A preparation method of PUR hot melt adhesive for binding

By adding PBAT, corn starch and eucalyptus essential oil to PUR hot melt adhesive, and using ε-caprolactone and 1,4-butane diisocyanate to react to synthesize isocyanate-terminated polyester, combined with microprocessor control of argon atmosphere, to solve the problem The problems of biodegradability and moisture resistance of PUR hot melt adhesive for binding have been solved, and an environmentally friendly binding adhesive has been realized.

CN117757404BActive Publication Date: 2024-10-22GUANGZHOU JIAYAN ADHESIVE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311773528.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-22
Publication Date
2024-10-22
Estimated Expiration
2043-12-22

AI Technical Summary

Technical Problem

The existing PUR hot-melt adhesive used for binding lacks biodegradability and moisture and insect repellent properties. It is difficult to naturally degrade in the environment and is easily degummed by moisture and attacked by insects.

Method used

PUR hot melt adhesive is prepared by adding PBAT, corn starch and eucalyptus essential oil to the polymer, mixing and stirring evenly under vacuum conditions, and using ε-caprolactone, 1,4-butane diisocyanate and 1,4-butanediol to react. Isocyanate-terminated polyester is synthesized and microprocessor-controlled argon atmosphere makes it biodegradable and insect repellent.

Benefits of technology

The prepared PUR hot melt adhesive is biodegradable, and the degradation products are non-toxic. It has enhanced viscosity and moisture resistance, effectively prevents insect invasion, and reduces environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004621891500000091
    Figure BDA0004621891500000091
  • Figure BDA0004621891500000101
    Figure BDA0004621891500000101
  • Figure BDA0004621891500000121
    Figure BDA0004621891500000121
Patent Text Reader

Abstract

The invention discloses a method for preparing a PUR hot melt adhesive for bookbinding, which belongs to the technical field of adhesives. The method comprises adding PBAT (polybutylene terephthalate-adipate), corn starch and eucalyptus essential oil to a polymer, mixing and stirring uniformly under vacuum conditions to obtain a PUR hot melt adhesive for bookbinding, wherein the raw materials for preparation include 50-65 parts of polymer, 30-40 parts of PBAT, 2-5 parts of corn starch, and 6-8 parts of eucalyptus essential oil in parts by mass. The PUR hot melt adhesive prepared by the method for preparing a PUR hot melt adhesive for bookbinding is biodegradable, green and environmentally friendly, safe, environmentally friendly, in line with the national environmental strategy, and can resist moisture and repel insects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, in particular to a method for preparing a PUR hot melt adhesive for bookbinding. Background Art

[0002] PUR hot melt adhesive is widely used in bookbinding because it does not use any solvent in production and use, is non-toxic, odorless, and does not pollute the environment. In recent years, with the increasing awareness of environmental protection, more and more companies have begun to pay attention to the research and application of degradable materials. Bio-paper and other materials that can be naturally degraded in nature are promoted by the national government, but books after binding are susceptible to moisture and degumming and falling pages, and are susceptible to insect attacks. A kind of PUR hot melt adhesive for bookbinding prepared by the present invention fully considers the particularity of bookbinding, enhances the waterproof and insect repellent of PUR hot melt adhesive, is not easy to be affected by climate and environment during storage and transportation, and can also protect paper from insect attacks. Usually, polyurethane is made by reacting polyols with diisocyanates and then extending the chain with diols. Commonly used polyurethanes are based on aromatic diisocyanates. However, due to the toxic degradation products derived from aromatic hard segments, these products lack biodegradability. The hard segment based on 1,4-butane diisocyanate (BDI) may be a good non-toxic alternative because the degradation product 1,4-butanediamine putrescine is a non-toxic diamine, and the reaction of ε-caprolactone, 1,4-butane diisocyanate (BDI) and 1,4-butanediol (BDO) does not require a catalyst and is biodegradable, which is in line with the national environmental strategy and is green and environmentally friendly. When combined with biodegradable paper, it can greatly reduce pollution to the environment. Summary of the invention

[0003] The purpose of the present invention is to solve the problem that the PUR hot melt adhesive prepared by the prior art preparation method for PUR hot melt adhesive for binding does not have both biodegradability and moisture resistance and insect repellency, and to propose a preparation method for PUR hot melt adhesive for binding.

[0004] In the first aspect of the present invention, the present invention proposes a method for preparing a PUR hot melt adhesive for binding, wherein PBAT (polybutylene terephthalate-adipate), corn starch and eucalyptus essential oil are added to a polymer, and the mixture is mixed and stirred evenly under vacuum conditions to obtain a PUR hot melt adhesive for binding.

[0005] Furthermore, the PUR hot melt adhesive raw material for bookbinding includes, by weight, 50-65 parts of polymer, 15-20 parts of PBAT, 2-5 parts of corn starch and 6-8 parts of eucalyptus essential oil.

[0006] Furthermore, the polymer raw material includes, by weight: 25-30 parts of ε-caprolactone, 7-9 parts of BDI (1,4-butane diisocyanate) and 3-4 parts of BDO.

[0007] Furthermore, in the preparation method of the PUR hot melt adhesive for bookbinding, the mass ratio of ε-caprolactone, BDI and PBAT is (25-30): (7-9): (15-20).

[0008] Furthermore, the mass ratio of ε-caprolactone, BDI, PBAT and eucalyptus essential oil is (25-30):(7-9):(15-20):(6-8).

[0009] Further, the polymer is prepared by the following steps:

[0010] (1) heating ε-caprolactone to 100-120° C., dehydrating under vacuum conditions, adding the mixture to a reaction kettle, heating the mixture to 150° C., adding BDO, stirring the mixture under an argon atmosphere, and reacting the mixture for 7 days to obtain poly(ε-caprolactone) diol;

[0011] (2) poly(ε-caprolactone) diol and BDI (1,4-butane diisocyanate) were stirred and reacted under an argon atmosphere, with a vacuum degree of ≤0.095 MPa, and reacted at 80° C. for 4 hours, and then poly(ε-caprolactone) diol and BDI (1,4-butane diisocyanate) were added, and stirred and reacted under an argon atmosphere, and reacted at 80° C. for 4 hours to obtain an isocyanate-terminated polyester;

[0012] (3) The isocyanate-terminated polyester was reacted with BDO, and the reaction was stirred under an argon atmosphere at 80° C. for 72 hours to obtain a polymer.

[0013] Furthermore, the mass fraction of ε-caprolactone in step (1) is 25-30 parts.

[0014] Furthermore, in the step (2), the mass fraction of BDI (1,4-butane diisocyanate) is 8-10 parts; and the vacuum degree of the stirring reaction under argon atmosphere is ≤0.095 MPa.

[0015] Furthermore, the reaction temperature of the isocyanate-terminated polyester and 1,4-butanediol is 80°C.

[0016] Furthermore, the method further includes controlling the maintenance of the argon atmosphere, and the specific steps are:

[0017] S1: setting a microprocessor, an argon blowing device and an online detector; the microprocessor is connected to the argon blowing device and the online detector respectively; the online detector is used to detect the content value of the preset component contained in the product in the reactor in real time, and send the content value to the microprocessor; the argon blowing device is used to generate argon gas; the microprocessor is used to control the argon blowing flow rate and opening and closing degree of the argon blowing device;

[0018] S2: The microprocessor obtains the content value of the preset component contained in the product sent by the online detector; inputs the content value into the preset neural network probability prediction model to obtain the probability value that the content value reaches the preset content threshold value, and generates a control signal if the probability value is greater than the preset probability threshold value;

[0019] S3: based on a preset matching relationship library between the content value and the standard value of the argon blowing flow rate, obtaining the standard value of the argon blowing flow rate; and according to the initial value of the argon blowing flow rate, obtaining the difference between the standard value of the argon blowing flow rate and the initial value of the argon blowing flow rate;

[0020] S4: According to the control signal, the argon blowing equipment is controlled to supplement the argon blowing flow rate and adjust the opening and closing degree according to the difference; the supplementation includes: according to the reaction time in step (1), or step (2) and or step (3), supplementing according to the fixed division period of the back pressure time or supplementing according to the random division period of the back pressure time; the opening and closing degree adjustment includes: according to the size of the difference and the reaction time, adjusting according to the preset adjustment amplitude value and adjustment frequency; the larger the difference and the longer the reaction time, the larger the adjustment amplitude value and the higher the adjustment frequency.

[0021] The present invention provides a method for preparing a PUR hot melt adhesive for bookbinding, which has the following beneficial effects:

[0022] 1. ε-caprolactone, BDI, BDO, PBAT, corn starch and eucalyptus essential oil are biodegradable materials with little impact on the environment;

[0023] 2. 1,4-Butane diisocyanate has a non-toxic biodegradable product, 1,4-butanediamine, which is green and environmentally friendly with little impact on the environment;

[0024] 3. Use a two-step method to synthesize isocyanate-terminated polyester, broaden the molecular weight distribution, increase the molecular weight of PUR, enhance the viscosity, and make the reaction more complete;

[0025] 4. PBAT is a thermoplastic biodegradable material, which is green and environmentally friendly, and has good ductility, elongation at break, heat resistance and impact resistance. PBAT is a copolymer of aliphatic and aromatic polyesters, which combines the excellent degradation properties of aliphatic polyesters and the good mechanical properties of aromatic polyesters.

[0026] 5. Eucalyptus essential oil is a natural high antioxidant and insect repellent. Ants like to gnaw on books, and adding eucalyptus essential oil can prevent insects from invading.

[0027] 6. No catalyst is needed to synthesize polyurethane by reacting ε-caprolactone, BDO and BDI, which reduces the impact of catalyst on the environment and increases the biodegradation rate of hot melt adhesive;

[0028] 7. By setting up a microprocessor, argon blowing equipment and online detector, the argon atmosphere can be accurately controlled in real time, which can provide stable argon atmosphere conditions, ensure the reaction standards of the reactants, and improve the preparation quality of the polymer. DETAILED DESCRIPTION

[0029] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0030] Unless otherwise specified, the examples and comparative examples are parallel tests with the same components, component contents, preparation steps and preparation parameters. The experimental methods in the following examples are conventional methods unless otherwise specified. The experimental materials used in the following examples are purchased from commercial channels unless otherwise specified.

[0031] The sources of materials mentioned in the present invention are as follows:

[0032] ε-Caprolactone was purchased from aladdin (model C109521), bio-paper was purchased from Weifang Sanmu Paper Products Factory, BDI was purchased from Sigma-Aldrich, BDO (1,4-butanediol) model: B110395, purchased from aladdin, corn starch was purchased from Jinan Haiwei Chemical Co., Ltd., PBAT was purchased from Shanghai Jujia Plastic Raw Materials Co., Ltd., catalyst bismuth laurate was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., and eucalyptus essential oil was purchased from Jiangxi Yuanshangcao Spice Co., Ltd.

[0033] In the preparation examples and embodiments of the present invention, the "parts" are parts by weight unless otherwise specified.

[0034] Example 1

[0035] Step 1: Preparation of polymer

[0036] (1) heating 29 parts of ε-caprolactone to 100-120° C., dehydrating under vacuum conditions, adding to a reaction kettle, heating to 150° C., adding 1.7 parts of BDO, and reacting for 7 days under an argon atmosphere with a vacuum degree of 0.095 MPa to obtain poly(ε-caprolactone) diol;

[0037] (2) 16.8 parts of poly(ε-caprolactone) diol and 5.6 parts of BDI were reacted at 80°C for 4 hours under an argon atmosphere with a vacuum degree of 0.095 MPa, and then 5.6 parts of poly(ε-caprolactone) diol and 3 parts of BDI were added and reacted at 80°C for 4 hours under an argon atmosphere with a vacuum degree of 0.095 MPa to obtain an isocyanate-terminated polyester;

[0038] (3) 30 parts of isocyanate-terminated polyester was reacted with 1.5 parts of BDO under an argon atmosphere with a vacuum degree of 0.095 MPa at 80° C. for 72 hours to obtain a polymer.

[0039] Step 2: Preparation of PUR hot melt adhesive for binding

[0040] 65 parts of polymer were added to 20 parts of PBAT, 5 parts of corn starch and 8 parts of eucalyptus essential oil, stirred evenly at a temperature of 25° C. and a vacuum degree of 0.095 MPa, and dehydrated for 3 hours to obtain a PUR hot melt adhesive for binding.

[0041] Example 2

[0042] Step 1: Preparation of polymer

[0043] (1) heating 25 parts of ε-caprolactone to 100-120° C., dehydrating under vacuum conditions, adding to a reaction kettle, heating to 150° C., adding 1.5 parts of BDO, and reacting for 7 days under an argon atmosphere with a vacuum degree of 0.095 MPa to obtain poly(ε-caprolactone) diol;

[0044] (2) 16.8 parts of poly(ε-caprolactone) diol and 5 parts of BDI were reacted at 80°C for 4 hours under an argon atmosphere with a vacuum degree of 0.095 MPa, and then 5.6 parts of poly(ε-caprolactone) diol and 3 parts of BDI were added and reacted at 80°C for 4 hours under an argon atmosphere with a vacuum degree of 0.095 MPa to obtain an isocyanate-terminated polyester;

[0045] (3) 30 parts of isocyanate-terminated polyester was reacted with 1.5 parts of BDO under an argon atmosphere with a vacuum degree of 0.095 MPa at 80° C. for 72 hours to obtain a polymer.

[0046] Step 2: Preparation of PUR hot melt adhesive for binding

[0047] 50 parts of polymer were added to 15 parts of PBAT, 2 parts of corn starch and 6 parts of eucalyptus essential oil, stirred evenly at a temperature of 25° C. and a vacuum degree of 0.095 MPa, and dehydrated for 3 hours to obtain a PUR hot melt adhesive for binding.

[0048] Example 3

[0049] Step 1: Preparation of polymer

[0050] (1) heating 30 parts of ε-caprolactone to 100-120° C., dehydrating under vacuum conditions, adding to a reaction kettle, heating to 150° C., adding 2.5 parts of BDO, and reacting for 7 days under an argon atmosphere with a vacuum degree of 0.095 MPa to obtain poly(ε-caprolactone) diol;

[0051] (2) 16.8 parts of poly(ε-caprolactone) diol and 7 parts of BDI were reacted at 80° C. for 4 hours under an argon atmosphere with a vacuum degree of 0.095 MPa, and then 5.6 parts of poly(ε-caprolactone) diol and 3 parts of BDI were added and reacted at 80° C. for 4 hours under an argon atmosphere with a vacuum degree of 0.095 MPa to obtain an isocyanate-terminated polyester;

[0052] (3) 30 parts of isocyanate-terminated polyester was reacted with 1.5 parts of BDO under an argon atmosphere with a vacuum degree of 0.095 MPa at 80° C. for 72 hours to obtain a polymer.

[0053] Step 2: Preparation of PUR hot melt adhesive for binding

[0054] 50 parts of polymer were added to 15 parts of PBAT, 2 parts of corn starch and 7 parts of eucalyptus essential oil, stirred evenly at a temperature of 25° C. and a vacuum degree of 0.095 MPa, and dehydrated for 3 hours to obtain a PUR hot melt adhesive for bookbinding.

[0055] The difference between Comparative Example 1 and Example 1 is that no eucalyptus essential oil is added in step 2 of Comparative Example 1.

[0056] The difference between Comparative Example 2 and Example 1 is that in step 1 (2) of Comparative Example 2, 22.4 parts of poly(ε-caprolactone) diol and 8.6 parts of BDI are reacted at 80°C for 8 hours under an argon atmosphere with a vacuum degree of 0.095 MPa to obtain an isocyanate-terminated polyester; Comparative Example 2 does not synthesize the isocyanate-terminated polyester in two steps.

[0057] The difference between Comparative Example 3 and Example 1 is that the reactant used in step 1 of Comparative Example 3 is the same molar number of lysine ethyl diisocyanate (LDI).

[0058] The difference between Comparative Example 4 and Example 1 is that the reactant used in step 1 of Comparative Example 4 is the same molar number of dicyclohexylmethane diisocyanate (HMDI).

[0059] The difference between Comparative Example 5 and Example 1 is that in step 1 (2) of Comparative Example 5, 5.6 parts of poly(ε-caprolactone) diol and 3 parts of BDI are reacted at 80° C. for 4 hours under an argon atmosphere with a vacuum degree of 0.095 MPa, and then 16.8 parts of poly(ε-caprolactone) diol and 5.6 parts of BDI are added, and the reaction is carried out at 80° C. for 4 hours under an argon atmosphere with a vacuum degree of 0.095 MPa to obtain an isocyanate-terminated polyester;

[0060] The difference between Comparative Example 6 and Example 1 is that 0.1 parts of bismuth laurate is added as a catalyst in step 1 (2) of Comparative Example 6.

[0061] Performance Testing

[0062] 1. Moisture resistance test

[0063] The polyurethane hot melt adhesive obtained in the above examples and comparative examples was heated to 140°C to melt, and a manual glue gun was used to dispense glue on the surface of the substrate to prepare PC-PP water vapor transmission rate test samples. The glue thickness was 0.8 mm and the cutting area was 5*5 cm 2 After curing for 7 days at 25±1℃, 65±5RH%, the corresponding water vapor transmission rate test was carried out.

[0064] The water vapor transmission rate of Examples 1-5 of the present invention was tested according to GB1037-2021, and the performance is shown in Table 1:

[0065] Table 1

[0066]

[0067]

[0068] It can be seen from Table 1 that Example 1 has the lowest water vapor permeability. In Comparative Example 1, eucalyptus essential oil is not added. The volatile components in eucalyptus essential oil can improve the surface tension of the colloid, thereby improving the moisture resistance of the adhesive; in Comparative Example 2, the isocyanate-terminated polyester is synthesized in one step, which reduces the molecular weight distribution and reduces the moisture resistance of the PUR hot melt adhesive; in Comparative Example 3, the reactant is LDI, and the LDI side group contains a hydrolyzable ester bond, which will reduce the moisture resistance of the PUR hot melt adhesive; in Comparative Example 4, the reactant is HMDI, and the cyclohexane in HMDI affects the flexibility of the polymer chain and reduces the moisture resistance of the PUR hot melt adhesive; in Comparative Example 5, the reactant with a small mass is synthesized in the first step reaction, so there is no sufficient reactant and the second step reaction, the reaction is not sufficient, and the molecular width of the obtained isocyanate-terminated polyester is narrow, which reduces the moisture resistance of the PUR hot melt adhesive.

[0069] 2. Biodegradation test

[0070] The polyurethane hot melt adhesive obtained in the above examples and comparative examples was heated to 140°C to melt, and a manual glue gun was used to dispense glue on the paper surface to prepare biodegradable test samples. The glue thickness was 0.8 mm and the cutting area was 5*5 cm. 2 After curing for 7 days at 25±1℃, 65±5RH%, the composting method was used to study the biodegradability. The cut samples were buried in an alluvial soil box obtained from the topsoil of farmland to keep the soil moist. The sample burial depth was 10-15 cm. Samples were taken once at intervals, and three samples were taken each time. The samples were cleaned with distilled water, dried in a vacuum oven at 35±2℃, weighed, and the average weight loss rate was calculated. The final results are shown in Table 2.

[0071] Table 2 Results of the average weight loss rate (%) of biodegradable tapes

[0072] Group 10d 30d 60d 120d Example 1 9.7 28.4 52.6 82.4 Example 2 9.2 25.7 49.8 79.2 Example 3 9.5 26.1 50.2 80.1 Comparative Example 1 9.8 27.2 51.2 81.3 Comparative Example 2 9.6 28.6 49.2 79.6 Comparative Example 3 7.3 14.5 32.4 52.3 Comparative Example 4 8.1 14.9 33.1 54.8 Comparative Example 5 9.1 26.3 51.8 78.9 Comparative Example 6 8.4 24.3 48.7 74.2

[0073] It can be seen from the experimental results that the biodegradability of Example 1 is the best at 120 days. Since the reactants of Comparative Examples 3 and 4 are not BDI, they cannot generate non-toxic biodegradable products; Comparative Example 5 does not react fully, and the remaining reactants affect the biodegradation rate; Comparative Example 6 adds a catalyst, which reduces the biodegradation rate.

[0074] 3. Mechanical properties test

[0075] The polyurethane hot melt adhesive obtained in the above examples and comparative examples was heated to 140°C to melt, and a manual glue gun was used to dispense glue on the surface of the substrate to prepare PC-PP test samples. The glue thickness was 0.8 mm and the cutting area was 5*5 cm. 2 , after curing for 7 days at 25±1℃, 65±5RH%, the corresponding tests were carried out.

[0076] Shear strength is tested according to GB / T7124-2008. Shear strength I is the test result after 10 minutes of curing, which indicates the magnitude of initial adhesion; shear strength II is the final bonding strength after 5 days of curing. The final results are shown in Table 3.

[0077] The elongation at break was tested according to GB / T528-2009. The final results are shown in Table 3.

[0078] Table 3

[0079]

[0080]

[0081] It can be seen from Table 3 that Example 1 has the best shear strength and elongation at break. In Comparative Example 1, eucalyptus essential oil is not added, and the elongation at break is reduced; in Comparative Example 2, the polymer is synthesized in one step, the molecular weight distribution is reduced, and the shear strength of the PUR hot melt adhesive is reduced; in Comparative Example 3, the reactant is LDI, and the LDI side group contains a hydrolyzable ester bond, which will reduce the shear strength of the PUR hot melt adhesive; in Comparative Example 4, the reactant is HMDI, and the cyclohexane in HMDI affects the flexibility of the polymer chain, and the shear strength of the PUR hot melt adhesive is enhanced, but the elongation at break is reduced; in Comparative Example 5, the reactant with a small mass is synthesized in the first step reaction, and there is no sufficient reactant and second step reaction, the reaction is insufficient, and the shear strength and elongation at break of the PUR hot melt adhesive are reduced.

[0082] 4. Anti-insect test

[0083] The polyurethane hot melt adhesive obtained in the above examples and comparative examples was heated to 140°C and melted. A manual glue gun was used to dispense glue on the paper surface to prepare a biodegradable test sample. The glue thickness was 0.8 mm. A 10 cm × 10 cm × 10 cm box was prepared. Candies were then added to the box, and holes were opened on the surface of the box. Then 200 ants were added to the outside of the box. After two hours, the number of ants in the box was recorded and the average value was taken. The test data is shown in Table 4.

[0084] Table 4

[0085]

[0086]

[0087] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing PUR hot melt adhesive for bookbinding, characterized in that: Polybutylene terephthalate-adipate, corn starch and eucalyptus essential oil are added to the polymer, and the mixture is uniformly stirred under vacuum to obtain a PUR hot melt adhesive for bookbinding; The raw materials for preparing the PUR hot melt adhesive for bookbinding include, in parts by mass: 50-65 parts of polymer, 15-20 parts of polybutylene terephthalate-adipate, 2-5 parts of corn starch and 6-8 parts of eucalyptus essential oil; the raw materials for preparing the polymer include, in parts by mass: 25-30 parts of ε-caprolactone, 7-9 parts of 1,4-butane diisocyanate and 3-4 parts of 1,4-butanediol; the polymer is prepared by the following steps: (1) ε-caprolactone is heated to 100-120°C, dehydrated under vacuum conditions, and then added to a reaction kettle, heated to 150°C, and BDO is added. The mixture is stirred and reacted under an argon atmosphere for 7 days to obtain poly(ε-caprolactone) diol; (2) poly(ε-caprolactone) diol and 1,4-butane diisocyanate were stirred and reacted under an argon atmosphere with a vacuum degree of ≤0.095 MPa at 80°C for 4 hours, and then poly(ε-caprolactone) diol and 1,4-butane diisocyanate were added and stirred and reacted under an argon atmosphere at 80°C for 4 hours to obtain an isocyanate-terminated polyester; (3) The isocyanate-terminated polyester was reacted with BDO under stirring in an argon atmosphere at 80° C. for 72 hours to obtain a polymer.

2. The method for preparing PUR hot melt adhesive for bookbinding according to claim 1, characterized in that: The mass ratio of ε-caprolactone, 1,4-butane diisocyanate and polybutylene terephthalate-adipate is (25-30): (7-9): (15-20).

3. The method for preparing PUR hot melt adhesive for bookbinding according to claim 1 or 2, characterized in that: The mass ratio of the ε-caprolactone, 1,4-butane diisocyanate, polybutylene terephthalate-adipate and eucalyptus essential oil is (25-30): (7-9): (15-20): (6-8).

4. The method for preparing PUR hot melt adhesive for bookbinding according to claim 1, characterized in that: The vacuum degree of the stirring reaction under argon atmosphere is ≤0.095MPa.

5. The method for preparing PUR hot melt adhesive for bookbinding according to claim 1, characterized in that: The reaction temperature of the isocyanate-terminated polyester and 1,4-butanediol is 80°C.