and FeB and element M as raw materials so as to form (Nd, La, Sm)-Fe-BM. When the microstructure of the samples is observed by the above method, it can be confirmed that the first subphase 21 has a higher concentration of Sm than the second subphase 22. Furthermore, it can be confirmed that the second subphase 22 has a higher concentration of element M than the first subphase 21. In addition, the magnetic properties of these samples were evaluated by the above method, and the residual magnetic flux density was "good", the coercive force was "good", the temperature coefficient of the residual magnetic flux density was "good", and the temperature coefficient of the coercive force was "good".
[0128] In Example 8, a sample of a rare earth sintered magnet 1 was produced according to the manufacturing method of Embodiment 2 using Nd, La, Sm, Fe and FeB, element M, and further adding element N as raw materials in a manner of forming (Nd, La, Sm)-Fe-BMN. If the organizational morphology of the sample is observed according to the above method, it can be confirmed that the first subphase 21 has a higher concentration of Sm than the second subphase 22. Furthermore, it can be confirmed that the second subphase 22 has a higher concentration of element M than the first subphase 21. In addition, the magnetic properties of these samples were evaluated according to the above method, and the residual magnetic flux density was "good", the coercive force was "good", the temperature coefficient of the residual magnetic flux density was "good", and the temperature characteristic of the coercive force was evaluated as "good". This means that as long as an appropriate organizational morphology can be formed, the effect obtained will not change even if the additional element N is added.
[0129] The samples of Examples 1 to 8 are rare earth sintered magnets 1 satisfying the general formula (Nd, La, Sm)-Fe-BM, and having: 14 The main phase 10 is a crystal grain having a basic B crystal structure, the crystalline first subphase 21 mainly composed of an oxide phase represented by (Nd, La, Sm)-O, and the crystalline second subphase 22 mainly composed of an oxide phase represented by (Nd, La)-O. As described above, the rare earth sintered magnets 1 of Examples 1 to 8 are characterized in that the first subphase 21 has a higher Sm concentration than the second subphase 22, and the second subphase 22 has a higher element M concentration than the first subphase 21. As a result, these rare earth sintered magnets 1 can suppress the use of Nd and heavy rare earth elements that are expensive, highly uneven in region, and have procurement risks, as compared to rare earth sintered magnets that satisfy Nd-Fe-B, and can achieve improvement in magnetic properties at room temperature and suppression of reduction in magnetic properties associated with temperature rise.
[0130] The configurations shown in the above embodiments are merely examples, and may be combined with other known technologies, or the embodiments may be combined with each other. Part of the configuration may be omitted or changed without departing from the spirit and scope of the invention.
[0131] Description of Reference Numerals
[0132] 1 rare earth sintered magnet, 10 main phase, 20 auxiliary phase, 21 first auxiliary phase, 22 second auxiliary phase, 31 crucible, 32 alloy melt, 33 tundish, 34 single roller, 35 solidified alloy, 36 tray container, 37 rare earth magnet alloy, 100 rotor, 101 rotor core, 102 magnet insertion hole, 120 rotating machine, 130 stator, 131 tooth portion, 132 winding.
Claims
1. A rare earth sintered magnet, wherein the element M is one or more elements selected from Cu, Al and Ga and satisfies the general formula (Nd, La, Sm)-Fe-BM, characterized in that: have: Contains R2Fe 14 B crystal structure is the main phase of the basic grain; a crystalline first subphase mainly composed of an oxide phase represented by (Nd, La, Sm)-O; and A crystalline second subphase mainly composed of an oxide phase represented by (Nd, La)—O, R is Nd, La and Sm, The concentration of Sm segregated in the crystalline subphase composed of the first subphase and the second subphase is higher than the concentration of Sm in the main phase, and the concentration of Sm in the first subphase is higher than the concentration of Sm in the second subphase. The concentration of the element M in the second subphase is higher than the concentration of the element M in the first subphase.
2. The rare earth sintered magnet according to claim 1, characterized in that: The sum of the La concentrations in the first subphase and the second subphase is equal to or greater than the La concentration in the main phase, The sum of the concentrations of Sm in the first subphase and the second subphase is equal to or higher than the concentration of Sm in the main phase.
3. The rare earth sintered magnet according to claim 1 or 2, characterized in that: The concentration of La in the first subphase is equal to or higher than the concentration of La in the second subphase.
4. The rare earth sintered magnet according to claim 1 or 2, characterized in that: When the composition ratios of Nd, La, and Sm are represented by a, b, and c, respectively, a>(b+c).
5. The rare earth sintered magnet according to claim 1 or 2, characterized in that: When the La concentration contained in the main phase is set to X, the La concentration contained in the first subphase is set to X1, the La concentration contained in the second subphase is set to X2, the Sm concentration contained in the main phase is set to Y, the Sm concentration contained in the first subphase is set to Y1, and the Sm concentration contained in the second subphase is set to Y2, 1<(Y1+Y2) / Y<(X1+X2) / X.
6. The rare earth sintered magnet according to claim 1 or 2, characterized in that: It further contains one or more additional elements N selected from the group consisting of Co, Zr, Ti, Pr, Nb, Dy, Tb, Mn, Gd and Ho.
7. A method for producing a rare earth sintered magnet, the method for producing a rare earth sintered magnet according to any one of claims 1 to 6, characterized in that: include: A melting step of melting a raw material of a rare earth magnet alloy containing elements constituting the rare earth sintered magnet; A first cooling step of cooling the raw material in a molten state in the melting step to obtain a solidified alloy; A second cooling step of further cooling the solidified alloy to obtain a rare earth magnet alloy; A pulverizing step of pulverizing the rare earth magnet alloy satisfying (Nd, La, Sm)-Fe-BM to obtain a powder of the rare earth magnet alloy; A molding step of preparing a molded body by molding the powder of the rare earth magnet alloy; A sintering step of preparing a sintered body by maintaining the molded body at a sintering temperature in a range of 900° C. to 1300° C. for a time in a range of 0.1 hour to 10 hours; The sintered body is subjected to a first aging step of maintaining the sintered body at a first aging temperature in a range of 700° C. to 900° C., which is lower than the sintering temperature, for a period of 0.1 hour to 10 hours. A second aging step of maintaining the sintered body maintained in the first aging step at a second aging temperature lower than the first aging temperature, that is, in the range of 450° C. to less than 700° C., for a period of 0.1 hour to 10 hours; and A cooling step of holding the sintered body held in the second aging step at a temperature lower than the second aging temperature, that is, in a range of 200° C. to less than 450° C., for a period of 0.1 hour to 5 hours.
8. A rotor, characterized in that: include: Rotor core; and The rare earth sintered magnet according to any one of claims 1 to 6 provided in the rotor core.
9. A rotating machine, characterized in that: have: The rotor as claimed in claim 8; and An annular stator is arranged to face the rotor, and the annular stator has a winding disposed on a tooth portion, and the tooth portion protrudes toward the rotor on an inner surface of a side where the rotor is arranged.