A high temperature resistant cast aluminum alloy and its preparation method and application
By introducing specific element composition and microstructure design into aluminum alloys, combined with heat treatment technology, the problem of insufficient performance of existing cast heat-resistant aluminum alloys in high-temperature environments has been solved, and its high-temperature tensile strength has been significantly improved to meet the needs of automobile engines. high temperature performance requirements.
Patent Information
- Application Number
- CN202311742584.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-18
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-12-18
AI Technical Summary
Existing cast heat-resistant aluminum-silicon alloys cannot meet the growing high-temperature performance requirements of automobile engines in high-temperature environments. They have problems such as poor thermal stability, difficulty in balancing casting performance and mechanical properties, and incompatibility between room temperature and high-temperature properties.
Using Si 1%-10%, Cu 0.1%-4%, Mg 0.05%-0.5%, Fe 0.05%-0.3%, Ti 0.01%-0.3%, Mn 0.1%-0.5%, Cr 0.01%-0.6%, V 0.02%-0.2%, Sn 0.02%-0.2%, Sc High-temperature-resistant cast aluminum alloys composed of 0.02%-0.2%, Hf 0.02%-0.2%, Er 0.02%-0.2% and other elements are formed by introducing submicron and nanometer precipitated phases, combined with solid solution heat treatment and aging treatment, to form alloys with The coherent or semi-coherent relationship of the matrix improves the high-temperature tensile properties.
It significantly improves the tensile strength of aluminum alloy at high temperatures, meets the high-temperature performance requirements in the automotive engineering field, and ensures that the tensile strength of aluminum alloy at 200°C, 300°C and 400°C is greater than 250MPa, 129MPa and 85MPa respectively.
Smart Images

Figure CN117758110B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of aluminum alloys, and in particular relates to a high temperature resistant casting aluminum alloy and a preparation method and application thereof. Background Art
[0002] Cast aluminum silicon alloys have attracted widespread attention due to their low density, high specific strength, good casting performance and excellent comprehensive performance. They have been used in industries such as ships, machinery, aviation, aerospace, weapons and automobiles, especially in the preparation and production of parts such as pistons, cylinder blocks, cylinder liners and connecting rods of automobile engines. However, driven by the improvement of engine efficiency and emission standards, the engine needs to further increase the combustion pressure, which means that the operating temperature of the engine will be higher than 250°C. The existing cast heat-resistant aluminum silicon alloys are increasingly unable to meet the growing high-temperature performance requirements of automobile engines.
[0003] There are several major problems that are difficult to solve in high temperature resistant cast aluminum alloys: First, there are a large number of precipitates with poor thermal stability in the existing alloy structure. These phases will gradually grow and lose their precipitation strengthening effect at high temperatures. It is difficult to control the structure to inhibit the large-scale appearance of these precipitates; second, it is difficult to balance the casting performance and mechanical properties of the alloy; third, it is difficult to balance the room temperature performance and high temperature performance of the alloy. Therefore, developing or optimizing a cast heat-resistant aluminum alloy so that the alloy can be used normally in a high temperature environment is a key issue that needs to be solved urgently. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a high temperature resistant cast aluminum alloy and a preparation method and application thereof, which significantly improve the mechanical properties of the cast aluminum alloy at high temperatures.
[0005] The first object of the present invention is to provide a high temperature resistant cast aluminum alloy, the element composition and mass percentage of the high temperature resistant cast aluminum alloy are: Si 1%-10%, Cu 0.1%-4%, Mg 0.05%-0.5%, Fe 0.05%-0.3%, Ti 0.01%-0.3%, Mn 0.1%-0.5%, Cr 0.01%-0.6%, V 0.02%-0.2%, Sn0.02%-0.2%, Sc 0.02%-0.2%, Hf0.02%-0.2%, Er 0.02%-0.2%, and the balance is other inevitable impurities and Al; the microstructure of the high temperature resistant cast aluminum alloy includes submicron precipitate phases and / or nano precipitate phases.
[0006] Furthermore, the element composition and mass percentage of the high temperature resistant cast aluminum alloy are: Si 1%-6%, Cu 0.5%-4%, Mg 0.2%-0.5%, Fe 0.1%-0.2%, Ti 0.1%-0.2%, Mn 0.2%-0.5%, Cr0.1%-0.6%, V 0.1%-0.2%, Sn 0.1%-0.2%, Sc 0.1%-0.2%, Hf0.1%-0.2%, Er0.1%-0.2%, other inevitable impurities 0-0.15%, and the rest is Al.
[0007] In one embodiment of the present invention, the size of the submicron precipitated phase is 50nm-300nm; the size of the nano precipitated phase is 20nm-100nm.
[0008] In one embodiment of the present invention, after the submicron precipitate phase or nano precipitate phase is kept at 100° C.-400° C. for 1 h-30 h, the increase range of the size ratio is less than 10%.
[0009] In one embodiment of the present invention, after the submicron precipitate phase or nano precipitate phase is kept at 100° C.-400° C. for 1 h-30 h, the interface relationship between the submicron precipitate phase and the alloy matrix is coherent and / or semi-coherent.
[0010] In one embodiment of the present invention, the submicron precipitated phase is selected from submicron precipitated phases containing one or more elements of Al, Fe, Mn, Cr, V and Sc, for example, it can be submicron precipitated phases such as Al3Sc, Al4(Cr,Mn), Al(MnCrFe)Si, Al(FeMn)Si, etc.;
[0011] In one embodiment of the present invention, the nano-precipitated phase is selected from the nano-precipitated phase containing one or more elements of Al, Sc, Hf and Er, for example, it can be Al3Er, Al3(Er,Hf) and other nano-precipitated phases; and / or, the nano-precipitated phase is selected from the nano-precipitated phase containing one or more elements of Al, Cu, Mg, Si and Sc, for example, it can be θ-Al2Cu, Q-Al5Cu2Mg8Si6, Al(Si,Sc) and other nano-precipitated phases.
[0012] The second object of the present invention is to provide a method for preparing the high temperature resistant cast aluminum alloy, comprising the following steps:
[0013] S1. After drying the raw materials, add them into a smelting furnace in the form of pure metal or master alloy, heat and melt them, and stir them evenly to obtain an aluminum alloy melt;
[0014] S2, under a protective atmosphere, mixing the aluminum alloy melt described in step S1 with a refining agent to perform refining, degassing and impurity removal;
[0015] S3, casting, solution heat treatment and aging treatment are performed on the aluminum alloy melt refined in S2 to obtain a high temperature resistant cast aluminum alloy.
[0016] In one embodiment of the present invention, in S1, the drying temperature is 100°C-500°C; the heating and melting temperature is 700°C-800°C; and the stirring time is 5 min-15 min.
[0017] In one embodiment of the present invention, in S2, the refining agent is hexachloroethane gas.
[0018] In one embodiment of the present invention, in S3, the solution heat treatment is divided into three stages, the temperature of the first stage is 200°C-350°C, and the time is 1h-5h; the temperature of the second stage is 400°C-470°C, and the time is 1h-6h; the temperature of the third stage is 480°C-535°C, and the time is 1h-6h;
[0019] The aging treatment is divided into two stages. The temperature of the first stage is 140°C-190°C, and the time is 1h-20h; the temperature of the second stage is 200°C-230°C, and the time is 0.5h-2h.
[0020] The third object of the present invention is to provide an application of the high temperature resistant cast aluminum alloy in automobile engines.
[0021] The technical solution of the present invention has the following advantages over the prior art:
[0022] (1) In order to improve the high temperature performance of aluminum alloy, the high temperature resistant cast aluminum alloy described in the present invention mainly improves the tensile properties of aluminum alloy at high temperature by introducing micron-level high temperature resistant phases at the grain boundaries. By controlling the alloy composition, proportion and preparation method, and reasonably setting the heat treatment and aging treatment parameters, at the same time, more than one submicron-level and nano-level high temperature resistant coarsening precipitation phases of certain components, sizes and characteristics are obtained, which effectively improves the strength of aluminum alloy in high temperature environment and strengthens the high temperature resistance of aluminum alloy. It effectively improves the problem of low strength of cast aluminum alloy at high temperature and meets the growing high temperature performance demand in the field of automotive engineering.
[0023] (2) The high temperature resistant cast aluminum alloy described in the present invention has a tensile strength of greater than 250 MPa when kept at 200°C for more than 10 hours, a tensile strength of greater than 129 MPa when kept at 300°C for more than 10 hours, and a tensile strength of greater than 85 MPa when kept at 400°C for more than 10 hours. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments of the present invention in conjunction with the accompanying drawings, wherein:
[0025] Figure 1 This is the microstructure diagram of the cast aluminum alloy prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0026] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0027] In the present invention, unless otherwise explained, technical and scientific terms used in the present invention have the same meanings as commonly understood by those skilled in the art to which the present invention belongs.
[0028] In the present invention, unless otherwise stated, the term "and / or" used in the present invention includes any and all combinations of one or more of the associated listed items.
[0029] In the present invention, unless otherwise stated, the experimental methods used in the embodiments of the present invention are conventional methods unless otherwise stated, and the materials, reagents, etc. used are all commercially available unless otherwise stated.
[0030] In the present invention, unless otherwise stated, when the terms "comprise" and / or "include" are used in the specification of the present invention, it indicates the existence of the described features, integers, steps, operations, raw materials or components, but does not exclude the existence or addition of one or more other features, integers, steps, operations, raw materials, components or their combinations.
[0031] Example 1
[0032] The element composition and mass percentage of the high temperature resistant casting aluminum alloy of the present invention are: Si 4.87%, Cu 1.23%, Mg 0.49%, Fe 0.10%, Ti 0.12%, Mn 0.30%, Cr 0.21%, V 0.11%, Sn 0.13%, Sc 0.11%, Hf 0.20%, Er 0.10%, other inevitable impurities 0-0.15%, and the rest is Al.
[0033] The preparation of high temperature resistant cast aluminum alloy specifically includes the following steps:
[0034] S1. Melting: weigh the raw materials according to the designed composition and dry them in a furnace at 300°C. Add pure Al and Al-Si into the melting furnace and melt them at 720°C. After they are melted, add Al-Fe, Al-Ti, Al-Mn, Al-Cr, Al-V, Al-RE (Sc, Er, Hf) intermediate alloys to continue melting. Then add pure Mg, pure Cu and pure Sn. After they are completely melted, stir for 10 minutes to obtain a uniform aluminum alloy melt.
[0035] S2. Refining: Hexachloroethane gas is introduced into the aluminum alloy melt for refining. The gas introduction rate is 0.1L / min. The refining time is 12min. After standing for 5min, the slag is removed and impurities are removed.
[0036] S3. Forming: The refined aluminum alloy melt is subjected to gravity casting to obtain an aluminum alloy ingot; the aluminum alloy ingot is subjected to three-level solution heat treatment and two-level aging treatment to obtain a high-temperature resistant cast aluminum alloy; wherein, the first-level temperature of the solution heat treatment is 300°C, and the time is 2h; the second-level temperature is 400°C, and the time is 4h; the third-level temperature is 500°C, and the time is 2h; the first-level temperature of the aging treatment is 150°C, and the time is 10h, and the second-level temperature is 200°C, and the time is 1h.
[0037] The microstructure of the cast aluminum alloy is as follows: Figure 1 As shown, from Figure 1 It can be seen that there are submicron and nano-precipitates of different compositions and sizes in the cast aluminum alloy. The size range of the submicron precipitates is 80nm-300nm, including Al3Sc, Al(MnCrFe)Si, etc.; the size range of the nano-precipitates is 50nm-100nm, including θ-Al2Cu, Q-Al5Cu2Mg8Si6, etc.
[0038] After being kept at high temperature for a certain period of time, it can be observed that these submicron precipitates and nano precipitates still maintain a coherent or semi-coherent relationship with the interface of the alloy matrix; mechanical tests are then performed on them, and the test results are shown in Table 1:
[0039] Table 1
[0040] Insulation temperature (℃) Insulation time (h) Size increase ratio (%) Tensile strength(MPa) 200 20 4.5 269 300 20 5.8 129 400 20 6.6 90
[0041] It can be seen from Table 1 that the method of this embodiment can obtain an aluminum alloy material with high tensile strength under a high temperature environment.
[0042] Example 2
[0043] The element composition and mass percentage of the high temperature resistant casting aluminum alloy of the present invention are: Si 5.13%, Cu 2.08%, Mg 0.45%, Fe 0.11%, Ti 0.12%, Mn 0.32%, Cr 0.22%, V 0.10%, Sn 0.14%, Sc 0.11%, Hf 0.20%, Er 0.10%, other inevitable impurities 0-0.15%, and the rest is Al.
[0044] The preparation of high temperature resistant cast aluminum alloy specifically includes the following steps:
[0045] S1. Melting: weigh the raw materials according to the designed composition and dry them in a furnace at 400°C. Add pure Al and Al-Si into the melting furnace and melt them at 730°C. After they are melted, add Al-Fe, Al-Ti, Al-Mn, Al-Cr, Al-V, Al-RE (Sc, Er, Hf) intermediate alloys to continue melting. Then add pure Mg, pure Cu and pure Sn. After they are completely melted, stir for 12 minutes to obtain a uniform aluminum alloy melt.
[0046] S2. Refining: Hexachloroethane gas is introduced into the aluminum alloy melt for refining. The gas introduction rate is 0.1L / min. The refining time is 15min. After standing for 6min, the slag is removed and impurities are removed.
[0047] S3. Forming: The refined aluminum alloy melt is subjected to gravity casting to obtain an aluminum alloy ingot; the aluminum alloy ingot is subjected to three-level solution heat treatment and two-level aging treatment to obtain a high-temperature resistant cast aluminum alloy; wherein, the first-level temperature of the solution heat treatment is 250°C, and the time is 3h; the second-level temperature is 450°C, and the time is 3h; the third-level temperature is 520°C, and the time is 4h; the first-level temperature of the aging treatment is 140°C, and the time is 12h; the second-level temperature is 200°C, and the time is 1h.
[0048] The microstructure of the obtained cast aluminum alloy contains submicron and nano-precipitates of different compositions and sizes. The size range of the submicron precipitates is 80nm-290nm, including Al3Sc, Al(MnCrFe)Si, etc.; the size range of the nano-precipitates is 30nm-90nm, including θ-Al2Cu, Q-Al5Cu2Mg8Si6, etc.
[0049] After being kept at high temperature for a certain period of time, it can be observed that these submicron precipitates and nano precipitates still maintain a coherent or semi-coherent relationship with the interface of the alloy matrix; mechanical tests were then performed on them, and the test results are shown in Table 2:
[0050] Table 2
[0051] Insulation temperature (℃) Insulation time (h) Size increase ratio (%) Tensile strength(MPa) 200 15 4.3 271 300 15 5.3 130 400 15 6.4 85
[0052] It can be seen from Table 2 that the method of this embodiment can obtain an aluminum alloy material with high tensile strength under high temperature environment.
[0053] Example 3
[0054] The element composition and mass percentage of the high temperature resistant casting aluminum alloy of the present invention are: Si 4.11%, Cu 1.51%, Mg 0.35%, Fe 0.10%, Ti 0.15%, Mn 0.31%, Cr 0.20%, V 0.11%, Sn 0.12%, Sc 0.10%, Hf 0.19%, Er 0.11%, other inevitable impurities 0-0.15%, and the rest is Al.
[0055] The preparation of high temperature resistant cast aluminum alloy specifically includes the following steps:
[0056] S1. Melting: weigh the raw materials according to the designed composition and dry them in a furnace at 400°C. Add pure Al and Al-Si into the melting furnace and melt them at 730°C. After they are melted, add Al-Fe, Al-Ti, Al-Mn, Al-Cr, Al-V, Al-RE (Sc, Er, Hf) intermediate alloys, and then add pure Mg, pure Cu and pure Sn. After they are completely melted, stir for 15 minutes to obtain a uniform aluminum alloy melt.
[0057] S2. Refining: Hexachloroethane gas is introduced into the aluminum alloy melt for refining. The gas introduction rate is 0.1L / min. The refining time is 15min. After standing for 8min, the slag is removed and impurities are removed.
[0058] S3. Forming: The refined aluminum alloy melt is subjected to gravity casting to obtain an aluminum alloy ingot; the aluminum alloy ingot is subjected to three-level solution heat treatment and two-level aging treatment to obtain a high-temperature resistant cast aluminum alloy; wherein, the first-level temperature of the solution heat treatment is 200°C, and the time is 4h; the second-level temperature is 470°C, and the time is 6h; the third-level temperature is 520°C, and the time is 4; the first-level temperature of the aging treatment is 140°C, and the time is 10h; the second-level temperature is 200°C, and the time is 1h.
[0059] The microstructure of the obtained cast aluminum alloy contains submicron and nano-precipitates of different compositions and sizes. The size range of the submicron precipitates is 50nm-280nm, including Al3Sc, Al(MnCrFe)Si, etc.; the size range of the nano-precipitates is 20nm-80nm, including θ-Al2Cu, Q-Al5Cu2Mg8Si6, etc.
[0060] After being kept at high temperature for a certain period of time, it can be observed that these submicron precipitates and nano precipitates still maintain a coherent or semi-coherent relationship with the interface of the alloy matrix; mechanical tests are then performed on them, and the test results are shown in Table 3:
[0061] Table 3
[0062] Insulation temperature (℃) Insulation time (h) Size increase ratio (%) Tensile strength(MPa) 200 10 3.9 270 300 10 5.0 135 400 10 6.0 87
[0063] It can be seen from Table 3 that the method of this embodiment can obtain an aluminum alloy material with high tensile strength under a high temperature environment.
[0064] Comparative Example 1
[0065] The element composition and mass percentage of the cast aluminum alloy are: Si 4.87%, Cu 1.23%, Mg 0.49%, Fe 0.10%, Ti 0.12%, other inevitable impurities 0-0.15%, and the rest is Al.
[0066] The preparation of cast aluminum alloy specifically includes the following steps:
[0067] S1. Melting: weigh the raw materials according to the designed composition and dry them in a furnace at 300°C. Add pure Al and Al-Si into the melting furnace and melt them at 720°C. After they are melted, add Al-Fe and Al-Ti master alloys to continue melting. Then add pure Mg and pure Cu. After they are completely melted, stir for 10 minutes to obtain a uniform aluminum alloy melt.
[0068] S2. Refining: Hexachloroethane gas is introduced into the aluminum alloy melt for refining. The gas introduction rate is 0.1L / min. The refining time is 12min. After standing for 5min, the slag is removed and impurities are removed.
[0069] S3. Forming: The refined aluminum alloy melt is subjected to gravity casting to obtain an aluminum alloy ingot; the aluminum alloy ingot is subjected to three-level solution heat treatment and two-level aging treatment to obtain a high-temperature resistant cast aluminum alloy; wherein, the first-level temperature of the solution heat treatment is 300°C, and the time is 2h; the second-level temperature is 400°C, and the time is 4h; the third-level temperature is 500°C, and the time is 2h; the first-level temperature of the aging treatment is 150°C, and the time is 10h, and the second-level temperature is 200°C, and the time is 3h.
[0070] After being kept at high temperature for a certain period of time, mechanical tests were performed on it. The test results are shown in Table 4:
[0071] Table 4
[0072] Insulation temperature (℃) Insulation time (h) Size increase ratio (%) Tensile strength(MPa) 200 20 4.8 235 300 20 5.7 108 400 20 6.3 50
[0073] It can be seen from Table 4 that the aluminum alloy material obtained by the method of this comparative example has poor tensile strength under high temperature environment.
[0074] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.
Claims
1. A high temperature resistant cast aluminum alloy, characterized in that: The element composition and mass percentage of the high temperature resistant casting aluminum alloy are: Si 1%-10%, Cu 0.1%-4%, Mg 0.05%-0.5%, Fe 0.05%-0.3%, Ti 0.01%-0.3%, Mn 0.1%-0.5%, Cr 0.01%-0.6%, V 0.02%-0.2%, Sn 0.02%-0.2%, Sc0.02%-0.2%, Hf 0.02%-0.2%, Er 0.02%-0.2%, the balance being other inevitable impurities and Al; the microstructure of the high temperature resistant cast aluminum alloy comprises a submicron precipitate phase and a nano precipitate phase; the size of the submicron precipitate phase is 50nm-300nm; the size of the nano precipitate phase is 20nm-100nm; after the submicron precipitate phase or the nano precipitate phase is kept at 100°C-400°C for 1h-30h, the increase range of the size ratio is less than 10%; The submicron precipitated phase is selected from submicron precipitated phases containing one or more elements of Al, Fe, Mn, Cr, V and Sc; The nano-precipitated phase is selected from the nano-precipitated phase containing one or more elements of Al, Sc, Hf and Er; and / or, the nano-precipitated phase is selected from the nano-precipitated phase containing one or more elements of Al, Cu, Mg, Si and Sc.
2. The high temperature resistant cast aluminum alloy according to claim 1, characterized in that: After the submicron precipitated phase or nano precipitated phase is kept at 100° C.-400° C. for 1 h-30 h, the interface relationship between the submicron precipitated phase and the alloy matrix is coherent and / or semi-coherent.
3. A method for preparing the high temperature resistant cast aluminum alloy according to any one of claims 1 to 2, characterized in that: The following steps are involved: S1. After drying the raw materials, add them into a smelting furnace in the form of pure metal or master alloy, heat and melt them, and stir them evenly to obtain an aluminum alloy melt; S2, under a protective atmosphere, mixing the aluminum alloy melt described in step S1 with a refining agent, and performing refining, degassing and impurity removal; S3, casting, solution heat treatment and aging treatment are performed on the aluminum alloy melt refined in S2 to obtain a high temperature resistant cast aluminum alloy.
4. The method for preparing a high temperature resistant cast aluminum alloy according to claim 2, characterized in that: In S1, the drying temperature is 100°C-500°C; the heating and melting temperature is 700°C-800°C; and the stirring time is 5min-15min.
5. The method for preparing a high temperature resistant cast aluminum alloy according to claim 2, characterized in that: In S2, the refining agent is hexachloroethane gas.
6. The method for preparing a high temperature resistant cast aluminum alloy according to claim 2, characterized in that: In S3, the solution heat treatment is divided into three stages, the temperature of the first stage is 200°C-350°C, and the time is 1h-5h; the temperature of the second stage is 400°C-470°C, and the time is 1h-6h; the temperature of the third stage is 480°C-535°C, and the time is 1h-6h; The aging treatment is divided into two stages. The temperature of the first stage is 140°C-190°C, and the time is 1h-20h; the temperature of the second stage is 200°C-230°C, and the time is 0.5h-2h.
7. Use of the high temperature resistant cast aluminum alloy according to any one of claims 1 to 2 in automobile engines.