A modified flame-retardant fiberglass tile and production process

By adjusting the modified asphalt coating formula and using materials such as SBS modifier and slag powder, the anti-chloride ion penetration performance of the glass fiber tiles has been improved, and the problems in the existing technology when the glass fiber tiles are used in conjunction with reinforced concrete structures have been solved. Chloride ion penetration problem ensures safety performance.

CN117774458BActive Publication Date: 2024-10-22ZHEJIANG RONGPING BUILDING MATERIALS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311762113.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-20
Publication Date
2024-10-22
Estimated Expiration
2043-12-20

AI Technical Summary

Technical Problem

When existing fiberglass tiles are used in conjunction with reinforced concrete structures, their resistance to chloride ion penetration is poor, causing chloride ions to easily pass through and corrode the reinforced concrete structure, posing safety risks.

Method used

Adjust the formula of the modified asphalt coating, use SBS modifier to replace the polyolefin processing modifier, and the preferred fillers include slag powder and waste concrete powder, and improve the modified asphalt coating through the joint action of SBS modifier and slag powder density and resistance to chloride ion penetration.

Benefits of technology

The anti-chloride ion penetration performance of glass fiber tiles is significantly improved, effectively preventing chloride ion penetration, reducing the risk of corrosion to reinforced concrete structures, and ensuring safety performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004618872370000041
    Figure BDA0004618872370000041
  • Figure BDA0004618872370000051
    Figure BDA0004618872370000051
  • Figure BDA0004618872370000061
    Figure BDA0004618872370000061
Patent Text Reader

Abstract

The present application relates to the field of building materials technology, and specifically discloses a modified flame-retardant fiberglass tile and a production process. The fiberglass tile includes a fiberglass base, a modified asphalt coating, a covering layer and an isolation layer. The modified asphalt coating includes the following components by weight percentage: 41-53% asphalt, 1-3% SBS modifier, 18-22% magnesium hydroxide, 6-12% desulfurized regenerated rubber powder, 20-24% filler, the SBS modifier is a copolymer of SBS and an unsaturated monomer, the unsaturated monomer is acrylic acid, and the filler includes slag powder, and the amount of slag powder is 8-25% of the total weight of the filler. Under the joint action of the SBS modifier and the slag powder, the fiberglass tile of the present application has good resistance to chloride ion penetration, and can play a good protective effect when used in conjunction with reinforced concrete structures.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of building materials, and more specifically, to a modified flame-retardant fiberglass tile and a production process. Background Art

[0002] Fiberglass shingles (asphalt shingles) usually refer to fiberglass asphalt shingles, which are a commonly used waterproof material. They are mainly used for waterproofing roofs. The processing technology of fiberglass shingles usually uses fiberglass felt as the base. After the fiberglass felt is dipped in asphalt coating, it is covered with colored mineral granules on one side and an isolation material is set on the other side to obtain the finished fiberglass shingles. Fiberglass felt itself is a combustible building material. In order to improve the safety performance of fiberglass felt, it is necessary to develop fiberglass shingles with certain flame retardant properties.

[0003] A Chinese patent with publication number CN104358362A discloses a heat-insulating and flame-retardant asphalt shingle, comprising a glass fiber tire, a modified asphalt coating formed on the front and back surfaces of the glass fiber tire, respectively, a covering material layer and an isolation material layer respectively covered on the modified asphalt coating, wherein the raw material formula of the modified asphalt coating is as follows (by weight percentage): 40% of 10# petroleum asphalt; 6% of 90# road asphalt; 2% of polyolefin processing modifier; 20% of magnesium hydroxide; 9% of rubber powder; the balance of filler; the raw material formula of the covering material layer is as follows (by weight percentage): 35% of hollow ceramic microspheres; 2% of powdered styrene-butadiene rubber; the balance of colored sand.

[0004] With regard to the above-mentioned related technologies, the inventor believes that although the asphalt shingles in the related technologies can achieve a certain flame retardant effect, the addition of rubber powder will affect the anti-chloride ion penetration performance of the modified asphalt coating. When the asphalt shingles in the related technologies are used in conjunction with reinforced concrete structures, the chloride ions that pass through the asphalt shingles can easily cause corrosion of the reinforced concrete structure, causing certain safety hazards. Summary of the invention

[0005] In the related art, asphalt shingles have poor resistance to chloride ion penetration. When the asphalt shingles in the related art are used in conjunction with reinforced concrete structures, the chloride ions that pass through the asphalt shingles easily cause corrosion of the reinforced concrete structures, causing certain safety hazards. In order to improve this defect, the present application provides a modified flame-retardant fiberglass shingle and a production process.

[0006] In the first aspect, the present application provides a modified flame-retardant fiberglass tile, which adopts the following technical solution:

[0007] A modified flame-retardant fiberglass shingle, comprising a fiberglass base, a modified asphalt coating, a covering layer and an isolation layer, wherein the modified asphalt coating comprises the following components by weight percentage: 41-53% asphalt, 1-3% SBS modifier, 18-22% magnesium hydroxide, 6-12% desulfurized regenerated rubber powder, and 20-24% filler, wherein the SBS modifier is a copolymer of SBS and an unsaturated monomer, wherein the unsaturated monomer is acrylic acid, and the filler comprises slag powder, wherein the amount of the slag powder is 8-25% of the total weight of the filler.

[0008] By adopting the above technical scheme, the present application adjusts the formula of the modified asphalt coating, replaces the polyolefin processing modifier with an SBS modifier, and preferably selects fillers including slag powder. In the modified asphalt coating of the present application, the grafting of acrylic acid makes the SBS modifier carry a carboxyl group, which not only improves the compatibility between SBS and asphalt, but also the carboxyl group of the SBS modifier is easily adsorbed with components such as slag powder and magnesium hydroxide, thereby improving the bonding effect between the components of the modified asphalt coating, improving the density of the modified asphalt coating, and hindering the penetration of chloride ions. On this basis, slag powder can also produce a certain adsorption effect on chloride ions, which helps to reduce the chloride ion concentration in the modified asphalt coating. Under the joint action of the SBS modifier and slag powder, the glass fiber shingles of the present application can have better resistance to chloride ion penetration, and can play a good protective effect when used in conjunction with reinforced concrete structures.

[0009] Preferably, the SBS modifier is prepared according to the following method:

[0010] (1) SBS, unsaturated monomer, toluene and benzoyl peroxide acetone solution are mixed, heated and magnetically stirred under nitrogen protection, and the product is cooled after being kept at a constant temperature of 60-68° C. for 2-4 hours;

[0011] (2) adding anhydrous ethanol to the product, then performing rotary evaporation to remove ethanol, toluene and acetone, and then drying the residue at a constant temperature to a constant weight to obtain a crude SBS modifier;

[0012] (3) The crude SBS modifier is subjected to Soxhlet extraction to remove impurities and obtain the SBS modifier.

[0013] By adopting the above technical solution, the present application grafts acrylic acid into the SBS molecule under the initiation of benzoyl peroxide, and obtains the SBS modifier after removing impurities.

[0014] Preferably, in step (1) of preparing the SBS modifier, the reaction temperature is selected to be 64-68°C.

[0015] By adopting the above technical scheme, the reaction temperature in the process of preparing the SBS modifier is optimized, which is conducive to the full grafting of acrylic acid into the SBS molecules, improves the compatibility between the SBS modifier and asphalt, helps to enhance the density of the modified asphalt coating, and improves the chloride ion penetration resistance of the fiberglass shingles.

[0016] Preferably, in step (1) of preparing the SBS modifier, the reaction time is 3-4 h.

[0017] By adopting the above technical scheme, the reaction time in the process of preparing the SBS modifier is optimized, which is beneficial to the full grafting of acrylic acid into the SBS molecules, improves the compatibility between the SBS modifier and asphalt, helps to enhance the density of the modified asphalt coating, and improves the chloride ion penetration resistance of the fiberglass shingles.

[0018] Preferably, the unsaturated monomer is acrylic acid, and the weight ratio of acrylic acid to SBS is (0.6-1):1.

[0019] By adopting the above technical scheme, the weight ratio of acrylic acid to SBS is optimized, which is beneficial to the full grafting of acrylic acid into the SBS molecules, improves the compatibility between the SBS modifier and asphalt, helps to enhance the density of the modified asphalt coating, and improves the chloride ion penetration resistance of the fiberglass shingles.

[0020] Preferably, the amount of slag powder used is 17-25% of the total weight of the filler.

[0021] By adopting the above technical solution, the proportion of slag powder in the filler is optimized, which helps to improve the chloride ion penetration resistance of the fiberglass shingles.

[0022] Preferably, the filler further comprises waste concrete powder, the amount of the waste concrete powder is 1-10% of the weight of the filler, and the average particle size of the waste concrete powder is 35-140 μm.

[0023] By adopting the above technical scheme, the present application preferably selects that the filler component also includes waste concrete powder. The waste concrete powder is alkaline, which not only easily adheres to the acidic components in asphalt, but also can be adsorbed with the carboxyl groups in the SBS modifier, which helps to improve the density of the modified asphalt coating and improve the glass fiber shingles' resistance to chloride ion penetration.

[0024] Preferably, the average particle size of the waste concrete powder is 35-80 μm.

[0025] By adopting the above technical solution, the average particle size of the waste concrete powder is optimized, which helps to improve the density of the modified asphalt coating and improve the chloride ion penetration resistance of the fiberglass shingles.

[0026] Preferably, the amount of the waste concrete powder is 6-10% of the weight of the filler.

[0027] By adopting the above technical solution, the amount of waste concrete powder is optimized, which helps to improve the density of the modified asphalt coating and improve the chloride ion penetration resistance of the fiberglass shingles.

[0028] In a second aspect, the present application provides a method for preparing a modified flame-retardant fiberglass tile, which adopts the following technical solution.

[0029] A method for preparing a modified flame-retardant glass fiber tile comprises the following steps:

[0030] (1) adding asphalt into a reaction kettle, heating and melting, adding desulfurized regenerated rubber powder, continuing to heat to and stirring and dispersing, then cooling, adding SBS modifier, stirring and dispersing, and continuing to cool, then adding magnesium hydroxide and filler, stirring and dispersing again to obtain an asphalt coating material; mixing hollow ceramic microspheres, powdered styrene-butadiene rubber and colored sand to obtain a coating mixture;

[0031] (2) unrolling the rolled fiberglass tire, dipping the surface of the fiberglass tire with an asphalt coating material to form a modified asphalt coating, and spreading a covering mixture on the surface of the modified asphalt coating on the upper surface of the fiberglass tire to form a covering material layer after compaction;

[0032] (3) covering the surface of the asphalt-modified asphalt coating on the lower surface of the glass fiber tire with an insulating material to form an insulating material layer, thereby obtaining a glass fiber tile precursor;

[0033] (4) Cutting the glass fiber tile precursor into a set size to obtain a modified flame retardant glass fiber tile.

[0034] By adopting the above technical solution, the present application first prepares the asphalt coating material and the covering mixture respectively, and then applies the asphalt coating material to the front and back sides of the glass fiber tire to obtain a modified asphalt coating. Then, by spreading the covering mixture and the covering isolation material on the surface of the modified asphalt coating on the front and back sides of the glass fiber tire respectively, a modified flame-retardant glass fiber tile is finally obtained.

[0035] In summary, this application has the following beneficial effects:

[0036] 1. The present application adjusts the formula of the modified asphalt coating, replaces the polyolefin processing modifier with an SBS modifier, and preferably selects fillers including slag powder. Under the combined effect of the SBS modifier and the slag powder, the fiberglass shingles of the present application can have better resistance to chloride ion penetration and can play a good protective effect when used in conjunction with reinforced concrete structures.

[0037] 2. In this application, waste concrete powder is preferably used as one of the components of the filler. Waste concrete powder is alkaline, which not only easily adheres to the acidic components in asphalt, but also can be adsorbed with the carboxyl group in the SBS modifier, which helps to improve the density of the modified asphalt coating and improve the glass fiber shingles' resistance to chloride ion penetration. DETAILED DESCRIPTION

[0038] The present application is further described in detail below in conjunction with embodiments, preparation examples and comparative examples. The raw materials involved in the present application can all be obtained commercially.

[0039] Preparation Example of SBS Modifier

[0040] The following is an explanation using Preparation Example 1.

[0041] Preparation Example 1

[0042] In this preparation example, the SBS modifier was prepared according to the following method:

[0043] (1) SBS (1101 type, Yanshan Petrochemical), unsaturated monomer, toluene, and acetone solution of benzoyl peroxide were mixed, heated and magnetically stirred under nitrogen protection, and the product was cooled to 20° C. after constant temperature reaction at 60° C. for 2 h; the unsaturated monomer was acrylic acid, and the weight ratio of acrylic acid to SBS was 0.2:1; the ratio of toluene to SBS was 40 mL:1 g, the volume ratio of acetone to toluene was 1:1, and the amount of benzoyl peroxide was 0.5% of the weight of SBS;

[0044] (2) adding anhydrous ethanol to the product (the amount of ethanol is based on the amount of no new white flocculent precipitate in the container), and then performing rotary evaporation to remove ethanol, toluene and acetone, and then drying the residue at a constant temperature of 60° C. in a vacuum oven to a constant weight to obtain a crude SBS modifier;

[0045] (3) The crude SBS modifier was soaked in ethanol for 2 hours, then filtered, and the filtered product was wrapped with filter paper, put into a Soxhlet extractor, and extracted with acetone for 12 hours to obtain the SBS modifier.

[0046] As shown in Table 1, the difference between Preparation Examples 1-5 is that in step (1) of preparing the SBS modifier, the reaction temperatures selected are different.

[0047] Table 1 Reaction temperature

[0048] sample Reaction temperature / ℃ Preparation Example 1 60 Preparation Example 2 62 Preparation Example 3 64 Preparation Example 4 66 Preparation Example 5 68

[0049] As shown in Table 2, the difference between Preparation Examples 5-9 is that in step (1) of preparing the SBS modifier, the selected reaction time is different.

[0050] Table 2 Reaction time

[0051]

[0052]

[0053] As shown in Table 3, the difference between Preparation Examples 9-13 is that the weight ratio of acrylic acid to SBS is different.

[0054] Table 3 Weight ratio of acrylic acid to SBS

[0055] sample Acrylic acid:SBS Preparation Example 9 0.2:1 Preparation Example 10 0.4:1 Preparation Example 11 0.6:1 Preparation Example 12 0.8:1 Preparation Example 13 1:1 Example

[0056] The following description is given by taking Example 1 as an example.

[0057] Example 1

[0058] In this embodiment, the modified flame-retardant fiberglass shingle includes a fiberglass tire, a modified asphalt coating, a covering layer and an isolation layer. The modified asphalt coating is formed by dipping an asphalt coating material, the covering layer is made of a covering mixture, and the material of the isolation layer is LDPE. The thickness of the fiberglass tire is 1.2 mm, the thickness of the modified asphalt coating on the upper and lower surfaces of the fiberglass tire is 1.8 mm, the thickness of the covering layer is 1.7 mm, and the thickness of the isolation layer is 0.01 mm.

[0059] The modified asphalt coating includes the following components by weight percentage: 40% of 10# petroleum asphalt; 6% of 90# road asphalt; 2% of SBS modifier of Preparation Example 1; 20% of magnesium hydroxide (average particle size 2.3 μm); 9% of desulfurized regenerated rubber powder (60 mesh); and 23% of filler. The filler is composed of 200-mesh calcium carbonate and a specific surface area of ​​727 kg / m 3 The slag powder is mixed with slag powder, and the amount of slag powder is 8% of the total weight of the filler; the chemical composition of the slag powder is as follows: aluminum oxide 14.21%, calcium oxide 39.74%, silicon dioxide 28.35%, iron oxide 0.34%, sulfur trioxide 2.51%, magnesium oxide 8.69%, sodium oxide 0.43%, potassium oxide 0.29%, total chlorine 0.01%, LOI 5.40%.

[0060] The raw material formula of the covering layer is as follows: 35% of hollow ceramic microspheres (average particle size 38 μm); 63% of colored sand (30 mesh); and 2% of powdered styrene-butadiene rubber (1588).

[0061] In this embodiment, the modified flame retardant glass fiber tile is prepared according to the following steps:

[0062] (1) Add asphalt to a reactor, heat it to 140°C, add desulfurized regenerated rubber powder, continue to heat it to 175°C, stir and disperse it for 0.5h, cool it to 165°C, add SBS modifier, stir and disperse it for 0.5h, continue to cool it to 150°C, add magnesium hydroxide and filler, stir and disperse it for 0.5h, and prepare asphalt coating material; mix hollow ceramic microspheres, powdered styrene-butadiene rubber and colored sand to obtain a covering mixture;

[0063] (2) unrolling the rolled fiberglass tire, dipping the surface of the fiberglass tire with an asphalt coating material to form a modified asphalt coating, and spreading a covering mixture on the surface of the modified asphalt coating on the upper surface of the fiberglass tire to form a covering material layer after compaction;

[0064] (3) covering the surface of the asphalt-modified asphalt coating on the lower surface of the glass fiber tire with an insulating material to form an insulating material layer, thereby obtaining a glass fiber tile precursor;

[0065] (4) Cutting the glass fiber tile precursor into a set size to obtain a modified flame retardant glass fiber tile.

[0066] As shown in Table 4, the main difference between Examples 1-3 is that the raw material ratios of the modified asphalt coating are different.

[0067] Table 4 Raw material ratio of modified asphalt coating

[0068] sample Example 1 Example 2 Example 3 10# petroleum asphalt / % 40 32 46 90# road asphalt / % 6 9 7 SBS modifier / % 2 1 3 Magnesium hydroxide / % 20 22 18 Desulfurized recycled rubber powder / % 9 12 6 filler / % 23 24 20

[0069] Embodiment 4-15

[0070] As shown in Table 5, the difference between Examples 4-15 and Example 3 is that the preparation examples of the SBS modifier are different.

[0071] Table 5 Preparation example of SBS modifier

[0072]

[0073]

[0074] Examples 16-19

[0075] As shown in Table 6, the difference between Examples 16-19 and Example 15 is that the percentage of slag powder used in the total weight of the filler (hereinafter referred to as slag powder percentage) is different.

[0076] Table 6

[0077] sample Slag powder proportion / % Embodiment 15 8 Example 16 12 Embodiment 17 17 Embodiment 18 21 Embodiment 19 25

[0078] Embodiment 20

[0079] The difference between this embodiment and Embodiment 19 is that the filler also includes waste concrete powder, the amount of the waste concrete powder is 1% of the weight of the filler, the average particle size of the waste concrete powder is 140 μm, and the waste concrete powder is the residue after C40 concrete is crushed and sieved to remove aggregates.

[0080] As shown in Table 7, the difference between Examples 20-24 is that the average particle size of the waste concrete powder is different.

[0081] Table 7 Average particle size of waste concrete powder

[0082] sample Average particle size / μm Embodiment 20 140 Embodiment 21 115 Embodiment 22 80 Embodiment 23 57 Embodiment 24 35

[0083] As shown in Table 8, the difference between Examples 24-28 is that the percentage of the amount of waste concrete to the total weight of the filler (hereinafter referred to as the percentage of waste concrete powder) is different.

[0084] Table 8 Proportion of waste concrete powder

[0085]

[0086] Comparative Example

[0087]

[0088] Comparative Example 1

[0089] The asphalt shingles prepared with reference to Example 1 of the Chinese patent with announcement number CN104358362A are as follows:

[0090] A heat-insulating flame-retardant asphalt shingle comprises a glass fiber tire, a modified asphalt coating formed on the front and back surfaces of the glass fiber tire, and a covering material layer and an insulating material layer respectively covered on the modified asphalt coating. The thickness of the glass fiber tire is 1.2 mm, the thickness of the modified asphalt coating on the upper and lower surfaces of the glass fiber tire is 1.8 mm, the thickness of the covering material layer is 1.7 mm, and the thickness of the insulating material layer is 0.01 mm.

[0091] The raw material formula of modified asphalt coating is as follows: 40% of 10# petroleum asphalt; 6% of 90# road asphalt; 2% of oxidized polyethylene modifier (Honeywell Integrated Technology Co., Ltd., 8903); 20% of magnesium hydroxide (particle size 2-3 microns); 9% of desulfurized regenerated rubber powder (60 mesh); 23% of calcium carbonate. The raw material formula of the covering material is as follows: 35% of hollow ceramic microspheres (particle size 30-50 microns); 63% of colored sand (20-30 mesh); 2% of powdered styrene-butadiene rubber (1588).

[0092] The preparation process of heat-insulating flame-retardant asphalt shingles is as follows:

[0093] (1) Add 10# petroleum asphalt and 90# road asphalt into a reactor, heat it to 150°C, add rubber powder, continue to heat it to 180°C, stir and disperse it for 2.5 hours, cool it to 165°C, add oxidized polyethylene modifier, stir and disperse it for 1.0 hour, continue to cool it to 155°C, add magnesium hydroxide and calcium carbonate, stir and disperse it for 2.0 hours, and prepare asphalt coating material.

[0094] (2) The hollow ceramic microbeads, colored sand and powdered styrene-butadiene rubber are uniformly mixed to prepare a covering mixture.

[0095] (3) Unroll the rolled fiberglass tire and send it into an asphalt coating device filled with asphalt coating material for dipping and coating. The soaked tire base is then spread and compacted on the upper surface by the coating device, and the LDPE isolation material is covered on the lower surface. Finally, it is cut and packaged.

[0096] Comparative Example 2

[0097] The difference between this comparative example and Example 1 is that the SBS modifier is replaced by SBS (1101 type, Yanshan Petrochemical).

[0098] Comparative Example 3

[0099] The difference between this comparative example and Example 1 is that the slag powder in the filler is completely replaced by calcium carbonate.

[0100] Performance testing methods

[0101] 1. Chloride ion penetration resistance

[0102] Referring to JTJ 275-2000 "Technical Specifications for Anti-corrosion of Concrete Structures in Seaport Engineering", the fiberglass tiles were cut into circular specimens with a diameter of 48 mm, and the isolation layer was torn off. Then, the two sides of the specimens were exposed to 3% sodium chloride solution and deionized water respectively under normal pressure, and the containers of deionized water and sodium chloride solution were not connected to each other. On the 30th day, the chloride ion concentration on the deionized water side was tested.

[0103] Taking the chloride ion concentration measured in Comparative Example 1 as a benchmark, the ratio between the chloride ion concentration measured in each embodiment and comparative example and the chloride ion concentration measured in Comparative Example 1 was calculated, and the ratio was recorded as the relative chloride ion permeability. The results are shown in Table 9.

[0104] 2. Flame retardant properties

[0105] The flame retardancy test of the glass fiber shingles of each embodiment and comparative example (asphalt shingles of comparative example 1) showed that the flame retardancy was B1 and difficult to burn.

[0106] Table 9 Relative permeability of chloride ions

[0107]

[0108] Combining Example 1 and Comparative Example 1 and Table 9, it can be seen that the relative chloride ion penetration measured in Example 1 is less than that in Comparative Example 1, indicating that the modified flame-retardant glass fiber shingles of the present application achieve better resistance to chloride ion penetration by adding SBS modifier and slag powder, which helps to reduce the damage of chloride ion penetration to reinforced concrete structures.

[0109] Combining Example 1 and Comparative Examples 2-3 with Table 9, it can be seen that when the modified asphalt coating lacks any of the SBS modifier and the slag powder, it is difficult for the modified flame-retardant glass fiber shingles to achieve good resistance to chloride ion penetration.

[0110] It can be seen from Examples 3-7 and Table 9 that in step (1) of preparing the SBS modifier, when the reaction temperature is 64-68°C, the reaction between acrylic acid and SBS is more complete, which improves the compatibility between the SBS modifier and asphalt, helps to enhance the density of the modified asphalt coating, and improves the chloride ion penetration resistance of the fiberglass shingles.

[0111] It can be seen from Examples 7-11 and Table 9 that in step (1) of preparing the SBS modifier, when the selected reaction time is 3-4h, it is conducive to the full grafting of acrylic acid into the SBS molecules, thereby improving the compatibility between the SBS modifier and asphalt, helping to enhance the density of the modified asphalt coating, and improving the chloride ion penetration resistance of the fiberglass shingles.

[0112] It can be seen from Examples 11-15 and Table 9 that in the preparation example of the SBS modifier, when the weight ratio of acrylic acid to SBS is (0.6-1):1, it is beneficial to fully graft acrylic acid into the SBS molecule, improves the compatibility between the SBS modifier and asphalt, helps to enhance the density of the modified asphalt coating, and improves the chloride ion penetration resistance of the fiberglass shingles.

[0113] It can be seen from Examples 15-19 and Table 9 that when the amount of slag powder is 17-25% of the total weight of the filler, it helps to enhance the density of the modified asphalt coating and improve the chloride ion penetration resistance of the fiberglass shingles.

[0114] Combining Example 19, Example 20 and Table 9, it can be seen that the relative chloride ion permeability measured in Example 20 is less than that in Example 19, indicating that the addition of waste concrete powder helps to improve the chloride ion penetration resistance of the fiberglass tile.

[0115] It can be seen from Examples 20-28 and Table 9 that when the average particle size of the waste concrete powder is 35-80 μm and the dosage is 6-10% of the filler weight, the glass fiber tile has relatively good resistance to chloride ion penetration.

[0116] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A modified flame retardant fiberglass tile, It is characterized in that The fiberglass shingle comprises a fiberglass base, a modified asphalt coating, a covering layer and an isolation layer. The modified asphalt coating comprises the following components by weight percentage: 41-53% asphalt, 1-3% SBS modifier, 18-22% magnesium hydroxide, 6-12% desulfurized regenerated rubber powder, and 20-24% filler. The SBS modifier is a copolymer of SBS and an unsaturated monomer, and the unsaturated monomer is acrylic acid. The filler comprises slag powder, and the amount of the slag powder is 8-25% of the total weight of the filler. The SBS modifier is prepared as follows: (1) SBS, unsaturated monomer, toluene and benzoyl peroxide acetone solution are mixed, heated and magnetically stirred under nitrogen protection, and the product is cooled after being reacted at a constant temperature of 64-68°C for 2-4 hours; (2) adding anhydrous ethanol to the product, then performing rotary evaporation to remove ethanol, toluene and acetone, and then drying the residue at a constant temperature to a constant weight to obtain a crude SBS modifier; (3) The crude SBS modifier is subjected to Soxhlet extraction to remove impurities and obtain the SBS modifier.

2. The modified flame retardant glass fiber tile according to claim 1, It is characterized in that In the step (1) of preparing the SBS modifier, the selected reaction time is 3-4 hours.

3. The modified flame retardant glass fiber tile according to claim 1, It is characterized in that The unsaturated monomer is acrylic acid, and the weight ratio of acrylic acid to SBS is (0.6-1):

1.

4. The modified flame retardant glass fiber tile according to claim 1, It is characterized in that The amount of the slag powder used is 17-25% of the total weight of the filler.

5. The modified flame retardant glass fiber tile according to claim 4, It is characterized in that The filler also includes waste concrete powder, the amount of the waste concrete powder is 1-10% of the weight of the filler, and the average particle size of the waste concrete powder is 35-140 μm.

6. The modified flame retardant glass fiber tile according to claim 5, It is characterized in that The average particle size of the waste concrete powder is 35-80 μm.

7. The modified flame retardant glass fiber tile according to claim 6, It is characterized in that The amount of the waste concrete powder is 6-10% of the weight of the filler.

8. A method for preparing a modified flame-retardant glass fiber tile according to any one of claims 1 to 7, It is characterized in that The following steps are involved: (1) Add asphalt into a reactor, heat and melt, then add desulfurized regenerated rubber powder, continue to heat to and stir and disperse, then cool down, add SBS modifier, continue to cool down after stirring and dispersing, then add magnesium hydroxide and filler, stir and disperse again to obtain asphalt coating material; Mixing hollow ceramic microspheres, powdered styrene-butadiene rubber and colored sand to obtain a covering mixture; (2) Unrolling the rolled fiberglass tire, dipping the surface of the fiberglass tire with an asphalt coating material to form a modified asphalt coating, and spreading a covering mixture on the surface of the modified asphalt coating on the upper surface of the fiberglass tire to form a covering material layer after compaction; (3) Covering the surface of the asphalt-modified asphalt coating on the lower surface of the glass fiber tire with an insulating material to form an insulating material layer, thereby obtaining a glass fiber tile precursor; (4) Cutting the glass fiber tile precursor into a set size to obtain a modified flame retardant glass fiber tile.