A method for determining the optimal exposure energy for light source-induced dry film forming
The optimal exposure energy determination method for light source-induced dry film molding solves the problem of inconsistent cross-sectional shapes of dry film circuits, enables accurate characterization and parameter adjustment of dry film circuits, and improves the yield and process capabilities of fine circuit production.
Patent Information
- Application Number
- CN202311836705.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-28
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-12-28
AI Technical Summary
The existing technology cannot accurately obtain the top and bottom line width information of dry film lines, resulting in inconsistent cross-sectional shapes of dry film lines, which affects the quality and signal integrity of subsequent graphic electroplated copper lines. Moreover, conventional characterization methods are cumbersome and the test cycle is long, making it impossible to timely Adjusting the parameters used in the production process reduces product yield and reliability.
The optimal exposure energy method for light source induced dry film formation is determined, including hot pressing of the dry film after micro-etching, gradient exposure and rapid development, through metallographic section preparation and 3D laser microscope observation, and using Image J software to measure the dry film line. The top and bottom line widths are selected to select the optimal exposure energy to ensure the vertical state of the sidewalls of the patterned electroplated copper lines and a stable line width/line space ratio.
It achieves accurate acquisition of dry film circuit cross-sectional shape information, provides appropriate exposure parameter guidance, improves the yield and process capabilities of fine circuit production, and ensures good vertical status and stable line width/line of graphic electroplated copper circuits. distance ratio.
Smart Images

Figure CN117806128B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of PCB board preparation, and particularly relates to a method for determining optimal exposure energy for light source-induced dry film forming. Background Art
[0002] In the context of the diversification and multi-functional complexity of consumer electronic products, the printed circuit board (PCB), as the carrier of the "mother of electronic products", realizes the electrical connection of electronic components, and it is constantly moving towards high density, high integration, high frequency and high speed. As one of the most forward-looking fine circuit manufacturing processes for PCB, the refinement and quality reliability of the circuits made by the modified semi-additive process (mSAP) can meet the needs of high-end electronic products. The mSAP process can make the signal lines more densely distributed and reduce the risk of short circuits. The wire spacing can be shortened to 25μm, thereby saving circuit wiring space and improving signal transmission on PCB. Therefore, it has a unique advantage to use mSAP as the leading process to make fine circuits to achieve the lightness, thinness and miniaturization of electronic products and better transmission signal integrity. Among them, the key process of pattern transfer as a PCB fine circuit manufacturing process includes micro-etching and copper reduction, hot pressing dry film, exposure, development, pattern electroplating and other steps. The verticality of the side wall of the dry film circuit attached to the copper clad board after development will affect the signal integrity and impedance of the subsequent pattern electroplated copper circuit.
[0003] Due to the difference in characteristic wavelengths emitted by different exposure light sources, the dry film undergoes different degrees of light curing during the exposure stage, thus giving the circuit different characteristic cross-sectional shapes. The main peak of the UV parallel exposure machine spectrum is located at 365nm, resulting in an approximately inverted trapezoidal circuit cross-sectional shape. The spectrum of the domestic supplier's LDI equipment is concentrated at a single wavelength of 405nm, resulting in an approximately trapezoidal circuit cross-sectional shape. In either case, the cross-sectional shape of the specific dry film circuit causes the top line width and the bottom line width to be inconsistent, affecting the circuit quality and signal integrity of the subsequent graphic electroplating copper, and even causing impedance fluctuations and reducing the signal transmission speed. Through the conventional method of directly observing the dry film through a microscope after exposure and development, it is impossible to accurately obtain the top line width and bottom line width information of the dry film circuit; the method of making a metallographic section of the dry film circuit attached to the copper clad board and then removing the film, and then using SEM to shoot the curing agent frame has the disadvantages of cumbersome process and long test cycle. The above characterization methods have limitations in judging the cross-sectional morphology information and actual line width of the dry film circuit, and thus cannot timely adjust the use parameters related to the dry film exposure process in the production process, reducing the product yield and reliability. Summary of the invention
[0004] The purpose of the present invention is to address the problem of fast and convenient characterization of fine circuit sidewall structures of dry films and propose a method for determining the optimal exposure energy for light source-induced dry film molding.
[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0006] A method for determining the optimal exposure energy for light source-induced dry film forming comprises the following steps:
[0007] (1) Hot pressing dry film on the surface of copper clad laminate after micro-etching;
[0008] (2) The dry film is exposed in a gradient manner and rapidly developed to form a dry film circuit;
[0009] (3) Metallographic sectioning: Metallographic sectioning is used to fix the position and direction of the sample, exposing the cross section of the dry film circuit to the polished surface of the metallographic section, and the dry film circuit is perpendicular to the polished surface of the metallographic section;
[0010] (4) Evaluation of the vertical state of the side wall structure of the dry film circuit: A 3D laser microscope was used to observe the cross-sectional shape of the dry film circuit, and Image J was used to measure the top line width L1 and bottom line width L2 of the dry film circuit at each exposure energy;
[0011] (5) Based on the line width data measured in step (4), the light source induced dry film exposure molding type is determined and the optimal exposure energy required for making dry film fine circuits is screened out, thereby ensuring a good vertical state of the side wall of the patterned electroplated copper circuit and a stable line width / line spacing ratio. The optimal exposure energy is affected by the properties and thickness of the dry film, but regardless of how it is affected, the judgment standard remains unchanged.
[0012] As a preferred embodiment, the light source device of the gradient exposure method in step (2) is selected from a UV parallel exposure machine and a 405nm laser direct imaging, and the exposure energy range is 10 to 100 mJ / cm 2 , the gradient step size increases from 5 to 20 mJ / cm 2 The exposure energy can be selected in a suitable preliminary range, such as 60-80mJ / cm 2 , after gradient exposure (e.g. 3 gradients, each gradient is 10mJ / cm 2 ), and obtain an optimal exposure energy within this range, i.e., setting it to 60, 70, 80 mJ / cm 2 The three exposure energies are processed in steps (3) to (5) to obtain an optimal exposure energy. If 60-80 mJ / cm 2 The best exposure energy for this segment is 70-80mJ / cm 2 If you want to get a more accurate value, you can continue to use 70-80mJ / cm2 Set gradient exposure (e.g. 11 gradients, each gradient is 1 mJ / cm 2 ), and obtain an optimal exposure energy within this range, that is, setting it to 70, 71, 72, 73...80mJ / cm 2 There are 11 exposure energies in total. After processing in steps (3)-(5), the optimal exposure energy is obtained based on the results.
[0013] As a preferred embodiment, the circuit formed by the dry film in step (2) consists of M groups of line arrays with a line width of A and a spacing of B, and one group of arrays consists of a line and a spacing between two lines, the line width A ranges from 20 to 100 μm, the spacing B ranges from 100 to 400 μm, M is a positive integer greater than or equal to 2, and the line thickness ranges from 20 to 120 μm.
[0014] As a preferred embodiment, the development conditions in step (2) are as follows: Na2CO3 mass concentration 0.7-1.0%, development temperature 28-32°C, spray pressure 1.0-2.0 kg / cm 2 , development time is 30 to 90 seconds, and the time interval between exposure and development is within 5 seconds.
[0015] As a preferred embodiment, the specific process of metallographic sectioning in step (3) is as follows: first, the dry film circuit is cut on the XOY plane, and then the cut dry film circuit is placed in a mold, and then a low-temperature epoxy resin curing agent is poured into the mold and then ground and polished, and the ground and polished surface is the XOZ plane; X is defined as the extension direction of the dry film circuit width, Y is defined as the extension direction of the dry film circuit length, and Z is defined as the extension direction of the dry film circuit thickness.
[0016] As a preferred method, in step (4), the vertical state of the dry film circuit side wall structure is evaluated by measuring the top line width L1 and the bottom line width L2 of the dry film circuit by using Image J software to determine the exposure molding effect and circuit structural integrity of the dry film circuit.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] The present invention provides a method for determining the optimal exposure energy for light source-induced dry film forming. In the pattern transfer process of a printed circuit board, the method of the present invention is adopted. After the copper clad board is subjected to micro-etching, hot pressing, dry film, exposure and development to form a pattern circuit, the cross-sectional shape information, top line width and bottom line width of the circuit under a specific exposure light source can be accurately obtained, providing a guiding direction for setting appropriate exposure parameters for the dry film in the pattern transfer, thereby ensuring a good vertical state of the side wall of the pattern electroplated copper circuit and a stable line width / line spacing ratio, and improving the fine circuit production yield and process capability index Cpk. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is a schematic diagram of the process of the present invention;
[0020] Figure 2 The three-dimensional direction marking diagram of the dry film circuit of the present invention; wherein X is the extension direction of the width of the dry film circuit, Y is the extension direction of the length of the dry film circuit, and Z is the extension direction of the thickness of the dry film circuit;
[0021] Figure 3 This is a metallographic slice diagram of a dry film circuit formed by using a 405nm laser direct imaging exposure method in Example 1 of the present invention; wherein 301 indicates that the exposure energy is 10mJ / cm 2 Metallographic section of dry film circuit cross section; 302 indicates exposure energy of 20mJ / cm 2 Metallographic section of dry film circuit cross section; 303 indicates exposure energy of 30mJ / cm 2 Metallographic section of dry film circuit cross section; 304 indicates exposure energy of 40mJ / cm 2 Metallographic section of dry film circuit cross section; 305 means the exposure energy is 50mJ / cm 2 Metallographic section of dry film circuit cross section;
[0022] Figure 4 This is a metallographic slice diagram of a dry film circuit formed by using a UV parallel exposure machine in Example 2 of the present invention; wherein 401 indicates that the exposure energy is 40 mJ / cm 2 Metallographic section of dry film circuit cross section; 402 indicates exposure energy of 50mJ / cm 2 Metallographic section of dry film circuit cross section; 403 indicates exposure energy of 60mJ / cm 2 Metallographic section of dry film circuit cross section; 404 indicates exposure energy of 70mJ / cm 2 Metallographic section of dry film circuit cross section; 405 indicates exposure energy of 80mJ / cm 2 Metallographic section of dry film circuit cross section. DETAILED DESCRIPTION
[0023] In order to allow those skilled in the art to understand the present invention more clearly and intuitively, the present invention will be further described below.
[0024] Example 1
[0025] like Figure 1 The embodiment shown provides a method for determining the optimal exposure energy for light source-induced dry film forming, comprising the following steps:
[0026] (1) After micro-etching, the copper clad laminate is hot-pressed to dry film; the hot-pressing temperature is 105°C and the hot-pressing pressure is 4.5kg / cm 2, hot pressing speed is 1.4m / min;
[0027] (2) Then, the 405 nm laser direct imaging method was used for exposure. The pattern of the exposure data was 7 dry film lines with the same size, parallel to each other, and line width and line spacing of 40 μm / 400 μm. The thickness of the dry film line was 50 μm. The exposure energy was 10, 20, 30, 40, and 50 mJ / cm 2 ;
[0028] (3) After exposure, the developer was developed quickly. The developer solution Na2CO3 had a mass percentage concentration of 0.9%, the development time was 63 seconds, and the spray pressure of the developer solution was 1.5 kg / cm 2 , developing temperature 29°C;
[0029] (4) After development, the copper clad laminate containing the dry film circuit pattern is cut to produce a metallographic slice; the specific process of metallographic slice preparation is as follows: first, the dry film circuit is cut on the XOY plane, and then the cut dry film circuit is placed in a mold, and then a low-temperature epoxy resin / curing agent set (EpoQuick from QMAXIS, USA) is poured into the mold and then ground and polished, and the ground and polished surface is the XOZ plane; Figure 2 As shown, X is defined as the extension direction of the dry film line width, Y is defined as the extension direction of the dry film line length, and Z is defined as the extension direction of the dry film line thickness. Figure 3 As shown in the figure, 301-305 are exposure energies of 10, 20, 30, 40, and 50 mJ / cm 2 Metallographic section of dry film circuit cross section.
[0030] (5) The top line width L1 and bottom line width L2 of the line at each exposure energy were measured by 3D laser microscope photography and Image J. The results were 33.77μm / 41.31μm; 40.52μm / 43.14μm; 39.02μm / 40.65μm; 38.03μm / 41.31μm; 42.30μm / 47.54μm. Therefore, the dry film obtained a nearly trapezoidal line cross-section shape under exposure with a 405nm laser direct imaging device and the optimal exposure energy range was 30mJ / cm 2 about.
[0031] Example 2
[0032] The difference between this embodiment and embodiment 1 is mainly in the exposure method and exposure energy.
[0033] Specifically, the method for evaluating light source-induced dry film exposure molding of this embodiment includes the following steps:
[0034] (1) Hot press the dry film on the copper clad laminate at a temperature of 110°C and a pressure of 4.0 kg / cm 2 , hot pressing speed is 1.7m / min;
[0035] (2) Then, a UV parallel exposure machine and film negative were used for exposure imaging. The film pattern consisted of 7 dry film lines of identical size, parallel to each other, with a line width and line spacing of 40 μm / 400 μm, and a dry film line thickness of 50 μm. The exposure energies were 40, 50, 60, 70, and 80 mJ / cm 2 ;
[0036] (3) After exposure, the developer was developed quickly. The developer solution Na2CO3 had a mass percentage concentration of 0.9%, the development time was 63 seconds, and the spray pressure of the developer solution was 1.5 kg / cm 2 , developing temperature 29°C;
[0037] (4) After development, the copper-clad laminate containing the dry film circuit pattern is cut to produce metallographic slices; the metallographic slices produced in this embodiment are as follows: Figure 4 As shown in the figure, 401-405 are respectively exposure energies of 40, 50, 60, 70, and 80 mJ / cm 2 Metallographic section of dry film circuit cross section.
[0038] (5) The top line width L1 and bottom line width L2 of the line at each exposure energy were measured by 3D laser microscope photography and Image J. The results were 43.61μm / 25.90μm; 47.21μm / 29.84μm; 53.77μm / 31.48μm; 48.52μm / 36.07μm; 48.52μm / 38.69μm. Therefore, the dry film obtained an approximately inverted trapezoidal line cross-section shape under UV parallel exposure, and the optimal exposure energy range was 70mJ / cm 2 about.
[0039] The above description of the embodiments is to facilitate the understanding and application of the present invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the embodiments herein, and improvements and modifications made to the present invention by those skilled in the art based on the disclosure of the present invention should be within the scope of protection of the present invention.
Claims
1. A method for determining the optimal exposure energy for light source-induced dry film forming, characterized in that: The steps include: S1, hot pressing dry film on the surface of copper clad laminate after micro-etching; S2, the dry film is exposed in a gradient manner and rapidly developed to form a dry film circuit; S3. Metallographic section sample preparation: Metallographic section sample preparation is used to fix the position and direction of the sample, exposing the cross section of the dry film circuit to the grinding and polishing surface of the metallographic section, and the dry film circuit is perpendicular to the grinding and polishing surface of the metallographic section; S4. Evaluation of the vertical state of the side wall structure of the dry film circuit: A 3D laser microscope was used to observe the cross-sectional shape of the dry film circuit, and Image J was used to measure the top line width L1 and the bottom line width L2 of the dry film circuit at each exposure energy; S5. Based on the line width data measured in S4, determine the light source induced dry film exposure molding type and screen out the optimal exposure energy required for making dry film fine circuits.
2. The method according to claim 1, characterized in that The light source device for the gradient exposure method in step S2 is selected from a UV parallel exposure machine and a 405nm laser direct imaging device.
3. The method according to claim 2, characterized in that The exposure energy range of the gradient exposure in step S2 is 10-100 mJ / cm 2 , the gradient step size increases from 5 to 20 mJ / cm 2 .
4. The method according to claim 1, characterized in that: The dry film circuit is composed of M groups of line arrays with line width A and spacing B, A ranges from 20 to 100 μm, B ranges from 100 to 400 μm, M is a positive integer greater than or equal to 2, and the circuit thickness ranges from 20 to 120 μm.
5. The method according to claim 1, characterized in that The developing conditions in step S2 are: Na2CO3 mass concentration 0.7-1.0%, developing temperature 28-32°C, spray pressure 1.0-2.0 kg / cm 2 , development time is 30 to 90 seconds, and the time interval between exposure and development is within 5 seconds.
6. The method according to claim 1, characterized in that The specific process of metallographic sectioning and sample preparation in step S3 is as follows: first, the dry film circuit is cut on the XOY plane, and then the cut dry film circuit is placed in a mold, and then a low-temperature epoxy resin curing agent is poured into the mold and then ground and polished, and the ground and polished surface is the XOZ plane; X is defined as the extension direction of the dry film circuit width, Y is the extension direction of the dry film circuit length, and Z is the extension direction of the dry film circuit thickness.
7. The method according to claim 1, characterized in that In step S4, the top line width L1 and the bottom line width L2 of the dry film circuit measured by the Image J software are used to determine the exposure forming effect and circuit structural integrity of the dry film circuit.
8. The method according to claim 1, characterized in that The top line width refers to the width of the dry film circuit away from the copper surface and parallel to the X direction, and the bottom line width refers to the width of the dry film circuit close to the copper surface and parallel to the X direction.