A method for preparing flexible conductive fiber
By pre-stretching the fiber bundles and performing chemical oxidation polymerization on the surface, a conductive layer with wrinkles is formed, which solves the problem of reduced breaking strength and conductivity of conductive polymer fibers and achieves high elongation at break and maintenance of conductivity. , suitable for the preparation of flexible sensors.
Patent Information
- Application Number
- CN202410046232.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-12
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-01-12
AI Technical Summary
The breaking strength and elongation at break of conductive polymer fibers are low, and the conductivity will decrease after the fiber is stretched, which affects its application in the field of conductive functional textiles.
By pre-stretching the original fiber bundles by 10% to 25%, and then chemically oxidizing the conductive polymer material on the surface to form a conductive layer with wrinkles, the breaking strength and elongation at break of the fiber are improved, and the stretch is maintained The final conductivity.
The breaking elongation and breaking strength of the conductive fiber are improved, and the resistance is less than 107Ω·cm. It is suitable for preparing wearable sensors, and the resistance change rate is small when stretched.
Smart Images

Figure CN117758514B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a fiber, in particular to a method for preparing a flexible conductive fiber. Background Art
[0002] Flexible sensors have diverse and flexible structures, which make up for the defects of miniaturization and singularity of traditional sensors. They can quickly and accurately measure and collect special environments and special signals. Currently, flexible sensors are developing towards electronic skin, wearable devices and aerospace, especially wearable devices.
[0003] Flexible sensors require fibers to be conductive. Conductivity means that the resistance of the fiber is below 107Ω·cm under atmospheric conditions, but ordinary conventional fibers are not conductive. Currently, conductive fibers are divided into the following categories: conductive metal fibers, metal compound conductive fibers, carbon black conductive fibers, and conductive polymer fibers. Since the conjugated structure in the main chain of polyaniline and polypyrrole makes the molecular chain rigid, insoluble, and infusible, it is difficult to directly spin and process to form fibers. Therefore, conductive polymer fibers are polymerized on the surface of fibers by polymerizing conductive polymer materials such as aniline and pyrrole.
[0004] However, due to the influence of polyaniline and polypyrrole on the surface, the breaking strength and elongation at break of the conductive polymer fiber are relatively low, and the conductivity will decrease significantly after the fiber is stretched, which affects its application in the field of conductive functional textiles. Summary of the invention
[0005] In response to the above technical requirements, the present invention provides a method for preparing a flexible conductive fiber, which improves the breaking strength and elongation at break of the conductive fiber and the conductivity after stretching.
[0006] The technical solution of the present invention is as follows: a method for preparing flexible conductive fibers, wherein the original fiber bundle is kept in a stretched state and a conductive polymer material is polymerized on the surface by chemical oxidation to obtain the flexible conductive fibers.
[0007] Furthermore, maintaining the original fiber bundle in a stretched state is to stretch the original fiber bundle by 10% to 25%.
[0008] Furthermore, the specific steps of keeping the original fiber bundle in a stretched state and polymerizing the conductive polymer material on the surface include: immersing the stretched original fiber bundle in the conductive polymer material monomer solution to swell it, then taking out the original fiber bundle and wiping the conductive polymer material monomer solution on the surface of the fiber bundle, and then immersing it in an oxidant solution for polymerization, washing the polymerized fiber bundle with deionized water, and letting it stand to wait for the residual conductive polymer material monomer to volatilize, thereby shrinking the fiber bundle.
[0009] Furthermore, the swelling time of the original fiber bundle in the conductive polymer material monomer solution is 10 to 30 minutes.
[0010] Furthermore, the original fiber bundle is TPU fiber prepared by centrifugal spinning.
[0011] Furthermore, the rotation speed during centrifugal spinning is set to 1000-4000 r / min.
[0012] Furthermore, the receiving distance of the centrifugal spinning during the centrifugal spinning is 8 to 10 cm.
[0013] Furthermore, the conductive polymer material is polypyrrole or polyaniline.
[0014] Furthermore, the oxidant solution is a 1-3 mol / L ammonium persulfate solution.
[0015] The advantages of the present invention compared with the prior art are:
[0016] The conductive fiber with a wrinkled conductive layer on the surface is obtained by pre-stretching the fiber bundle and then polymerizing the conductive polymer material. The conductive fiber has a resistance of less than 10 7 Ω·cm, the elongation at break and the breaking strength can reach up to 169% and 9.5% respectively, which are 20% and 42% higher than those of the conductive fiber without stretching polymerization. In addition, the resistance change rate of the finished flexible conductive fiber is small when stretched, and it can be used to prepare wearable sensors. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is an electron microscope image of the flexible conductive fiber prepared in Example 1.
[0018] Figure 2 The resistance of the flexible conductive fiber prepared in Example 1 at different stretching lengths. DETAILED DESCRIPTION
[0019] The present invention will be further described below in conjunction with the embodiments, but are not intended to limit the present invention.
[0020] Example 1
[0021] TPU (polyurethane) was dissolved in a mixture of tetrahydrofuran (THF) and N-N-dimethylformamide (DMF), the TPU concentration was 13.5-23.5%, the DMF:THF ratio was 1:1-1:3, the stirring time was 3-6 hours, and the stirring temperature was 35-55°C to prepare the TPU spinning solution. After the TPU spinning solution was prepared, the original fiber bundle was prepared by centrifugal spinning. In the centrifugal spinning process, the model of the filament needle was selected as No. 19, the receiving distance of the roller was 8 cm, and the speed was set to 1000 r / min.
[0022] The original fiber bundle was washed and dried with deionized water, then kept stretched 10%, immersed in pyrrole to swell for 10 minutes, the fiber bundle was taken out, the pyrrole solution on the surface of the fiber bundle was wiped with dust-free paper, and immersed in 2 mol / L ammonium persulfate (APS, acidic solution: pH=1) solution for polymerization. After the polymerized fiber bundle was washed with deionized water and left to stand for the residual pyrrole in the fiber to evaporate, the fiber bundle shrank to obtain a flexible conductive fiber with wrinkles on the surface. The electron microscope image of the flexible conductive fiber is shown in the figure. Figure 1 As shown, it can be seen that the fiber has a wrinkled outer surface.
[0023] Example 2
[0024] The original fiber bundle of Example 1 was used, and the original fiber bundle was washed and dried with deionized water, and then kept stretched by 15%, immersed in pyrrole for swelling for 10 minutes, and the fiber bundle was taken out, and the pyrrole solution on the surface of the fiber bundle was wiped with dust-free paper, and immersed in 2 mol / L ammonium persulfate (APS, acidic solution: pH=1) solution for polymerization. After the polymerized fiber bundle was washed with deionized water, it was left to stand and wait for the residual pyrrole in the fiber to volatilize, and the fiber bundle shrank to obtain a flexible conductive fiber with wrinkles on the surface.
[0025] Example 3
[0026] The original fiber bundle of Example 1 was used, and the original fiber bundle was washed and dried with deionized water, and then kept stretched by 20%, immersed in pyrrole for swelling for 10 minutes, and the fiber bundle was taken out, and the pyrrole solution on the surface of the fiber bundle was wiped with dust-free paper, and immersed in 2 mol / L ammonium persulfate (APS, acidic solution: pH=1) solution for polymerization. After the polymerized fiber bundle was washed with deionized water, it was left to stand and wait for the residual pyrrole in the fiber to volatilize, and the fiber bundle shrank to obtain a flexible conductive fiber with wrinkles on the surface.
[0027] Example 4
[0028] The original fiber bundle of Example 1 was used, and the original fiber bundle was washed and dried with deionized water, and then kept stretched by 25%, immersed in pyrrole for swelling for 10 minutes, and the fiber bundle was taken out, and the pyrrole solution on the surface of the fiber bundle was wiped with dust-free paper, and immersed in 2 mol / L ammonium persulfate (APS, acidic solution: pH=1) solution for polymerization. After the polymerized fiber bundle was washed with deionized water, it was left to stand and wait for the residual pyrrole in the fiber to volatilize, and the fiber bundle shrank to obtain a flexible conductive fiber with wrinkles on the surface.
[0029] Example 5
[0030] The original fiber bundle of Example 1 was used, and the original fiber bundle was washed and dried with deionized water, and then kept stretched by 35%, immersed in pyrrole for swelling for 10 minutes, and the fiber bundle was taken out, and the pyrrole solution on the surface of the fiber bundle was wiped with dust-free paper, and immersed in 2 mol / L ammonium persulfate (APS, acidic solution: pH=1) solution for polymerization. After the polymerized fiber bundle was washed with deionized water, it was left to stand and wait for the residual pyrrole in the fiber to volatilize, and the fiber bundle shrank to obtain a flexible conductive fiber with wrinkles on the surface.
[0031] Example 6
[0032] The original fiber bundle of Example 1 was used, and the original fiber bundle was washed and dried with deionized water, and then kept stretched by 5%, immersed in pyrrole for swelling for 10 minutes, and the fiber bundle was taken out, and the pyrrole solution on the surface of the fiber bundle was wiped with dust-free paper, and immersed in 2 mol / L ammonium persulfate (APS, acidic solution: pH=1) solution for polymerization. After the polymerized fiber bundle was washed with deionized water, it was left to stand and wait for the residual pyrrole in the fiber to volatilize, and the fiber bundle shrank to obtain a flexible conductive fiber with wrinkles on the surface.
[0033] Example 7
[0034] The original fiber bundle was prepared by centrifugal spinning process using the TPU spinning solution of Example 1. In the centrifugal spinning process, the model of the spinning needle was selected to be No. 20, the receiving distance of the roller was 10 cm, and the rotation speed was set to 2000 r / min.
[0035] The original fiber bundle was washed and dried with deionized water, then kept stretched by 10%, immersed in pyrrole for swelling for 10 minutes, and the fiber bundle was taken out. The pyrrole solution on the surface of the fiber bundle was wiped with dust-free paper, and immersed in 2 mol / L ammonium persulfate (APS, acidic solution: pH=1) solution for polymerization. After the polymerized fiber bundle was washed with deionized water, it was left to stand and wait for the residual pyrrole in the fiber to volatilize, and the fiber bundle shrank to obtain a flexible conductive fiber with wrinkles on the surface.
[0036] Example 8
[0037] The original fiber bundle was prepared by centrifugal spinning process using the TPU spinning solution of Example 1. In the centrifugal spinning process, the model of the spinning needle was selected to be No. 22, the receiving distance of the roller was 10 cm, and the rotation speed was set to 4000 r / min.
[0038] The original fiber bundle was washed and dried with deionized water, then kept stretched by 10%, immersed in pyrrole for swelling for 10 minutes, and the fiber bundle was taken out. The pyrrole solution on the surface of the fiber bundle was wiped with dust-free paper, and immersed in 2 mol / L ammonium persulfate (APS, acidic solution: pH=1) solution for polymerization. After the polymerized fiber bundle was washed with deionized water, it was left to stand and wait for the residual pyrrole in the fiber to volatilize, and the fiber bundle shrank to obtain a flexible conductive fiber with wrinkles on the surface.
[0039] Example 9
[0040] The original fiber bundle was prepared by centrifugal spinning process using the TPU spinning solution of Example 1. In the centrifugal spinning process, the model of the spinning needle was selected to be No. 20, the receiving distance of the roller was 10 cm, and the rotation speed was set to 2000 r / min.
[0041] The original fiber bundle was washed and dried with deionized water, then kept stretched by 10%, immersed in pyrrole for swelling for 20 minutes, and the fiber bundle was taken out. The pyrrole solution on the surface of the fiber bundle was wiped with dust-free paper, and then immersed in 1 mol / L ammonium persulfate (APS, acidic solution: pH=1) solution for polymerization. After the polymerized fiber bundle was washed with deionized water, it was left to stand and wait for the residual pyrrole in the fiber to volatilize, and the fiber bundle shrank to obtain a flexible conductive fiber with wrinkles on the surface.
[0042] Example 10
[0043] The original fiber bundle was prepared by centrifugal spinning process using the TPU spinning solution of Example 1. In the centrifugal spinning process, the model of the spinning needle was selected to be No. 20, the receiving distance of the roller was 10 cm, and the rotation speed was set to 2000 r / min.
[0044] The original fiber bundle was washed and dried with deionized water, then kept stretched by 10%, immersed in pyrrole for swelling for 30 minutes, and the fiber bundle was taken out. The pyrrole solution on the surface of the fiber bundle was wiped with dust-free paper, and immersed in 3 mol / L ammonium persulfate (APS, acidic solution: pH=1) solution for polymerization. After the polymerized fiber bundle was washed with deionized water, it was left to stand and wait for the residual pyrrole in the fiber to volatilize, and the fiber bundle shrank to obtain a flexible conductive fiber with wrinkles on the surface.
[0045] Embodiment 11
[0046] The original fiber bundle was prepared by centrifugal spinning process using the TPU spinning solution of Example 1. In the centrifugal spinning process, the model of the spinning needle was selected to be No. 20, the receiving distance of the roller was 10 cm, and the rotation speed was set to 2000 r / min.
[0047] The original fiber bundle was washed and dried with deionized water, then kept stretched by 10%, immersed in a solution of aniline and pentasulfosalicylic acid with a mass ratio of 1:1.5 to swell for 10 minutes, and the fiber bundle was taken out, and the surface solution of the fiber bundle was wiped with dust-free paper, and then immersed in a 2 mol / L ammonium persulfate (APS, acidic solution: pH=1) solution for polymerization. After the polymerized fiber bundle was washed with deionized water, it was left to stand and wait for the residual aniline solution in the fiber to evaporate, and the fiber bundle shrank to obtain a flexible conductive fiber with wrinkles on the surface.
[0048] Example 12
[0049] The TPU spinning solution of Example 1 was used to prepare the original fiber bundle by electrospinning process. The original fiber bundle was washed and dried with deionized water, then kept stretched by 10%, immersed in pyrrole for swelling for 10 minutes, the fiber bundle was taken out, the pyrrole solution on the surface of the fiber bundle was wiped with dust-free paper, and immersed in 2 mol / L ammonium persulfate (APS, acidic solution: pH=1) solution for polymerization. After the polymerized fiber bundle was washed with deionized water, it was left to stand and wait for the residual pyrrole in the fiber to volatilize, and the fiber bundle shrank to obtain a flexible conductive fiber with wrinkles on the surface.
[0050] Comparative Example 1
[0051] The original fiber bundle was prepared by centrifugal spinning process using the TPU spinning solution of Example 1. In the centrifugal spinning process, the model of the spinning needle was selected to be No. 20, the receiving distance of the roller was 10 cm, and the rotation speed was set to 2000 r / min.
[0052] The original fiber bundle was washed and dried with deionized water, then immersed in pyrrole to swell for 30 minutes, the fiber bundle was taken out, the pyrrole solution on the surface of the fiber bundle was wiped with dust-free paper, and then immersed in 3 mol / L ammonium persulfate (APS, acidic solution: pH=1) solution for polymerization. After the polymerized fiber bundle was washed with deionized water, it was left to stand and wait for the residual pyrrole in the fiber to volatilize, and the fiber bundle shrank to obtain a flexible conductive fiber.
[0053] Comparative Example 2
[0054] The original fiber bundle was prepared by centrifugal spinning process using the TPU spinning solution of Example 1. In the centrifugal spinning process, the model of the spinning needle was selected to be No. 19, the receiving distance of the roller was 8 cm, and the rotation speed was set to 1000 r / min.
[0055] The original fiber bundle was washed and dried with deionized water, then immersed in pyrrole to swell for 10 minutes, the fiber bundle was taken out, the pyrrole solution on the fiber bundle surface was wiped with dust-free paper, and then immersed in 2 mol / L ammonium persulfate (APS, acidic solution: pH=1) solution for polymerization. After the polymerized fiber bundle was washed with deionized water, it was left to stand and wait for the residual pyrrole in the fiber to volatilize, and the fiber bundle shrank to obtain a flexible conductive fiber.
[0056] The elongation at break and the breaking strength of the flexible conductive fibers prepared in the above-mentioned embodiments and comparative examples were tested with reference to the Chinese national standard GB / T 3916-2007 "Fiber strength test method", and the fiber resistance was tested with reference to the Chinese national standard GB / T 11017-2002 "Constant current method for determining the conductive properties of chemical fibers". The resistance values were compared when the fiber was at its original length of 10 cm and stretched by 5%. The results are shown in Table 1.
[0057] Table 1 Test results of elongation at break, breaking strength and fiber resistance of various embodiments and comparative examples
[0058]
[0059] In addition, the flexible conductive fiber obtained in Example 1 was stretched to different degrees and the fiber resistance was tested. The resistance value changes were as follows: Figure 2 shown.
[0060] From the test results of the above embodiments and comparative examples, it can be seen that whether the conductive material is stretched when polymerizing affects the resistance change of the fiber and also affects the mechanical properties of the fiber. Compared with comparative example 2, when the conductive material is stretched by 10%, the elongation at break is 11.5%, and the breaking strength is 169cN / dTex. The elongation at break and the breaking strength of the conductive fiber are 20% and 42% higher than those without stretching, respectively. Compared with comparative example 1, the elongation at break and the breaking strength of the conductive fiber in embodiment 10 are 18% and 36% higher than those without stretching, respectively. The resistance change amplitude of the finished fiber that is not stretched during the preparation process increases when stretched. When the elongation is low (5%), the elongation at break of the fiber is low at 11.1%, at which time the polymerized pyrrole is less and the resistance value is slightly larger, which is 9.07MΩ. When the stretching length is high (35%), the elongation at break of the fiber is low at 11.3%, and the breaking strength is poor at 128cN / dTex. At this time, there is too much polymerized pyrrole, which destroys the surface structure of the fiber and affects the performance of the fiber. When the needle size and receiving distance, polymerization time and concentration are changed, the elongation at break, breaking strength and resistance of the fiber are less affected. It can be seen from Example 12 that under the same stretching effect, the resistance of electrospinning is greater than that of centrifugal spinning. This is because the fibers produced by electrospinning are relatively compact and cannot fully react with pyrrole, resulting in a relatively large resistance under the same stretching.
Claims
1. A method for preparing a flexible conductive fiber, characterized in that: The flexible conductive fiber is prepared by keeping the original fiber bundle in a stretched state and polymerizing the conductive polymer material on the surface by chemical oxidation, wherein the conductive polymer material is polypyrrole or polyaniline. The specific steps include: stretching the original fiber bundle by 10% to 25% and immersing it in a monomer solution of the conductive polymer material to swell, then taking out the original fiber bundle and wiping the conductive polymer material monomer solution on the surface of the fiber bundle, and then immersing it in an oxidant solution for polymerization, washing the polymerized fiber bundle with deionized water, standing it to wait for the residual conductive polymer material monomer to volatilize, and then shrinking the fiber bundle, wherein the original fiber bundle is TPU fiber prepared by centrifugal spinning, and the receiving distance of the centrifugal spinning is 8 to 10 cm.
2. The method for preparing the flexible conductive fiber according to claim 1, characterized in that: The swelling time of the original fiber bundle in the conductive polymer material monomer solution is 10 to 30 minutes.
3. The method for preparing the flexible conductive fiber according to claim 1, characterized in that: The rotation speed during the centrifugal spinning is set to 1000-4000 r / min.
4. The method for preparing the flexible conductive fiber according to claim 1, characterized in that: The oxidant solution is a 1-3 mol / L ammonium persulfate solution.
Citation Information
Patent Citations
Liquid crystal display device with touch panel
JP1995084705A