A converter smelting method based on electrode heating of scrap steel
The three-stage smelting method using electrode heating of scrap steel solved the problem of low scrap ratio in converter smelting, achieving an increase in scrap ratio and energy utilization, and ensuring smooth smelting process and molten steel quality.
Patent Information
- Application Number
- CN202311859513.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-30
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-12-30
AI Technical Summary
The current low scrap ratio in converter smelting results in high heat consumption and unfavorable smelting conditions for smooth production, making it difficult to increase the scrap ratio.
A three-stage smelting method using electrode heating of scrap steel is adopted. By controlling the amount of scrap steel added and the electrode heating time at different stages, combined with oxygen blowing reaction, the scrap steel temperature and melting efficiency are improved.
The increased scrap ratio in the converter reduced energy consumption, decreased dioxin production, and ensured the final smelting temperature and steel quality.
Smart Images

Figure CN117821689B_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of converter smelting technology, specifically relating to a converter smelting method based on electrode heating of scrap steel. Background Technology
[0002] The blast furnace-converter process is the dominant smelting method in my country's steel production. For the converter steelmaking process, increasing the scrap ratio is an effective way to reduce carbon emissions and is a future development trend.
[0003] Compared to molten iron, scrap steel has a lower temperature, requiring additional heat to melt, which consumes a large amount of heat. Furthermore, the addition of scrap steel alters the converter smelting conditions, and an excessively high scrap steel ratio is detrimental to smooth production. In related technologies, the scrap steel ratio in converters is typically below 20%, and further increasing it is quite difficult. Summary of the Invention
[0004] To address the current technical problem of low scrap ratio in converter smelting, this application provides a converter smelting method based on electrode heating of scrap steel.
[0005] This application provides a converter smelting method for scrap steel based on electrode heating. The converter includes a furnace body and electrodes for heating that extend into the furnace body. The converter smelting method includes the following steps:
[0006] Step 1: Add molten iron into the furnace;
[0007] Step 2: Add scrap steel and carbon material into the furnace, then heat the lower electrode inside the furnace for a period of time until the electrode rises to the outside of the furnace.
[0008] Step 3: Blow oxygen into the material inside the furnace from Step 2 for a period of time, then stop blowing oxygen to complete the first stage of smelting.
[0009] Step 4: Repeat steps 2 and 3 to complete the second stage of smelting;
[0010] Step 5: Continue repeating steps 2 and 3 to complete the third stage of smelting;
[0011] The amount of scrap steel added in the second stage of smelting is no less than that in the first stage, and the amount of scrap steel added in the third stage of smelting is no less than that in the first stage. The electrode heating time in the first, second and third stages of smelting decreases sequentially.
[0012] In some embodiments, in the first stage smelting, the second stage smelting, and the third stage smelting, the amount of scrap steel added is 20%-25%, 25%-30%, and 30%-35% of the nominal capacity of the furnace body, respectively; the longest side dimension of the scrap steel does not exceed 1000mm, and the weight of each piece of scrap steel does not exceed 300kg.
[0013] In some embodiments, the electrode heating times in the first stage smelting, the second stage smelting, and the third stage smelting are 10-15 min, 8-12 min, and 6-10 min, respectively.
[0014] In some embodiments, in step 1, the amount of molten iron added is 10%-20% of the nominal capacity of the furnace body.
[0015] In some embodiments, in step 2, adding scrap steel and carbon materials into the furnace body specifically means: first adding carbon materials into the furnace body and then adding scrap steel.
[0016] In some embodiments, the amount of carbon material added in the first stage smelting, the second stage smelting, and the third stage smelting is 1.5%-2.5%, 2.6%-3.5%, and 2.6%-3.5% of the nominal capacity of the furnace body, respectively.
[0017] In some embodiments, when the nominal capacity of the furnace body is 200-300t, the amount of carbon material added in the first stage smelting, the second stage smelting, and the third stage smelting is 2-4t, 4-6t, and 4-6t, respectively.
[0018] In some embodiments, the oxygen blowing intensity in the first stage smelting, the second stage smelting, and the third stage smelting is 2.0-3.0 Nm, respectively. 3 / min / t, 2.5-3.5Nm 3 / min / t and 3.0-4.0Nm 3 / min / t.
[0019] In some embodiments, the oxygen blowing times in the first stage smelting, the second stage smelting, and the third stage smelting are 3-5 min, 5-8 min, and 6-10 min, respectively.
[0020] In some embodiments, in step 2, after the electrode rises to the outside of the furnace, a slagging agent is added into the furnace body. The slagging agent comprises the following components by mass fraction: CaO: 40-50%, SiO2: 15-20%, MgO: 8-15%.
[0021] In the first stage of smelting, the second stage of smelting, and the third stage of smelting, the amount of slag-forming agent added is 2.5%-3%, 3%-5%, and 3%-5% of the nominal capacity of the furnace body, respectively.
[0022] This application provides a converter smelting method based on electrode heating of scrap steel. The converter includes a furnace body and electrodes for heating that extend into the furnace body. The converter smelting method includes the following steps: Step 1, adding molten iron into the furnace body; Step 2, adding scrap steel and carbon materials into the furnace body, then heating the lower electrodes inside the furnace body for a period of time until the electrodes rise to the outside of the furnace body; Step 3, blowing oxygen into the material inside the furnace body from Step 2 for a period of time, then stopping the oxygen blowing to complete the first stage of smelting; Step 4, repeating Steps 2 and 3 to complete the second stage of smelting; Step 5, continuing to repeat Steps 2 and 3 to complete the third stage of smelting. This application divides the converter smelting into three stages. Before the three stages of smelting, molten iron is added into the converter. In the first stage of smelting, the molten iron reacts with the blown oxygen to produce an exothermic oxidation reaction. In all three stages of smelting, the material inside the furnace body is first heated through electrodes, which can increase the temperature of the scrap steel and facilitate its melting. In the first stage of smelting, the oxygen blown in can react with the molten iron and carbon materials in an exothermic oxidation reaction. In the second and third stages of smelting, the carbon in the molten iron has been basically oxidized. At this time, the oxygen blown in mainly reacts with the added carbon materials in an exothermic oxidation reaction, which helps to melt the scrap steel and also increases the temperature inside the furnace.
[0023] In the initial stage of the reaction, which is the first stage of smelting, the furnace heat is low and the scrap steel is difficult to melt. Therefore, the amount of scrap steel added in the first stage of smelting is relatively low. In the second and third stages of smelting, the furnace has a certain amount of heat, so more scrap steel can be added in these two stages to increase the scrap steel ratio.
[0024] In the first stage of smelting, only molten iron introduces heat, resulting in relatively little heat inside the converter. Therefore, the electrode heating time is longer to increase the heating rate, facilitating the melting of scrap steel and reducing the risk of dioxin formation in the low-temperature zone during scrap heating. In the second and third stages of smelting, the furnace contains more heat, providing better conditions for scrap steel melting. Therefore, the electrode heating time in these two stages decreases sequentially, saving energy, ensuring the converter reaches its final temperature, and increasing the scrap steel ratio in the converter.
[0025] Therefore, this application adopts electrode heating combined with three-stage smelting, and controls the amount of scrap steel added in each stage and the electrode heating time, thereby increasing the scrap steel ratio in the converter and improving energy utilization. Attached Figure Description
[0026] Figure 1 A top view of a converter in one or more embodiments of this application is shown.
[0027] Explanation of reference numerals in the attached figures:
[0028] 10 - Furnace body, 20 - Electrode. Detailed Implementation
[0029] To enable those skilled in the art to more clearly understand this application, the technical solutions in the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of this application, and not all of the embodiments. Based on the embodiments of this application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of this application.
[0030] This application provides a converter smelting method based on electrode heating of scrap steel, which can significantly increase the scrap steel ratio in the converter process and achieve ultra-low carbon emissions in the converter smelting process.
[0031] The converter used in this application is a traditional converter with added heating electrodes. Figure 1 A top view of the converter is shown, combined with Figure 1 The converter includes a furnace body 10 and electrodes 20 for heating that extend into the furnace body.
[0032] The electrodes 20 can be heated by AC power. In some embodiments, multiple electrodes 20 can be provided, spaced apart, with the lower end of each electrode 20 extending into or out of the furnace body 10. In some embodiments, three electrodes 20 are provided, arranged in a triangular formation, which is an equilateral triangle with the center of the equilateral triangle being the central axis of the converter. The length of the electrodes 20 can be determined according to the dimensions of the converter body 10. For example, the length of the electrode 20 is 8-10m, the diameter D of the electrode 20 is 400-600mm, the distance D1 between the outer edge of the electrode 20 and the inner wall of the furnace opening of the furnace body 10 is not less than 700mm, and the distance D2 between the outer edges of adjacent electrodes 20 is not less than 600mm.
[0033] Please see Figure 1 The converter smelting method based on electrode 20 heating scrap steel provided in this application includes the following steps:
[0034] Step 1: Add molten iron into the furnace body 10;
[0035] Step 2: Add scrap steel and carbon materials into the furnace body 10, and then heat the lower electrode 20 into the furnace body 10 for a period of time until the electrode 20 rises outside the furnace body 10.
[0036] Step 3: Blow oxygen into the material inside the furnace body 10 from Step 2 for a period of time, then stop blowing oxygen to complete the first stage of smelting;
[0037] Step 4: Repeat steps 2 and 3 to complete the second stage of smelting;
[0038] Step 5: Continue repeating steps 2 and 3 to complete the third stage of smelting;
[0039] In the second stage of smelting, the amount of scrap steel added is not less than that in the first stage, and in the third stage of smelting, the amount of scrap steel added is not less than that in the first stage. The heating time of electrode 20 in the first stage of smelting, the second stage of smelting, and the third stage of smelting decreases sequentially.
[0040] Electrode 20 can extend vertically, with its upper end located outside the furnace body 10. Electrode 20 can reciprocate vertically so that its lower end can extend from outside the furnace body 10 into the furnace body 10. Electrode 20 can quickly preheat the scrap steel inside the furnace body 10. Using electrode 20 to preheat the scrap steel can reduce the residence time of the scrap steel in the low-temperature zone and reduce the amount of dioxins generated.
[0041] The converter smelting process is divided into three stages: the first stage smelting, the second stage smelting, and the third stage smelting, as described above. Before the third stage smelting, molten iron is added to the converter. In the first stage smelting, the molten iron reacts with the blown-in oxygen in an exothermic oxidation reaction. In all three stages, the material inside the furnace body 10 is first heated through electrodes 20, which increases the temperature of the scrap steel and facilitates its melting. In the first stage smelting, the blown-in oxygen reacts with both the molten iron and the carbon materials in an exothermic oxidation reaction. In the second and third stages, the carbon in the molten iron has been largely oxidized. At this point, the blown-in oxygen mainly reacts with the added carbon materials in an exothermic oxidation reaction, which helps to melt the scrap steel and also increases the furnace temperature.
[0042] In the initial stage of the reaction, which is the first stage of smelting, the furnace temperature is low, making it difficult for the scrap steel to melt. Therefore, the amount of scrap steel added in the first stage is relatively low. In the second and third stages of smelting, the furnace has reached a certain level of heat, so more scrap steel can be added in these two stages to increase the scrap steel ratio.
[0043] During the first stage of smelting, only molten iron introduces heat, resulting in relatively little heat within the converter body 10. Therefore, the electrode 20 heating time is longer to increase the heating rate, facilitating scrap melting and reducing the risk of dioxin formation in the low-temperature zone during scrap heating. In the second and third stages of smelting, the furnace contains more heat, providing better conditions for scrap melting. Therefore, the electrode 20 heating time decreases sequentially in these two stages, saving energy, ensuring the converter reaches its final temperature, and increasing the scrap ratio in the converter.
[0044] This application uses a three-stage smelting process to control the amount of scrap steel added and the heating time of electrode 20 at each stage. The heating of electrode 20 is combined with oxygen blowing for heat release, which not only ensures the final temperature of the converter but also increases the scrap steel ratio of the converter.
[0045] In some embodiments, in the first stage smelting, the second stage smelting, and the third stage smelting, the amount of scrap steel added is 20%-25%, 25%-30%, and 30%-35% of the nominal capacity of the furnace body, respectively. That is, in the first stage smelting, the amount of scrap steel added accounts for 20%-25% of the nominal capacity of the converter; in the second stage smelting, the amount of scrap steel added accounts for 25%-30% of the nominal capacity of the converter; and in the third stage smelting, the amount of scrap steel added accounts for 30%-35% of the nominal capacity of the converter.
[0046] In some embodiments, the longest side of the scrap steel does not exceed 1000 mm, and the weight of each piece of scrap steel does not exceed 300 kg. The size of the scrap steel affects the melting time. If the longest side of the scrap steel is too large, it will increase the difficulty of adding the scrap steel into the furnace through the converter opening to some extent, and will also prolong the melting time. Excessive weight of the scrap steel will also prolong the melting time to some extent.
[0047] In some embodiments, the heating times of electrode 20 in the first stage smelting, the second stage smelting, and the third stage smelting are 10-15 min, 8-12 min, and 6-10 min, respectively. The heating time of electrode 20 affects the heat of the material in the furnace. Before the first stage smelting, only the molten iron carries heat, while the scrap steel is at room temperature. Therefore, the heating time of electrode 20 in the first stage smelting is relatively long to increase the heat in the furnace and facilitate the melting of the scrap steel. In the second stage smelting, the material in the furnace already has considerable heat from the first stage smelting. Therefore, even if the amount of scrap steel added in this stage exceeds that in the first stage smelting, the scrap steel can still be melted in a shorter heating time than in the first stage smelting. In the third stage smelting, the material in the furnace has even more heat, and the quantity of material is also very large. Therefore, the added scrap steel can be melted quickly, so the heating time of electrode 20 in the third stage smelting is shorter than that in the second stage smelting.
[0048] In some embodiments, in step 1, the amount of molten iron added is 10%-20% of the nominal capacity of the furnace body 10, that is, the amount of molten iron added is 10%-20% of the nominal capacity of the converter. If too much molten iron is added, the scrap ratio will be reduced to a certain extent. If too little molten iron is added, the heat generated in the first stage of smelting will be reduced, the heating time of the electrode 20 will be extended, and the smelting efficiency of the converter will be reduced.
[0049] In some embodiments, in step 2, adding scrap steel and carbon materials into the furnace body 10 specifically means: first adding carbon materials into the furnace body 10 and then adding scrap steel.
[0050] The carbon feedstock can be graphite, coke, or carbon powder, etc. The added carbon feedstock reacts with oxygen in an exothermic oxidation reaction to form carbon monoxide and carbon dioxide bubbles. As these bubbles escape from the molten steel, they remove nitrogen introduced by scrap steel and air, effectively controlling the nitrogen content at the end of the converter smelting process. Adding the carbon feedstock before the scrap steel utilizes the high density of the scrap steel, which helps to hold the carbon feedstock in place and prevents the less dense carbon feedstock from scattering and being wasted.
[0051] In some embodiments, the amount of carbon added in the first stage of smelting is less than that in the second stage of smelting, and also less than that in the third stage of smelting; that is, the amount of carbon added in the first stage of smelting is the smallest. During the first stage of smelting, oxygen reacts exothermically with carbon in the molten iron, and the amount of scrap steel added is relatively small, resulting in less nitrogen introduced by the scrap steel. Therefore, less carbon can be added to participate in the exothermic carbon-oxygen reaction. The molten iron has essentially reacted completely in the first stage of smelting. In the second and third stages of smelting, the reaction is mainly exothermic with oxygen; therefore, the amount of carbon added in these two stages is larger.
[0052] Specifically, in the first stage of smelting, the second stage of smelting, and the third stage of smelting, the amount of carbon material added is 1.5%-2.5%, 2.6%-3.5%, and 2.6%-3.5% of 10 nominal furnace capacity, respectively.
[0053] In some embodiments, when the nominal capacity of the furnace body 10 is 200-300t, the amount of carbon material added in the first stage smelting, the second stage smelting, and the third stage smelting is 2-4t, 4-6t, and 4-6t, respectively.
[0054] In some embodiments, in the first stage of smelting, carbon materials account for 8%-10% of the total carbon materials and scrap steel; in the second stage of smelting, carbon materials account for 5%-8% of the total carbon materials and scrap steel; and in the third stage of smelting, carbon materials account for 5%-8% of the total carbon materials and scrap steel.
[0055] In some embodiments, the oxygen blowing intensity increases sequentially in the first, second, and third stages of smelting. This is because as smelting progresses, the amount of molten steel in the converter 10 increases, and the liquid level rises. At low liquid levels, a low oxygen blowing intensity prevents the liquid from churning, while at high liquid levels, a high oxygen blowing intensity allows for an exothermic carbon-oxygen reaction, simultaneously achieving uniformity in the temperature and composition of the molten steel. Specifically, the oxygen blowing intensity in the first, second, and third stages of smelting is 2.0-3.0 Nm³, respectively. 3 / min / t, 2.5-3.5Nm 3 / min / t and 3.0-4.0Nm 3 / min / t.
[0056] In some embodiments, the oxygen blowing time for the first stage smelting, the second stage smelting, and the third stage smelting increases sequentially because: the amount of molten iron added is limited, and the reaction is completed within a short blowing time, thus the oxygen blowing time for the first stage smelting is the shortest; the scrap steel added in the first stage smelting does not completely melt during the first stage smelting process, and may need to continue into the second or third stage smelting process; moreover, new scrap steel and the amount of carbon agent added are added in the second and third stages smelting, thus requiring more oxygen blowing time for the carbon agent to undergo an exothermic reaction and heat up, and the scrap steel also needs time to gradually melt, therefore, the oxygen blowing time is the longest in the third stage smelting process. Specifically, the oxygen blowing times for the first stage smelting, the second stage smelting, and the third stage smelting are 3-5 min, 5-8 min, and 6-10 min, respectively.
[0057] In some embodiments, in step 2, after the electrode 20 rises to the outside of the furnace body 10, a slagging agent is added into the furnace body 10. The slagging agent includes the following components by mass fraction: CaO: 40-50%, SiO2: 15-20%, MgO: 8-15%.
[0058] In the first stage of smelting, the second stage of smelting, and the third stage of smelting, the amount of slag-forming agent added is 2.5%-3%, 3%-5%, and 3%-5% of 10 nominal furnace capacity, respectively.
[0059] In some embodiments, in step 1, the furnace body 10 adopts a slag retention operation before adding molten iron, and the amount of slag retained is 1%-3% of the nominal capacity of the furnace body 10.
[0060] The converter smelting method based on electrode 20 heating scrap steel provided by the present invention will be further described in detail below with reference to specific embodiments.
[0061] Example 1
[0062] The converter body has a nominal capacity of 200t, the electrode 20 has a diameter of 450mm, there are three electrodes 20, and the length of the electrodes 20 is 8m. The slag retention rate after tapping is 20kg / t, and the amount of molten iron added is 20t. Scrap steel and graphite are added to the converter in three stages, and the scrap steel is melted by heating with electrodes 20.
[0063] First stage of smelting: Graphite (3 tons) is added to the converter, followed by 40 tons of scrap steel, totaling 43 tons; AC electrode 20 is inserted into the converter and energized for 13 minutes; electrode 20 is removed, and slag-forming material (5 tons) is added to the converter; an oxygen lance is inserted, with an oxygen supply intensity of 2.5 Nm. 3 / min / t, while bottom blowing oxygen at an intensity of 0.1Nm. 3 / min / t; blowing time is 3min; lift the oxygen lance. See Table 1 for details.
[0064] Second stage smelting: First, add graphite (5.5g) to the converter, then add 60 steel, totaling 65.5g. Insert AC electrodes 20 into the converter and energize for 10 minutes; remove electrodes 20; add 8 tons of slag-forming material to the converter; insert an oxygen lance with an oxygen supply intensity of 2.7m. 3 / min / t, while bottom blowing oxygen at an intensity of 0.1Nm. 3 / min / t; blowing time is 6min; lift the oxygen lance. See Table 2 for details.
[0065] The third stage of smelting: First, graphite is added to the converter, with a weight of 5.5t to 70t, totaling 75.5t. An AC electrode 20 is inserted into the furnace and energized for 9 minutes. The electrode 20 is then removed. Next, 8 tons of slag-forming material is added to the converter. An oxygen lance is then inserted, with an oxygen supply intensity of 3.2 Nm. 3 / min / t, while bottom blowing oxygen at an intensity of 0.1Nm. 3 / min / t; blowing time is 8min; lift the oxygen lance, smelting ends, and steel is tapped. See Table 3 for details.
[0066] The main components of the slag-forming material are CaO: 45%, SiO2: 16%, and MgO: 9%.
[0067] Example 2
[0068] The converter body has a nominal capacity of 300t, the electrode 20 has a diameter of 500mm, there are three electrodes 20, and the length of the electrodes 20 is 10m. The slag retention rate after tapping is 30kg / t, and the amount of molten iron added is 60t. Scrap steel and graphite are added to the converter in three stages, and the scrap steel is melted by heating with electrodes 20.
[0069] First stage of smelting: Graphite (6 tons) is added to the converter, followed by 60 tons of scrap steel, totaling 66 tons; AC electrodes 20 are inserted into the converter and energized for 13 minutes; electrodes 20 are then removed; slag-forming material (8 tons) is added to the converter; an oxygen lance is inserted, with an oxygen supply intensity of 2.3 Nm. 3 / min / t, while bottom blowing oxygen at an intensity of 0.12 Nm. 3 / min / t; blowing time is 5min; lift the oxygen lance.
[0070] Second stage smelting: First, add 8 tons of graphite to the converter, then add 90 tons of scrap steel, totaling 98 tons; insert AC electrodes 20 into the converter and energize for 10 minutes; remove electrodes 20; add 10 tons of slag-forming material to the converter; insert an oxygen lance with an oxygen supply intensity of 3.5 Nm. 3 / min / t, while bottom blowing oxygen at an intensity of 0.1Nm. 3 / min / t; blowing time is 8min; lift the oxygen lance.
[0071] The third stage of smelting: First, 9 tons of graphite are added to the converter, followed by 90 tons of scrap steel, for a total of 99 tons; 20 AC electrodes are inserted into the converter and energized for 8 minutes; the electrodes are then removed; 10 tons of slag-forming material are added to the converter; and an oxygen lance is inserted with an oxygen supply intensity of 3.8 Nm. 3 / min / t, while bottom blowing oxygen at an intensity of 0.12 Nm. 3 / min / t; the blowing time is 9min; lift the oxygen lance, the smelting is finished, and the steel is tapped.
[0072] The main components of the slag-forming material are CaO: 50%, SiO2: 18%, and MgO: 10%.
[0073] Examples 3 to 5
[0074] The converter smelting methods based on electrode 20 heating scrap steel provided in Examples 3 to 5 are based on Example 1. The nominal capacity of furnace body 10 in Examples 3 and 4 is the same as that in Example 1, which is 200t. The nominal capacity of Example 5 is 300t. Other differences between Examples 3 to 5 and Example 1 are the parameters in Tables 1 to 3.
[0075] Comparative Example 1
[0076] Conventional converter smelting: The converter has a nominal capacity of 300 tons. At the start of each heat, slag splashing is performed for furnace protection, followed by the addition of 35 tons of scrap steel, then 270 tons of molten iron, with a charging time of 3 minutes. After the iron charging is complete, the first batch of slag-forming material is added, and oxygen blowing begins at an oxygen flow rate of 3.5 Nm³. 3 The blowing time was 6 minutes, followed by the addition of the second batch of slag-forming material. Blowing continued for another 10 minutes. After blowing, the temperature and composition were measured, and the steel was tapped. The steel composition and temperature met the requirements, with a nitrogen content of 20 ppm.
[0077] Comparative Example 2
[0078] Electric furnace smelting: The nominal capacity of the electric furnace is 60t. First, scrap steel is added to the furnace, and the lower electrode (20mm) is energized for heating. After 3-5 minutes, carbon powder is injected to supply oxygen and create foamy slag. During foamy slag formation, the carbon powder flow rate is 20-60 kg / min, and the oxygen flow rate is 1500-2000 m³ / min. 3 / h; Oxygen flow rate during decarbonization: 2500-3000 m³ / h 3 / h. No slag-forming material is added during the first and last 5 minutes of the electric furnace smelting cycle. During the middle stage, slag-forming material is added in 4-5 batches continuously. During the smelting process, multiple samples are taken to measure the composition and monitor the temperature. Steel is tapped after reaching the target value. The entire smelting cycle is 60-70 minutes. The composition and temperature of the molten steel meet the requirements, with a nitrogen content of 80 ppm.
[0079] Table 1
[0080] Table 2
[0081] Table 3
[0082] Table 4 serial number molten iron / t scrap steel / t scrap steel ratio Nitrogen content / ppm Total smelting time / min Example 1 30 170 85% 20 65 Example 2 60 240 80% 19 70 Example 3 40 160 80% 21 64 Example 4 50 150 75% 22 60 Example 5 45 255 85% 18 72 Comparative Example 1 270 35 11.7% 20 45 Comparative Example 2 / 60 100% 80 70
[0083] As can be seen from the data in Table 4, the converter smelting method based on electrode 20 heating scrap steel provided in Examples 1 to 5 of this application can achieve a scrap steel ratio of 75%-85%, which is high. The nitrogen content of the molten steel at the smelting endpoint is 18-21 ppm, which is low.
[0084] The converter smelting method based on electrode 20 heating of scrap steel provided in this application adopts a staged smelting approach. Scrap steel is added in each stage and heated and melted using electrode 20. At the same time, the amount of scrap steel added, the amount of carbon material added, the heating time of electrode 20, and the oxygen blowing time are controlled in each stage. This not only increases the scrap steel ratio in the converter and greatly reduces carbon emissions, but also ensures a low final nitrogen content in the converter and improves energy utilization. At the same time, the advantages of converter blowing are utilized to ensure good quality of molten steel.
[0085] In this application, unless otherwise expressly specified and limited, "above" or "below" the second feature can include direct contact between the first and second features, or contact between the first and second features through another feature between them. Furthermore, "above," "over," and "on top" of the second feature includes the first feature being directly above or diagonally above the second feature, or simply indicates that the first feature is at a higher horizontal level than the second feature. "Below," "below," and "under" the second feature includes the first feature being directly below or diagonally below the second feature, or simply indicates that the first feature is at a lower horizontal level than the second feature.
[0086] In the description of this application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "upper", "lower", "front", "rear", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", "outer", "clockwise", and "counterclockwise" indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this application.
[0087] In this application, unless otherwise expressly specified and limited, the terms "connection," "fixed," etc., should be interpreted broadly. For example, "fixed" can mean a fixed connection, a detachable connection, or an integral part; it can mean a mechanical connection or an electrical connection; it can mean a direct connection or an indirect connection through an intermediate medium; it can mean the internal communication of two components or the interaction between two components. Those skilled in the art can understand the specific meaning of the above terms in this application according to the specific circumstances.
[0088] Furthermore, the use of terms such as "first" and "second" in this application is for descriptive purposes only and should not be construed as indicating or implying their relative importance or implicitly specifying the number of technical features indicated. Therefore, features defined with "first" or "second" may explicitly or implicitly include one or more features. In the description of this application, "multiple" means two or more, unless otherwise explicitly specified.
[0089] Although embodiments of this application have been shown and described, those skilled in the art will understand that various changes, modifications, substitutions and variations can be made to these embodiments without departing from the principles and spirit of this application, the scope of which is defined by the claims and their equivalents.
Claims
1. A converter smelting method based on electrode heating of scrap steel, the converter comprising a furnace body and electrodes for heating extending into the furnace body, characterized in that, The converter smelting method includes the following steps: Step 1: Add molten iron into the furnace; Step 2: Add scrap steel and carbon material into the furnace body, then heat the lower electrode inside the furnace body for a period of time until the electrode rises outside the furnace body; the longest side dimension of the scrap steel does not exceed 1000mm, and the weight of each piece of scrap steel does not exceed 300kg; in Step 2, after the electrode rises outside the furnace body, add a slagging agent into the furnace body. The slagging agent includes the following components by mass fraction: CaO: 40-50%, SiO2: 15-20%, MgO: 8-15%; Step 3: Blow oxygen into the material inside the furnace from Step 2 for a period of time, then stop blowing oxygen to complete the first stage of smelting. Step 4: Repeat steps 2 and 3 to complete the second stage of smelting; Step 5: Continue repeating steps 2 and 3 to complete the third stage of smelting; Among them, the amount of scrap steel added in the second stage of smelting is not less than the amount of scrap steel added in the first stage, the amount of scrap steel added in the third stage of smelting is not less than the amount of scrap steel added in the first stage, and the electrode heating time in the first stage of smelting, the second stage of smelting and the third stage of smelting decreases in sequence. In the first stage of smelting, the second stage of smelting, and the third stage of smelting, the amount of scrap steel added is 20%-25%, 25%-30%, and 30%-35% of the nominal furnace capacity, respectively, and the oxygen blowing intensity is 2.0-3.0 Nm. 3 / min / t, 2.5-3.5Nm 3 / min / t and 3.0-4.0Nm 3 / min / t, the oxygen blowing time is 3-5min, 5-8min and 6-10min respectively, and the amount of slagging agent added is 2.5%-3%, 3%-5% and 3%-5% of the nominal capacity of the furnace body respectively.
2. The converter smelting method based on electrode-heated scrap steel according to claim 1, characterized in that, In the first stage of smelting, the second stage of smelting, and the third stage of smelting, the electrode heating time is 10-15 min, 8-12 min, and 6-10 min, respectively.
3. The converter smelting method based on electrode-heated scrap steel according to claim 1, characterized in that, In step 1, the amount of molten iron added is 10%-20% of the nominal capacity of the furnace.
4. The converter smelting method based on electrode-heated scrap steel according to any one of claims 1-3, characterized in that, In step 2, the addition of scrap steel and carbon material into the furnace body specifically involves adding carbon material into the furnace body first, followed by adding scrap steel.
5. The converter smelting method based on electrode-heated scrap steel according to any one of claims 1-3, characterized in that, In the first stage of smelting, the second stage of smelting, and the third stage of smelting, the amount of carbon material added is 1.5%-2.5%, 2.6%-3.5%, and 2.6%-3.5% of the nominal capacity of the furnace body, respectively.
6. The converter smelting method based on electrode-heated scrap steel according to claim 5, characterized in that, When the nominal capacity of the furnace body is 200-300t, the amount of carbon material added in the first stage smelting, the second stage smelting, and the third stage smelting is 2-4t, 4-6t, and 4-6t, respectively.
Citation Information
Patent Citations
Smelting method of low phosphate steel
CN108950127A
Method for smelting low nitrogen steel using electric furnace
WO2020063671A1