A regeneration process for graphite negative electrode of lithium-ion battery for vehicle and regenerated graphite negative electrode
By using separator and modified asphalt coating technology in the mixing machine, combined with aminourea modified primary graphite powder, the problem of insufficient purity and cycle stability of graphite materials in the prior art is solved, and efficient graphite negative electrode regeneration is achieved The process improves the efficiency of resource recycling.
Patent Information
- Application Number
- CN202311841025.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-29
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-12-29
AI Technical Summary
In the prior art, the regeneration process of graphite negative electrodes of lithium-ion batteries for automotive use cannot effectively improve the purity and cycle stability of graphite materials, and cannot meet the high market demand for graphite performance, resulting in low resource recycling and utilization efficiency.
Add a separator to the mixer, match the appropriate stirring speed and time, and use ultrasonic dispersion and modified asphalt coating technology to combine with the aminourea modified primary graphite powder to significantly improve the purity and circulation stability of the graphite.
The purity of recycled graphite materials is greater than 99.5%, and the gram capacity and cycle stability of graphite are significantly improved, which meets the high market demand for graphite performance and promotes efficient recycling and utilization of resources.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of processing waste lithium-ion batteries, and specifically relates to a regeneration process for a graphite negative electrode of a lithium-ion battery for a vehicle and a regenerated graphite negative electrode. Background Art
[0002] New energy vehicles refer to vehicles that use non-fossil energy as power, such as pure electric vehicles, plug-in hybrid vehicles, etc. In recent years, with the improvement of environmental awareness and the advancement of new energy technology, the development of new energy vehicles has gradually received policy and market support.
[0003] In recent years, with the widespread application of lithium-ion batteries, the recycling of end-of-life lithium-ion batteries has become an important issue in the development of new energy vehicles. Lithium-ion batteries are one of the core components of new energy vehicles, and their performance and quality directly affect the vehicle's range and service life. The recycling of end-of-life lithium-ion batteries involves issues such as environmental protection and resource utilization. At present, there are some difficulties and challenges in the recycling of lithium-ion batteries in China, such as high recycling costs, poor recycling channels, and immature recycling technology. Therefore, it is necessary to increase research and investment in the recycling of lithium-ion batteries to promote the sustainable development of the new energy vehicle industry.
[0004] The regeneration of lithium-ion battery graphite negative electrode refers to the process of recycling and reprocessing the used lithium-ion battery graphite negative electrode to extract the useful substances and make new lithium-ion battery graphite negative electrode materials again. Graphite negative electrode is one of the main components of lithium-ion batteries, and the production of this material consumes a lot of resources and energy. By regenerating and recycling graphite negative electrode materials, a lot of resources can be saved and the impact on the natural environment can be reduced. Regenerating and recycling graphite negative electrode materials can further reduce the cost of battery manufacturing, which has a positive effect on promoting the popularization and promotion of new energy vehicles and improving their market competitiveness. At the same time, the waste of lithium-ion batteries will cause pollution and harm to the environment. By regenerating and recycling graphite negative electrode materials, the discharge of waste can be reduced, and the pollution and harm to the environment can be reduced. Regenerating and recycling graphite negative electrode materials conforms to the concept of circular economy, can promote the development of circular economy, improve resource utilization efficiency, and achieve sustainable development.
[0005] Therefore, the regeneration of graphite negative electrodes of lithium-ion batteries has positive significance in promoting the development of the new energy vehicle industry, promoting the construction of a circular economy, protecting the environment and reducing resource consumption. Recycling and disassembling waste lithium-ion batteries and reusing the positive and negative electrode materials after processing is an important direction to further promote energy conservation and emission reduction. The lithium-ion battery recycling process can usually be divided into pretreatment, impurity removal and recycling. However, the gram capacity of graphite materials obtained by the current recycling process of the negative electrode of automotive ion batteries is significantly lower than the specific capacity of commercial graphite materials, which does not meet the market's increasingly high performance requirements for graphite materials. Therefore, there is an urgent need for a regeneration process for graphite negative electrodes of automotive lithium-ion batteries to improve the performance of recycled graphite negative electrodes prepared from graphite materials and truly achieve resource recycling and utilization. Summary of the invention
[0006] The purpose of the present invention is to provide a regeneration process for graphite negative electrodes of automotive lithium-ion batteries and a regenerated graphite negative electrode. The graphite material in the discarded graphite negative electrodes of automotive lithium-ion batteries is recycled, and the regenerated graphite material prepared by the recycled graphite negative electrode has high purity. The battery prepared by the recycled graphite negative electrode has good gram capacity and cycle stability, which is of great significance for the recycling and reuse of waste lithium-ion batteries and environmental protection.
[0007] In order to achieve the above object, the present invention provides the following technical solutions:
[0008] A regeneration process for a graphite negative electrode of a lithium-ion battery for a vehicle comprises the following steps:
[0009] (1) placing a graphite negative electrode sheet of a waste automotive lithium-ion battery and a separation aid in a kneader for kneading at a stirring speed of 15-20 rpm, a temperature of 20-30° C., and a time of 2-3 h, so that the graphite powder is peeled off from the copper foil to obtain a mixture containing separated graphite powder and copper foil; wherein the separation aid comprises the following components in parts by weight: 50-55 parts of cycloalkanes, 30-45 parts of tetracyclic aromatic hydrocarbons, 15-20 parts of tricyclic aromatic hydrocarbons, and 1-3 parts of surfactants;
[0010] (2) passing the mixture containing the separated graphite powder and copper foil through a 30-40 mesh sieve to obtain a mixed slurry of copper foil and graphite powder;
[0011] (3) centrifugally separating the mixed slurry containing graphite powder to obtain wet graphite powder, washing it with deionized water for 3-4 times, separating it by filter pressing, and drying it to obtain primary graphite powder;
[0012] (4) dispersing 10 parts by mass of primary graphite powder in 30-40 parts by mass of deionized water to obtain a dispersion, adding 3-4 parts by mass of semicarbazide, and uniformly dispersing by ultrasonication, and then reacting at 170-180° C. for 17-20 hours, centrifuging, washing, and drying to obtain modified primary graphite powder;
[0013] (5) Mix a carbon source and modified primary graphite powder in a mass ratio of 0.3-0.6:1, calcine under a nitrogen atmosphere at 800-900° C. for 6-7 hours, and cool to room temperature to obtain a regenerated graphite material.
[0014] Furthermore, the mass ratio of the graphite negative electrode sheet to the separator is 1:5-6.
[0015] Furthermore, the surfactant is selected from one or more of cocamidopropyl betaine, stearyl polyoxyethylene ether, and sodium dodecylbenzene sulfonate.
[0016] Furthermore, the surfactant is a compound of cocamidopropyl betaine, stearyl polyoxyethylene ether and sodium dodecylbenzene sulfonate in a mass ratio of 1:1.3-1.6:0.4-0.8.
[0017] In the prior art, a kneading machine is usually used to peel graphite and copper, but the peeling is often incomplete, and the purity of the regenerated graphite is not high. The present invention adds a separation aid in the kneading machine, and matches the appropriate stirring speed and time to improve the purity of the regenerated graphite. It is speculated that when the graphite part is peeled off the copper plate in the kneading machine, the components of the separation aid can play the role of solubilizing, wetting and adsorbing graphite, assisting the kneading machine to better separate graphite from copper foil, reducing ash doping in graphite, and improving purity. The inventor unexpectedly found that when the surfactant is a specific mass ratio of cocamidopropyl betaine, octadecyl alcohol polyoxyethylene ether and sodium dodecylbenzene sulfonate, the stirring speed can be 15-20rpm, the temperature is 20-30℃, and the kneading time is not more than 3 hours, that is, the regenerated graphite material with a purity greater than 99.5% can be obtained, and at the same time, the kneading time of the existing process is shortened, and the efficiency is improved.
[0018] Furthermore, the carbon source is modified asphalt.
[0019] Furthermore, the preparation method of the modified asphalt is as follows: medium-temperature coal tar is crushed and sieved to make asphalt powder, 5-6 parts of sodium polystyrene sulfonate and 8-10 parts of dispersant are mixed, heated to 250-260°C, stirred evenly, 100-140 parts of asphalt powder are added, stirred at 230-250°C for 3-5h, 3-6 parts of silicon monoxide are added, the temperature is reduced to 90-100°C, stirred for 6-7h, vacuum dried, nitrogen is used as protective gas, the temperature is increased to 900-1000°C, and the temperature is kept for 4-5h to obtain modified asphalt.
[0020] Furthermore, the dispersant is Dow Corning PMX-200.
[0021] Furthermore, the particle size of the silicon monoxide is 3-5 μm.
[0022] Furthermore, the screening is specifically through a 60-80 mesh sieve.
[0023] Most of the graphite negative electrode regeneration processes in the prior art recycle graphite and copper foil, but the gram capacity of the obtained graphite is often not able to meet the market's high demand for graphite performance when it is truly applied to commercial production, and the true meaning of resource recovery and utilization is lost. The inventor tried to use asphalt to carbon-coat the primary recovered graphite obtained after separation, but the improvement effect on the gram capacity of graphite was minimal. The present invention uses modified asphalt as a carbon source, which can significantly improve the gram capacity of graphite. It is speculated that the modified asphalt is more uniformly and densely coated on the graphite, and at the same time, silicon monoxide with high gram capacity is added to the modified asphalt, which can be inserted into the graphite during the calcination process, synergistically improving the gram capacity of graphite. However, the inventor found that the cycle stability of graphite is not ideal. The inventor unexpectedly discovered that the cycle stability of graphite can be improved by first modifying the primary graphite powder with aminourea and then carbon-coating it. It is speculated that the modified primary graphite powder and the modified asphalt have better compatibility. After calcination, the structure inside the graphite is more three-dimensional and disordered, which can improve the cycle stability.
[0024] The present invention also provides a regenerated graphite negative electrode prepared by using the regenerated graphite material.
[0025] Compared with the prior art, the advantages and beneficial effects of the present invention are:
[0026] 1. The present invention provides a regeneration process for graphite negative electrodes of automotive lithium-ion batteries and a regenerated graphite negative electrode. The graphite material in the discarded graphite negative electrodes of automotive lithium-ion batteries is recycled, and the regenerated graphite prepared by the recycled graphite negative electrode has high purity. The battery prepared by the recycled graphite negative electrode has good gram capacity and cycle stability, which is of great significance for the recycling and reuse of waste lithium-ion batteries and environmental protection.
[0027] 2. The present invention adds a separation aid to the kneading machine, and matches the appropriate stirring speed and time to improve the purity of the regenerated graphite. When the surfactant is a compound of cocamidopropyl betaine, octadecyl alcohol polyoxyethylene ether and sodium dodecylbenzene sulfonate in a specific mass ratio, the graphite with a purity greater than 99.5% can be obtained at a stirring speed of 15-20rpm and a temperature of 20-30°C for a kneading time of no more than 3 hours. At the same time, the kneading time of the existing process is shortened, and the efficiency is improved.
[0028] 3. The present invention uses modified asphalt as a carbon source, which can significantly improve the gram capacity of graphite. It is speculated that the modified asphalt covers the graphite more evenly and densely, and at the same time, silicon monoxide with high gram capacity is added to the modified asphalt, which can be inserted into the graphite during the calcination process, synergistically improving the gram capacity of graphite. The inventor unexpectedly found that the cyclic stability of graphite can be improved by first modifying the primary graphite powder with aminourea and then carbon coating it. DETAILED DESCRIPTION
[0029] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] The raw materials in the examples of the present invention were purchased from the following manufacturers, and all were commercially available unless otherwise specified:
[0031] Dow Corning PMX-200 was purchased from Dow Chemical - Dow Corning Series.
[0032] Cycloalkane is cyclohexane, which was purchased from Shandong West Asia Chemical Co., Ltd.
[0033] The tetracyclic aromatic hydrocarbon is pyrene, which was purchased from Shandong West Asia Chemical Co., Ltd.
[0034] The tricyclic aromatic hydrocarbon was 9,10-dimethylanthracene, which was purchased from Shandong West Asia Chemical Co., Ltd.
[0035] Example 1
[0036] This embodiment provides a regeneration process for a graphite negative electrode of a lithium-ion battery for a vehicle, comprising the following steps:
[0037] (1) placing a graphite negative electrode sheet of a waste automotive lithium-ion battery and a separation aid in a kneader for kneading at a stirring speed of 18 rpm, a temperature of 25° C., and a time of 2.5 h, so that the graphite powder is peeled off from the copper foil to obtain a mixture containing separated graphite powder and copper foil; the separation aid comprises the following components in parts by weight: 52 parts of cycloalkanes, 40 parts of tetracyclic aromatic hydrocarbons, 18 parts of tricyclic aromatic hydrocarbons, and 2 parts of surfactants;
[0038] (2) passing the mixture containing the separated graphite powder and copper foil through a 30-mesh sieve to obtain a mixed slurry of copper foil and graphite powder;
[0039] (3) centrifuging the mixed slurry containing graphite powder to obtain wet graphite powder, washing it with deionized water for 4 times, separating it by filter pressing, and drying it to obtain primary graphite powder;
[0040] (4) dispersing 10 parts by mass of primary graphite powder in 35 parts by mass of deionized water to obtain a dispersion, adding 3.5 parts by mass of semicarbazide, and uniformly dispersing by ultrasonication, and then reacting at 175°C for 19 hours, centrifuging, washing, and drying to obtain a modified primary graphite powder;
[0041] (5) A carbon source and modified primary graphite powder in a mass ratio of 0.5:1 were mixed, calcined at 850° C. for 6.5 h in a nitrogen atmosphere, and cooled to room temperature to obtain a regenerated graphite material.
[0042] The mass ratio of the graphite negative electrode sheet to the separator is 1:5.5.
[0043] The surfactant is a compound of cocamidopropyl betaine, stearyl polyoxyethylene ether and sodium dodecylbenzene sulfonate in a mass ratio of 1:1.5:0.6.
[0044] The carbon source is modified asphalt. The preparation method of the modified asphalt is as follows: by weight, medium-temperature coal tar is crushed and passed through a 60-mesh sieve to prepare asphalt powder, 5.5 parts of sodium polystyrene sulfonate and 9 parts of Dow Corning PMX-200 are mixed, heated to 255°C, stirred evenly, 125 parts of asphalt powder are added, stirred at 240°C for 4h, 5 parts of silicon monoxide with a particle size of 3-5μm are added, the temperature is reduced to 95°C, stirred for 6.5h, vacuum dried, nitrogen is used as a protective gas, the temperature is increased to 950°C, and the temperature is kept for 4.5h to obtain the modified asphalt.
[0045] Example 2
[0046] This embodiment provides a regeneration process for a graphite negative electrode of a lithium-ion battery for a vehicle, comprising the following steps:
[0047] (1) placing a graphite negative electrode sheet of a waste automotive lithium-ion battery and a separation aid in a kneader for kneading at a stirring speed of 15 rpm, a temperature of 20° C., and a time of 2 h, so that the graphite powder is peeled off from the copper foil to obtain a mixture containing separated graphite powder and copper foil; the separation aid comprises the following components in parts by weight: 50 parts of cycloalkanes, 30 parts of tetracyclic aromatic hydrocarbons, 15 parts of tricyclic aromatic hydrocarbons, and 1 part of a surfactant;
[0048] (2) passing the mixture containing the separated graphite powder and copper foil through a 30-mesh sieve to obtain a mixed slurry of copper foil and graphite powder;
[0049] (3) centrifugally separating the mixed slurry containing graphite powder to obtain wet graphite powder, washing it with deionized water for three times, separating it by filter pressing, and drying it to obtain primary graphite powder;
[0050] (4) dispersing 10 parts by mass of primary graphite powder in 30 parts by mass of deionized water to obtain a dispersion, adding 3 parts by mass of semicarbazide, and uniformly dispersing by ultrasonication, and then reacting at 170°C for 17 hours, centrifuging, washing, and drying to obtain a modified primary graphite powder;
[0051] (5) A carbon source and modified primary graphite powder in a mass ratio of 0.3:1 were mixed, calcined at 800°C for 6 h in a nitrogen atmosphere, and then cooled to room temperature to obtain a regenerated graphite material.
[0052] The mass ratio of the graphite negative electrode sheet to the separator is 1:5.
[0053] The surfactant is a compound of cocamidopropyl betaine, stearyl polyoxyethylene ether and sodium dodecylbenzene sulfonate in a mass ratio of 1:1.3:0.4.
[0054] The carbon source is modified asphalt. The preparation method of the modified asphalt is as follows: by weight, medium-temperature coal tar is crushed and passed through a 60-mesh sieve to prepare asphalt powder, 5 parts of sodium polystyrene sulfonate and 8 parts of Dow Corning PMX-200 are mixed, heated to 250°C, stirred evenly, 100 parts of asphalt powder are added, stirred at 230°C for 3h, 3 parts of silicon monoxide with a particle size of 3-5μm are added, the temperature is reduced to 90°C, stirred for 6h, vacuum dried, nitrogen is used as a protective gas, the temperature is increased to 900°C, and the temperature is kept for 4h to obtain the modified asphalt.
[0055] Example 3
[0056] This embodiment provides a regeneration process for a graphite negative electrode of a lithium-ion battery for a vehicle, comprising the following steps:
[0057] (1) placing a graphite negative electrode sheet of a waste automotive lithium-ion battery and a separation aid in a kneader for kneading at a stirring speed of 20 rpm, a temperature of 30° C., and a time of 3 h, so that the graphite powder is peeled off from the copper foil to obtain a mixture containing separated graphite powder and copper foil; the separation aid comprises the following components in parts by weight: 55 parts of cycloalkanes, 45 parts of tetracyclic aromatic hydrocarbons, 20 parts of tricyclic aromatic hydrocarbons, and 3 parts of surfactants;
[0058] (2) passing the mixture containing the separated graphite powder and copper foil through a 40-mesh sieve to obtain a mixed slurry of copper foil and graphite powder;
[0059] (3) centrifuging the mixed slurry containing graphite powder to obtain wet graphite powder, washing it with deionized water for 4 times, separating it by filter pressing, and drying it to obtain primary graphite powder;
[0060] (4) dispersing 10 parts by mass of primary graphite powder in 40 parts by mass of deionized water to obtain a dispersion, adding 4 parts by mass of semicarbazide, and uniformly dispersing by ultrasonication, and then reacting at 180°C for 20 hours, centrifuging, washing, and drying to obtain a modified primary graphite powder;
[0061] (5) A carbon source and modified primary graphite powder in a mass ratio of 0.6:1 were mixed, calcined at 900°C for 7 hours in a nitrogen atmosphere, and then cooled to room temperature to obtain a regenerated graphite material.
[0062] The mass ratio of the graphite negative electrode sheet to the separator is 1:6.
[0063] The surfactant is a compound of cocamidopropyl betaine, stearyl polyoxyethylene ether and sodium dodecylbenzene sulfonate in a mass ratio of 1: 1.6: 0.8.
[0064] The carbon source is modified asphalt. The preparation method of the modified asphalt is as follows: by weight, medium-temperature coal tar is crushed and passed through an 80-mesh sieve to prepare asphalt powder, 6 parts of sodium polystyrene sulfonate and 10 parts of Dow Corning PMX-200 are mixed, heated to 260°C, stirred evenly, 140 parts of asphalt powder are added, stirred at 250°C for 5 hours, 6 parts of silicon monoxide with a particle size of 3-5 μm are added, the temperature is reduced to 100°C, stirred for 7 hours, vacuum dried, nitrogen is used as a protective gas, the temperature is increased to 1000°C, and the temperature is kept for 5 hours to obtain the modified asphalt.
[0065] Comparative Example 1
[0066] The difference between this comparative example and Example 1 is that no separation aid is added. Specifically, a regeneration process of a graphite negative electrode of a lithium-ion battery for a vehicle comprises the following steps:
[0067] (1) placing the graphite negative electrode sheet of the waste automotive lithium-ion battery in a kneading machine for kneading at a stirring speed of 15 rpm, a temperature of 20° C., and a time of 2 h, so that the graphite powder is peeled off from the copper foil to obtain a mixture containing separated graphite powder and copper foil;
[0068] (2) passing the mixture containing the separated graphite powder and copper foil through a 30-mesh sieve to obtain a mixed slurry of copper foil and graphite powder;
[0069] (3) centrifugally separating the mixed slurry containing graphite powder to obtain wet graphite powder, washing it with deionized water for three times, separating it by filter pressing, and drying it to obtain primary graphite powder;
[0070] (4) dispersing 10 parts by mass of primary graphite powder in 30 parts by mass of deionized water to obtain a dispersion, adding 3 parts by mass of semicarbazide, and uniformly dispersing by ultrasonication, and then reacting at 170°C for 17 hours, centrifuging, washing, and drying to obtain a modified primary graphite powder;
[0071] (5) A carbon source and modified primary graphite powder in a mass ratio of 0.3:1 were mixed, calcined at 800°C for 6 h in a nitrogen atmosphere, and then cooled to room temperature to obtain a regenerated graphite material.
[0072] Comparative Example 2
[0073] The difference between this comparative example and Example 1 is that the separation aid comprises the following components in parts by mass: 65 parts of cycloalkanes, 15 parts of tetracyclic aromatic hydrocarbons, 35 parts of tricyclic aromatic hydrocarbons and 1 part of a surfactant; the surfactant is a compound of cocamidopropyl betaine, Tween-60 and sodium dodecylbenzene sulfonate in a mass ratio of 1:1:1.
[0074] Comparative Example 3
[0075] The difference between this comparative example and Example 1 is that the asphalt is not modified.
[0076] Comparative Example 4
[0077] The difference between this comparative example and Example 1 is that the carbon source is modified asphalt. The preparation method of the modified asphalt is as follows: by weight, medium-temperature coal tar is crushed and passed through a 100-mesh sieve to prepare asphalt powder, 3 parts of sodium polystyrene sulfonate and 12 parts of Dow Corning PMX-200 are mixed, heated to 255° C., stirred evenly, 125 parts of asphalt powder are added, stirred at 240° C. for 4 hours, 2 parts of silicon monoxide with a particle size of 3-5 μm are added, the temperature is reduced to 95° C., stirred for 6.5 hours, vacuum dried, nitrogen is used as a protective gas, the temperature is increased to 950° C., and the temperature is kept for 4.5 hours to obtain modified asphalt.
[0078] Comparative Example 5
[0079] The difference between this comparative example and Example 1 is that the primary graphite powder is not modified. Specifically, a regeneration process of a graphite negative electrode of a lithium-ion battery for a vehicle comprises the following steps:
[0080] (1) placing a graphite negative electrode sheet of a waste automotive lithium-ion battery and a separation aid in a kneader for kneading at a stirring speed of 18 rpm, a temperature of 25° C., and a time of 2.5 h, so that the graphite powder is peeled off from the copper foil to obtain a mixture containing separated graphite powder and copper foil; the separation aid comprises the following components in parts by weight: 52 parts of cycloalkanes, 40 parts of tetracyclic aromatic hydrocarbons, 18 parts of tricyclic aromatic hydrocarbons, and 2 parts of surfactants;
[0081] (2) passing the mixture containing the separated graphite powder and copper foil through a 30-mesh sieve to obtain a mixed slurry of copper foil and graphite powder;
[0082] (3) centrifuging the mixed slurry containing graphite powder to obtain wet graphite powder, washing it with deionized water for 4 times, separating it by filter pressing, and drying it to obtain primary graphite powder;
[0083] (4) A carbon source and primary graphite powder in a mass ratio of 0.5:1 were mixed, calcined at 850° C. for 6.5 h in a nitrogen atmosphere, and then cooled to room temperature to obtain a regenerated graphite material.
[0084] Comparative Example 6
[0085] The difference between this comparative example and Example 1 is that silicon monoxide is not added to the modified asphalt. Specifically, the preparation method of the modified asphalt is as follows: by weight, medium-temperature coal tar is crushed and passed through a 60-mesh sieve to prepare asphalt powder, 5.5 parts of sodium polystyrene sulfonate and 9 parts of Dow Corning PMX-200 are mixed, heated to 255°C, stirred evenly, 125 parts of asphalt powder are added, stirred at 240°C for 4h, cooled to 95°C, stirred for 6.5h, vacuum dried, nitrogen is used as a protective gas, the temperature is raised to 950°C, and the temperature is kept for 4.5h to obtain the modified asphalt.
[0086] Performance Testing
[0087] 1. The regenerated graphite prepared in Examples 1-3 and Comparative Examples 1-6 was uniformly mixed with a conductive agent (SP), a thickener (CMC), and a binder (SBR) in a mass ratio of 95.2:1:1.9:1.9, and then slurried, coated, and rolled to form a negative electrode sheet on a copper mesh, and then a lithium sheet was used as a counter electrode to make a button battery. Charge and discharge tests were performed in accordance with GB / T24533-2019 "Graphite Negative Electrode Materials for Lithium-ion Batteries", and full battery tests were performed using lithium iron phosphate as the positive electrode.
[0088] 2. The primary graphite powder prepared in Examples 1-3 and Comparative Examples 1-6 is tested for ash content, fixed carbon (%) = 100% - ash (%) - volatile matter (%). Specifically: accurately weigh two portions of 1 gram of primary graphite powder using an electronic analytical balance, put them into a double-covered porcelain crucible and a graphite boat of known weight, dry them in a drying oven at 105°C until they are balanced, and record the weights of the primary graphite powder G1 and G2. Put the double-covered porcelain crucible containing the primary graphite powder into a high-temperature furnace, keep it at a constant temperature of 950°C, use a stopwatch to count to 7 minutes, take it out and cool it to room temperature in a dryer, and weigh it G3; keep the graphite boat containing the primary graphite powder at a constant temperature of 950°C in a high-temperature furnace for 90 minutes, take it out, and cool it to room temperature. The weight of the material at this time is the weight of the ash content G4. First, the volatile matter V (%) of the primary graphite powder is calculated to be (G1-G3) / G1×100%, and the calculation formula for the purity of the primary graphite powder is obtained to be C (%)=[(G2-V-G4) / G2]×100%. The results are shown in Table 1.
[0089] Table 1 Performance test results
[0090]
[0091] It can be seen from Examples 1-3 that the purity of the primary graphite powder prepared by the present invention is higher than 99.95, and the lithium ion battery prepared therefrom has high specific capacity and good cycle stability, which improves the problem of low purity and poor performance of recycled graphite in the prior art.
[0092] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A regeneration process for graphite negative electrode of lithium-ion battery for vehicle, characterized in that: The following steps are involved: (1) placing a graphite negative electrode sheet of a waste automotive lithium-ion battery and a separation aid in a kneader for kneading at a stirring speed of 15-20 rpm, a temperature of 20-30° C., and a time of 2-3 h, so that the graphite powder is peeled off from the copper foil to obtain a mixture containing separated graphite powder and copper foil; the separation aid comprises the following components in parts by weight: 50-55 parts of cycloalkanes, 30-45 parts of tetracyclic aromatic hydrocarbons, 15-20 parts of tricyclic aromatic hydrocarbons, and 1-3 parts of surfactants; (2) passing the mixture containing the separated graphite powder and copper foil through a 30-40 mesh sieve to obtain a mixed slurry of copper foil and graphite powder; (3) centrifugally separating the mixed slurry containing graphite powder to obtain wet graphite powder, washing it with deionized water for 3-4 times, separating it by filter pressing, and drying it to obtain primary graphite powder; (4) dispersing 10 parts by mass of primary graphite powder in 30-40 parts by mass of deionized water to obtain a dispersion, adding 3-4 parts by mass of semicarbazide, and uniformly dispersing by ultrasonication, and then reacting at 170-180° C. for 17-20 hours, centrifuging, washing, and drying to obtain modified primary graphite powder; (5) Mixing a carbon source and modified primary graphite powder in a mass ratio of 0.3-0.6:1, calcining at 800-900°C for 6-7h under a nitrogen atmosphere, and cooling to room temperature to obtain a regenerated graphite material; The carbon source is modified asphalt; The preparation method of the modified asphalt is as follows: by weight, medium-temperature coal tar is crushed and sieved to prepare asphalt powder, 5-6 parts of sodium polystyrene sulfonate and 8-10 parts of dispersant are mixed, heated to 250-260° C., stirred evenly, 100-140 parts of asphalt powder are added, stirred at 230-250° C. for 3-5 hours, 3-6 parts of silicon monoxide are added, the temperature is reduced to 90-100° C., stirred for 6-7 hours, vacuum dried, nitrogen is used as protective gas, the temperature is increased to 900-1000° C., and the temperature is kept for 4-5 hours to obtain the modified asphalt; The surfactant is a compound of cocamidopropyl betaine, stearyl alcohol polyoxyethylene ether and sodium dodecylbenzene sulfonate in a mass ratio of 1:1.3-1.6:0.4-0.
8.
2. The regeneration process of a graphite negative electrode of a lithium-ion battery for a vehicle according to claim 1, characterized in that: The mass ratio of the graphite negative electrode sheet to the separator is 1:5-6.
3. The regeneration process of a graphite negative electrode of a lithium-ion battery for a vehicle according to claim 1, characterized in that: The dispersant is Dow Corning PMX-200.
4. The regeneration process of a graphite negative electrode of a lithium-ion battery for a vehicle according to claim 1, characterized in that: The particle size of the silicon monoxide is 3-5 μm.
5. The regeneration process of a graphite negative electrode of a lithium-ion battery for a vehicle according to claim 1, characterized in that: The sieving specifically includes sieving through a 60-80 mesh sieve.
6. A regenerated graphite negative electrode, characterized in that: The regenerated graphite negative electrode is made of regenerated graphite material prepared by the regeneration process described in any one of claims 1 to 5.