Yellowing-resistant, highly wettable ultra-thin component positioning tape and preparation method thereof

By using a combination structure of UV coating, PET substrate layer, high wet primer layer and high temperature pressure-sensitive adhesive layer in the photovoltaic module positioning tape, the existing tape is solved by resistant to yellowing and deterioration during the lamination process and The problem of insufficient adhesive strength achieves stronger adhesiveness and cohesive strength, ensuring the stable positioning of the battery cell.

CN117801696BActive Publication Date: 2024-12-03SUZHOU TONYSHARE ELECTRONICS MATERIALS TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311827472.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-28
Publication Date
2024-12-03
Estimated Expiration
2043-12-28

AI Technical Summary

Technical Problem

During the lamination process, existing photovoltaic module positioning tapes have problems such as yellowing resistance, insufficient adhesiveness, layering and bubble formation, and the reduction in viscosity at high temperatures makes it difficult to prevent cell deviation.

Method used

Using a combined structure of anti-UV coating, PET substrate layer, high wet primer layer and high temperature pressure-sensitive adhesive layer, the anti-UV coating is triggered by polyurethane acrylate oligomer, UVB type anti-UV absorber and UVA type The high wet primer is composed of amorphous polyester and hydrophilic oxide, and the high-temperature pressure-sensitive adhesive layer is silicone-type, which forms ultra-thin component positioning tape through UV curing and baking processes.

Benefits of technology

It improves the UV aging resistance, adhesion and cohesion strength of the tape, enhances the fixing ability of the battery cell, reduces production costs, and maintains good viscosity at high temperatures, avoiding cell deviation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117801696B_ABST
    Figure CN117801696B_ABST
Patent Text Reader

Abstract

The present invention provides a photovoltaic positioning tape with high temperature resistance and high adhesive force and a preparation method thereof, including an anti-ultraviolet coating, a PET substrate layer 1, a high-wetting primer layer and a high-temperature resistant pressure-sensitive adhesive layer arranged in sequence; the anti-ultraviolet coating is a UV curing coating, and the UV curing coating includes the following components according to mass fraction: 30-60 parts of polyurethane acrylate oligomer, 30-60 parts of mixed reactive diluent, 1-5 parts of silane coupling agent, 0.5-2 parts of UVB type anti-ultraviolet absorber, and 1-3 parts of UVA type initiator; the mixed diluent is IBOA:THFA mixed in a ratio of 2:3 to 3:2. The present invention has a simple structure and can effectively and systematically solve the problems of poor yellowing resistance of photovoltaic positioning tape, poor bonding strength with adhesive film during lamination, reduced adhesiveness of acrylic pressure-sensitive adhesive during high-temperature lamination, and separation from battery cells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of photovoltaic materials, and in particular to a yellowing-resistant, highly wettable ultra-thin component positioning tape and a preparation method thereof. Background Art

[0002] In photovoltaic modules, in order to prevent the cell from shifting due to the fluidity of the melted adhesive film during lamination, acrylic pressure-sensitive tape is usually used to fix the cell.

[0003] The acrylic pressure-sensitive adhesive tape used in the prior art has many problems such as poor yellowing resistance, poor bonding with the adhesive film during lamination, reduced adhesion of the acrylic pressure-sensitive adhesive during high-temperature lamination, and separation from the battery cell.

[0004] Patent CN113528032A proposes a simple upper and lower layer structure that is bonded to the adhesive film and the battery, but does not disclose the adhesive formula. In addition, the adhesive base layer itself will melt at the lamination temperature, causing the positioning tape structure to be destroyed, and basically cannot prevent the battery cell from shifting.

[0005] Patent CN114891452A only focuses on solving the yellowing resistance problem of the positioning tape, but does not solve the bonding problem and the delamination and bubbling problems that occur in the later lamination. Summary of the invention

[0006] The technical problem solved by the invention is to provide a yellowing-resistant high-wetting ultra-thin component positioning tape, which has good wetting performance and good yellowing resistance.

[0007] The technical solution adopted by the present invention to solve the technical problem is: a yellowing-resistant high-wetting ultra-thin component positioning tape, comprising an anti-ultraviolet coating, a PET substrate layer, a high-wetting primer layer and a high-temperature resistant pressure-sensitive adhesive layer arranged in sequence;

[0008] The anti-ultraviolet coating is a UV curing coating, and the UV curing coating comprises the following components by mass fraction: 30-60 parts of polyurethane acrylate oligomer, 30-60 parts of mixed reactive diluent, 1-5 parts of silane coupling agent, 0.5-2 parts of UVB type anti-ultraviolet absorber, and 1-3 parts of UVA type initiator;

[0009] The mixed diluent is IBOA and THFA, IBOA:THFA=2:3~3:2.

[0010] Furthermore, the high wettability primer layer is composited by non-crystalline polyester and hydrophilic oxide;

[0011] The high wettability coating comprises the following components in terms of mass fraction: 10-30 parts of non-crystalline polyester, 50-80 parts of solvent, 5-10 parts of hydrophilic oxide, and 3-10 parts of amino curing agent.

[0012] Furthermore, the molecular weight of the non-crystalline polyester is 3000-8000, and the glass transition temperature is 7-20°C.

[0013] Furthermore, the solvent is one or more of toluene, ethyl acetate and butanone.

[0014] Furthermore, the hydrophilic oxide is one or more of zirconium oxide and cerium oxide.

[0015] Furthermore, the amino curing agent is an amino resin, and the amino resin can be one or more of Cytec 303 and Cytec 327.

[0016] Furthermore, the high temperature resistant pressure sensitive adhesive layer is a silicone type pressure sensitive adhesive.

[0017] The present invention also discloses a method for preparing a yellowing-resistant high-wetting ultra-thin component positioning tape, comprising the mass fractions and proportions of the yellowing-resistant high-wetting ultra-thin component positioning tape described above, and the steps of:

[0018] S1: The anti-ultraviolet coating is coated on one side of the PET substrate layer by gravure or micro-concave process, and then irradiated for 3-5 seconds at a light intensity of 1500-2500mJ / cm2, and then rolled up for use;

[0019] S2: The high wettability primer layer is coated on one side of the PET substrate layer using a micro-concave or gravure process, baked in an oven at 130°C for 2-3 minutes, and then rolled up for use;

[0020] S3: The high temperature resistant pressure-sensitive adhesive layer is coated on the side of the high wettability base coating away from the PET substrate layer by using a comma blade or lip extrusion process, and is baked in an oven at 150°C for 1-3 minutes after coating, and finally rolled up to form a finished product.

[0021] The beneficial effects of the present invention are:

[0022] In the present invention, the anti-ultraviolet coating is made of excellent weather-resistant polyurethane acrylic resin, matched with UVB type anti-ultraviolet absorber and UVA type photoinitiator, which ensures the excellent anti-ultraviolet aging performance of the coating while ensuring UV curing, and adopts UV curing technology to increase the coating speed and reduce the production cost.

[0023] The addition of silane coupling agent in the anti-ultraviolet layer of the present invention can make the adhesion with EVA in the photovoltaic module stronger.

[0024] The resin in the high wetting coating contains a large amount of hydroxyl groups, and the oxides also form stable chemical bonds with the silicon atoms in the silica gel, so that the high wetting primer layer and the PET layer or the high temperature resistant pressure-sensitive adhesive layer have good wettability, thereby improving the cohesive strength of the tape itself. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a schematic structural diagram of the yellowing-resistant, highly wettable ultra-thin component positioning tape according to an embodiment of the present application.

[0026] Marked in the figure are: anti-ultraviolet coating 1, PET substrate layer 2, high-wetting primer layer 3, and high-temperature resistant pressure-sensitive adhesive layer 4. DETAILED DESCRIPTION

[0027] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and understandable, the specific implementation methods of the present invention are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present invention.

[0028] The embodiment of the present application discloses a yellowing-resistant high-wetting ultra-thin component positioning tape, which is characterized by comprising an anti-ultraviolet coating, a PET substrate layer, a high-wetting primer layer and a high-temperature resistant pressure-sensitive adhesive layer arranged in sequence;

[0029] The anti-ultraviolet coating is a UV curing coating, and the UV curing coating comprises the following components by mass fraction: 30-60 parts of polyurethane acrylate oligomer, 30-60 parts of mixed reactive diluent, 1-5 parts of silane coupling agent, 0.5-2 parts of UVB type anti-ultraviolet absorber, and 1-3 parts of UVA type initiator;

[0030] The mixed diluent is IBOA and THFA, IBOA:THFA=2:3~3:2.

[0031] Specifically, the polyurethane acrylate oligomer can be 30 parts, 40 parts, 60 parts, etc., the mixed active diluent can be 30 parts, 40 parts, 60 parts, etc., the silane coupling agent can be 1 part, 3 parts, 5 parts, etc., the UVB type anti-ultraviolet absorber can be 0.5 parts, 1 part, 2 parts, etc., the UVA type initiator can be 1 part, 2 parts, 3 parts, etc., and the ratio of IBOA to THFA can be 2:3, 3:2, etc.

[0032] In this application, the anti-ultraviolet coating uses excellent weather-resistant polyurethane acrylate oligomers, UVB type anti-ultraviolet absorbers, and UVA type photoinitiators, which ensures UV curing while ensuring the excellent anti-ultraviolet aging performance of the coating. In addition, the use of UV curing technology increases the coating speed and reduces the production cost.

[0033] In this embodiment, the high wettability primer layer is composited by non-crystalline polyester and hydrophilic oxide; the high wettability primer layer comprises the following components in terms of mass fraction: 10-30 parts of non-crystalline polyester, 50-80 parts of solvent, 5-10 parts of hydrophilic oxide, and 3-10 parts of amino curing agent.

[0034] Specifically, the molecular weight of the non-crystalline polyester is 3000-8000, the glass transition temperature is 7-20°C, the solvent is one or more of toluene, ethyl acetate, and butanone, the hydrophilic oxide is one or more of zirconium oxide and cerium oxide, the amino curing agent is an amino resin, and the amino resin can be one or more of Cytec 303 and Cytec 327.

[0035] In the present application, the resin in the high wettability coating contains a large amount of hydroxyl groups, and the oxides also form stable chemical bonds with the silicon atoms in the silica gel, so that the primer and PET or the silicone pressure-sensitive adhesive coating form good wettability, thereby improving the cohesive strength of the tape itself.

[0036] The present invention also discloses a method for preparing a yellowing-resistant high-wetting ultra-thin component positioning tape, comprising the mass fractions and proportions of the yellowing-resistant high-wetting ultra-thin component positioning tape described above, characterized in that the steps are:

[0037] S1: The anti-ultraviolet coating is coated on one side of the PET substrate layer by gravure or micro-concave process, and then irradiated at a light intensity of 1500-2500mJ / cm2 for 3-5s, and then rolled up;

[0038] S2: The high wettability primer layer is coated on one side of the PET substrate layer using a micro-concave or gravure process, baked in an oven at 130°C for 2-3 minutes, and then rolled up;

[0039] S3: The high temperature resistant pressure-sensitive adhesive layer is coated on the side of the high wettability primer layer away from the PET substrate layer by using a comma blade or lip extrusion process. After coating, it is baked in an oven at 150°C for 1-3 minutes and finally rolled up.

[0040] The following are several specific embodiments of this application:

[0041] Example 1

[0042] 1. The tape structure is designed according to the anti-ultraviolet coating 2um, the PET substrate layer 18um, the high wettability primer layer 1um, and the high temperature resistant pressure-sensitive adhesive layer 20um.

[0043] 2. Design the anti-ultraviolet UV coating formula according to the following mass fractions: 40 parts of polyurethane acrylate oligomer, 30 parts of mixed active diluent, 2 parts of silane coupling agent, 0.5 parts of UVB anti-ultraviolet absorber, and 3 parts of UVA initiator. The mixed diluent is IBOA:THFA mixed in a ratio of 2:3.

[0044] 3. Design a high wetting coating formula according to the following mass fractions: 10 parts of non-crystalline polyester, 50 parts of ethyl acetate, 5 parts of cerium oxide, and 5 parts of 327 amino curing agent. The non-crystalline polyester has a molecular weight of 6000 and a glass transition temperature of 13°C.

[0045] 4. Prepare the tape according to the following process:

[0046] S1: The anti-ultraviolet coating is coated on one side of the PET substrate layer using a gravure or micro-concave process. After coating, the UV resistance is 1900mJ / cm 2 Irradiate under strong light for 3s and finally roll it up.

[0047] S2: The high wettability primer layer is coated on one side of the PET substrate layer by using a micro-concave or gravure process, and is baked in an oven at 130°C for 2 minutes after coating, and finally rolled up.

[0048] S3: The high temperature resistant pressure sensitive adhesive layer is coated on the side of the high wettability base coating away from the PET substrate layer by using a comma blade or lip extrusion process, and then baked in an oven at 150°C for 2 minutes. Finally, it is rolled up.

[0049] Example 2

[0050] 1. The tape structure is designed according to the anti-ultraviolet coating 2um, PET substrate layer 38um, high wettability primer layer 1um, and high temperature resistant pressure-sensitive adhesive layer 30um.

[0051] 2. Design the anti-ultraviolet UV coating formula according to the following mass fractions: 40 parts of polyurethane acrylate oligomer, 30 parts of mixed active diluent, 2 parts of silane coupling agent, 0.5 parts of UVB anti-ultraviolet absorber, and 3 parts of UVA initiator. The mixed diluent is IBOA:THFA mixed in a ratio of 2:3.

[0052] 3. Design a high wetting coating formula according to the following mass fractions: 10 parts of non-crystalline polyester, 50 parts of ethyl acetate, 5 parts of cerium oxide, and 5 parts of 327 amino curing agent. The non-crystalline polyester has a molecular weight of 6000 and a glass transition temperature of 13°C.

[0053] 4. Prepare the tape according to the following process:

[0054] S1: The anti-ultraviolet coating is coated on one side of the PET substrate layer using a gravure or micro-concave process. After coating, the UV resistance is 1900mJ / cm2 Irradiate under strong light for 3s and finally roll it up.

[0055] S2: The high wettability primer layer is coated on one side of the PET substrate layer by using a micro-concave or gravure process, and is baked in an oven at 130°C for 2 minutes after coating, and finally rolled up.

[0056] S3: The high temperature resistant pressure sensitive adhesive layer is coated on the side of the high wettability base coating away from the PET substrate layer by using a comma blade or lip extrusion process, and then baked in an oven at 150°C for 2 minutes. Finally, it is rolled up.

[0057] Example 3

[0058] 1. The tape structure is designed according to the anti-ultraviolet coating 2um, the PET substrate layer 18um, the high-wetting primer layer 1um, and the high-temperature resistant pressure-sensitive adhesive layer 20um.

[0059] 2. Design the anti-ultraviolet UV coating formula according to the following mass fractions: 50 parts of polyurethane acrylate oligomer, 35 parts of mixed active diluent, 5 parts of silane coupling agent, 1 part of UVB type anti-ultraviolet absorber, and 3 parts of UVA type initiator. The mixed diluent is IBOA:THFA mixed in a ratio of 2:3.

[0060] 3. Design a high wetting coating formula according to the following mass fractions: 10 parts of non-crystalline polyester, 50 parts of ethyl acetate, 5 parts of cerium oxide, and 5 parts of 327 amino curing agent. The non-crystalline polyester has a molecular weight of 6000 and a glass transition temperature of 13°C.

[0061] 4. Prepare the tape according to the following process:

[0062] S1: The anti-ultraviolet coating is coated on one side of the PET substrate layer using a gravure or micro-concave process. After coating, the UV resistance is 1900mJ / cm 2 Irradiate under strong light for 3s and finally roll it up.

[0063] S2: The high wettability primer layer is coated on one side of the PET substrate layer by using a micro-concave or gravure process, and is baked in an oven at 130°C for 2 minutes after coating, and finally rolled up.

[0064] S3: The high temperature resistant pressure sensitive adhesive layer is coated on the side of the high wettability base coating away from the PET substrate layer by using a comma blade or lip extrusion process, and then baked in an oven at 150°C for 2 minutes. Finally, it is rolled up.

[0065] Example 4

[0066] 1. The tape structure is designed according to the anti-ultraviolet coating 2um, PET substrate layer 38um, high wettability primer layer 1um, and high temperature resistant pressure-sensitive adhesive layer 30um.

[0067] 2. Design the anti-ultraviolet UV coating formula according to the following mass fractions: 40 parts of polyurethane acrylate oligomer, 30 parts of mixed active diluent, 2 parts of silane coupling agent, 0.5 parts of UVB anti-ultraviolet absorber, and 3 parts of UVA initiator. The mixed diluent is IBOA:THFA mixed in a ratio of 2:3.

[0068] 3. Design a high wetting coating formula according to the following mass fractions: 15 parts of non-crystalline polyester, 50 parts of ethyl acetate, 5 parts of cerium oxide, and 5 parts of 327 amino curing agent. The non-crystalline polyester has a molecular weight of 6000 and a glass transition temperature of 13°C.

[0069] 4. Prepare the tape according to the following process:

[0070] S1: The anti-ultraviolet coating is coated on one side of the PET substrate layer using a gravure or micro-concave process. After coating, the UV resistance is 1900mJ / cm 2 Irradiate under strong light for 3s and finally roll it up.

[0071] S2: The high wettability primer layer is coated on one side of the PET substrate layer by using a micro-concave or gravure process, and is baked in an oven at 130°C for 2 minutes after coating, and finally rolled up.

[0072] S3: The high temperature resistant pressure sensitive adhesive layer is coated on the side of the high wettability base coating away from the PET substrate layer by using a comma blade or lip extrusion process, and then baked in an oven at 150°C for 2 minutes. Finally, it is rolled up.

[0073] Comparative Example 1

[0074] 1. The tape structure is designed according to the PET substrate layer of 18um, the high wettability primer layer of 1um, and the high temperature resistant pressure sensitive adhesive layer of 20um.

[0075] 2 The high wetting coating formula was designed according to the following mass fractions: 10 parts of non-crystalline polyester, 50 parts of ethyl acetate, 5 parts of cerium oxide, and 5 parts of 327 amino curing agent. The non-crystalline polyester has a molecular weight of 6000 and a glass transition temperature of 13°C.

[0076] 4. Prepare the tape according to the following process:

[0077] S1: The high wettability primer layer is coated on one side of the PET substrate layer by using a micro-concave or gravure process, and is baked in an oven at 130°C for 2 minutes after coating, and finally rolled up.

[0078] S2: The high temperature resistant pressure sensitive adhesive layer is coated on the side of the high wettability base coating away from the PET substrate layer by using a comma blade or lip extrusion process, and then baked in an oven at 150°C for 2 minutes and finally rolled up.

[0079] Comparative Example 2

[0080] 1. The tape structure is designed according to the anti-ultraviolet coating 2um, the PET substrate layer 18um, and the high temperature resistant pressure sensitive adhesive layer 20um.

[0081] 2. Design the anti-ultraviolet UV coating formula according to the following mass fractions: 40 parts of polyurethane acrylate oligomer, 30 parts of mixed active diluent, 2 parts of silane coupling agent, 0.5 parts of UVB anti-ultraviolet absorber, and 3 parts of UVA initiator. The mixed diluent is IBOA:THFA mixed in a ratio of 2:3.

[0082] 4. Prepare the tape according to the following process:

[0083] S1: Anti-ultraviolet coating is applied on one side of the PET substrate layer by gravure or micro-concave process. After coating, the UV resistance is 1900mJ / cm 2 Irradiate under strong light for 3s and finally roll it up.

[0084] S2: The high temperature resistant pressure sensitive adhesive layer is coated on the other side of the PET substrate layer by using a comma blade or lip extrusion process, and then baked in an oven at 150°C for 2 minutes. Finally, it is rolled up.

[0085] The following is the test of yellowing resistance grade, water boiling, and the peeling force of the tape on the silicon wafer for the above 4 embodiments and 2 comparative examples.

[0086] When testing the yellowing resistance level: use a transmittance tester and a tensile machine to perform QUV testing. The total test power reaches 60 kWh and is divided into levels 0-5, where 0 represents no discoloration and 5 represents severe discoloration.

[0087] Boiling degumming test: Put the positioning tape into a water bath and boil it for about 24 hours, then take it out and wipe off the surface moisture, and rub the silicone layer of the positioning tape under the corresponding weights. Observe whether the silicone layer falls off.

[0088] Peel force test: Cut the positioning tape into strips of about 25mm wide and 300mm long, stick the positioning tape on the silicon battery cell, let it stand for 20 minutes, and then use a peel force tester to test it.

[0089] Serial number Yellowing resistance Boiling degumming test Silicon wafer peeling force (gif / in) Example 1 Level 1 No degumming 830 Example 2 Level 1 No degumming 990 Example 3 Level 1 No degumming 843 Example 4 Level 1 No degumming 845 Comparative Example 1 Level 3 No degumming 790 Comparative Example 2 Level 1 Degumming /

[0090] It can be seen from Example 1 and Comparative Example 1 that after adding the anti-ultraviolet coating, the yellowing resistance of the positioning tape is significantly improved. It can be seen from Example 1 and Comparative Example 2 that after adding the high-wetting coating, the silicone heat-resistant coating of the positioning tape will not debond, showing good wettability.

[0091] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A yellowing-resistant, highly wettable ultra-thin component positioning tape, characterized in that: It includes an anti-ultraviolet coating, a PET substrate layer, a high-wetting primer layer and a high-temperature resistant pressure-sensitive adhesive layer which are arranged in sequence; The anti-ultraviolet coating is a UV curing coating, and the UV curing coating comprises the following components in parts by mass: 30-60 parts of polyurethane acrylate oligomer, 30-60 parts of mixed reactive diluent, 1-5 parts of silane coupling agent, 0.5-2 parts of UVB type anti-ultraviolet absorber, and 1-3 parts of UVA type initiator; The mixed active diluent is IBOA and THFA, IBOA:THFA=2:3~3:2; The high-wetting primer layer is composed of the following components in parts by mass: 10-30 parts of non-crystalline polyester, 50-80 parts of solvent, 5-10 parts of cerium oxide, and 3-10 parts of amino curing agent.

2. The yellowing-resistant, highly wettable ultra-thin component positioning tape according to claim 1, characterized in that: The molecular weight of the non-crystalline polyester is 3000-8000, and the glass transition temperature is 7-20°C.

3. The yellowing-resistant, highly wettable ultra-thin component positioning tape according to claim 1, characterized in that: The solvent is one or more of toluene, ethyl acetate and butanone.

4. The yellowing-resistant, highly wettable ultra-thin component positioning tape according to claim 1, characterized in that: The amino curing agent is an amino resin, and the amino resin is one or more of Cytec 303 and Cytec 327.

5. The yellowing-resistant, highly wettable ultra-thin component positioning tape according to claim 1, characterized in that: The high temperature resistant pressure sensitive adhesive layer is a silicone type pressure sensitive adhesive.

6. A method for preparing a yellowing-resistant high-wetting ultra-thin component positioning tape, comprising the mass fractions and proportions of the yellowing-resistant high-wetting ultra-thin component positioning tape according to any one of claims 1 to 5, characterized in that: The steps are: S1: The anti-ultraviolet coating is coated on one side of the PET substrate layer by gravure process, and then irradiated at a light intensity of 1500-2500mJ / cm2 for 3-5s, and then rolled up; S2: The high-wetting primer layer is coated on one side of the PET substrate layer using a gravure process, baked in an oven at 130°C for 2-3 minutes, and then rolled up; S3: The high temperature resistant pressure-sensitive adhesive layer is coated on the side of the high wettability primer layer away from the PET substrate layer by using a comma blade or lip extrusion process. After coating, it is baked in an oven at 150°C for 1-3 minutes and finally rolled up.

Citation Information

Patent Citations

  • Positioning adhesive tape for photovoltaic module lamination

    CN113528032A

  • High-performance weather-resistant adhesive tape

    CN217578748U

  • Primer composition, kit, laminate and adhesive tape

    JP7263487B1