Graphene copper wire and preparation method thereof

By using a positive pressure tube furnace and aromatic ring structural compounds on copper wires, the problems of complex and high-cost graphene copper wire preparation processes in the existing technology are solved, and the continuous production of high-quality graphene copper wires is achieved. and low-cost processes to improve production efficiency.

CN117821929BActive Publication Date: 2024-10-08SUZHOU SHENGGUANG MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311873143.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-29
Publication Date
2024-10-08
Estimated Expiration
2043-12-29

AI Technical Summary

Technical Problem

The existing technology for preparing graphene on copper wires has a complicated process and high cost, making it difficult to achieve continuous production, especially under high vacuum conditions. This results in difficulty in industrialization, high energy consumption and cost, and cannot be successfully applied in downstream fields.

Method used

By controlling the tubular furnace reaction chamber to be in a positive pressure state, with the oxygen content below 1ppm, using compounds with aromatic ring structures as carbon sources, combined with a liquid seal structure and a reducing atmosphere, to reduce the oxygen content in the reaction chamber, using Low-temperature growth graphene is produced directly from copper wires.

Benefits of technology

The production process is simplified, the quality and production efficiency of the graphene copper wire are improved, the process complexity and cost are reduced, and the continuous production of high-quality graphene copper wire is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117821929B_ABST
    Figure CN117821929B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing graphene, comprising the following steps: controlling a tubular furnace reaction chamber to be in a positive pressure state, with an oxygen content of less than 1ppm; using a compound with an aromatic ring structure as a carbon source for generating graphene to generate graphene copper wire. The present invention adopts two means, namely, a liquid seal structural design and a reducing gas, to reduce the oxygen content in the reaction chamber, and makes the reaction chamber in a slightly positive pressure state, thereby improving production efficiency and the quality of graphene copper wire products; the liquid seal solution is a mixed solution of an organic solvent with a reducing ability and a low boiling point and a raw material with an aromatic ring structure, which can not only reduce the oxygen content in the reaction chamber and clean the copper wire, but also provide a carbon source for generating graphene, so that the raw material can easily react to generate high-quality graphene; the conditions for low-temperature growth of graphene are adopted, the process temperature range is 300-600°C, and copper wire is directly used for production, while producing high-quality graphene copper wire, the process complexity is reduced, and the cost is saved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of copper processing and manufacturing, and in particular to a graphene copper wire and a preparation method thereof. Background Art

[0002] Copper has the advantages of good ductility, conductivity and low cost, and is widely used in the fields of electricity, machinery manufacturing, construction, etc.

[0003] Chemical vapor deposition (CVD) is a common method for preparing high-quality graphene in the laboratory and has important research value. Although the CVD method has successfully produced high-quality graphene in the laboratory, it faces huge challenges in converting it into actual production. First of all, because the molecular free path is longer under vacuum conditions, the raw materials are more likely to react on the surface of the copper wire, so traditional CVD is grown under high vacuum conditions. However, maintaining a high vacuum environment is extremely difficult and costly in industrial production. Secondly, achieving roll-to-roll production, that is, continuous and large-area preparation of graphene, is a huge technical challenge. In addition, many problems such as complex operation and difficult control also make the engineering of the CVD method face many difficulties.

[0004] In the face of the above challenges, the preparation of graphene by CVD under normal pressure shows its unique significance. First, normal pressure conditions avoid the operational difficulties and equipment cost problems caused by high vacuum environment, making the production process simpler and more economical. Secondly, the CVD method under normal pressure may be more conducive to roll-to-roll production, thereby preparing graphene continuously and over a large area, which is expected to greatly improve production efficiency. In addition, operation under normal pressure is also conducive to further research and optimization of the process of preparing graphene by CVD, providing more possibilities for the development of new graphene preparation technologies.

[0005] The present invention improves the growth efficiency of graphene through a series of technical means from the perspective of carbon source, and then reduces the oxygen content in the atmosphere to avoid the corrosion of the graphene structure by oxygen molecules at high temperature, thereby ensuring the growth of high-quality graphene under normal pressure or slightly positive pressure conditions. Ultimately, the above-mentioned engineering problem is solved.

[0006] The Chinese invention patent with application publication number CN113481406A discloses a graphene copper wire and a preparation method thereof, which belongs to the first method mentioned above. It uses a few-layer graphene oxide powder and oxygen-free copper powder as raw materials to prepare a mixed powder, and prepares a graphene copper sintered blank by low-temperature hot pressing sintering. After vacuum melting by adding auxiliary materials, a graphene copper alloy with a volume content of more than 99.99% is prepared, and the graphene copper wire can be modified by annealing the graphene copper wire to rearrange and connect the graphene and the copper lattice to prepare a graphene copper wire with high electrical conductivity and high thermal conductivity. The graphene copper wire of the present invention can increase the thermal conductivity coefficient to 500W / m·K~600W / m·K in terms of thermal conductivity, so as to improve the heat conduction capacity generated by electronic components. At the same time, in terms of electrical conductivity characteristics, the volume resistivity can be reduced by 5%~20%, and the electrical conductivity percentage can be increased to 102%~120%.

[0007] The Chinese invention patent with application publication number CN114388167A discloses a graphene copper wire, a preparation method thereof and a cable, which belongs to the second method mentioned above. Isotropic flake graphene is evenly distributed inside the graphene copper wire; the graphene copper wire has a tensile strength of ≥230MPa, a conductivity of ≥116%IACS and an elongation of ≥20% at 20°C; the method comprises the following steps: hot isostatic pressing of graphene copper foil to obtain a graphene copper block, machining of the graphene copper block to obtain a copper rod, hot extrusion of the copper rod to obtain a copper rod, wire drawing and annealing of the copper rod to obtain the graphene copper wire; the preparation method realizes uniform distribution, high content and isotropy of graphene in the copper wire through chemical vapor deposition and hot isostatic pressing, and also makes the graphene copper wire have high conductivity. At the same time, vacuum hot extrusion and other steps are used to ensure the mechanical strength of the graphene copper wire. The low-cost and high-yield process makes the graphene copper wire suitable for preparing cables, thereby greatly reducing the power loss on the cable.

[0008] Both methods require the preparation of graphene copper wire at extremely high temperatures (greater than 1000°C, close to the melting point of copper). The former uses graphene oxide, which is very difficult to disperse during smelting and has a complex process. The diameter of the copper wire raw material used changes greatly during the processing (from 8 or 2.6mm to 0.015-0.6mm). The latter uses high vacuum conditions, uses methane as a carbon source, and can only use copper foil as a raw material, that is, the product can only be a sheet copper product. Both are difficult to industrialize and cannot achieve continuous production, resulting in very high energy consumption and costs, and cannot be successfully applied in downstream fields. Summary of the invention

[0009] In view of one or more of the above problems, the first aspect of the present invention provides a method for preparing a graphene copper wire, comprising the following steps:

[0010] The reaction chamber of the tubular furnace is controlled to be in a positive pressure state, and the oxygen content is less than 1ppm;

[0011] A compound with an aromatic ring structure is used as a carbon source for generating graphene to generate graphene copper wire.

[0012] According to one aspect of the present invention, the step of controlling the reaction chamber of the tubular furnace to be in a positive pressure state and the oxygen content to be less than 1 ppm comprises:

[0013] The tubular furnace is provided with a liquid sealing structure, wherein the liquid sealing solution of the liquid sealing structure has no oxidizing ability and does not react with copper;

[0014] A mixed gas of inert gas and hydrogen is introduced into the reaction chamber of the tubular furnace, and the hydrogen with reducing ability reduces the oxygen in the reaction chamber of the tubular furnace;

[0015] The inlet for the copper wire to enter the tube furnace from the liquid seal is set at 1 cm away from the liquid surface of the liquid seal.

[0016] According to one aspect of the present invention, the liquid seal structure may use an organic solvent with reducing ability as the liquid seal solution, and the organic solvent with reducing ability includes one or a combination of ethanol and benzene;

[0017] Preferably, the proportion of hydrogen in the mixed gas is 1% to 20%;

[0018] Preferably, the gas flow rate is 100 to 1000 sccm, preferably 10 to 60 sccm.

[0019] According to one aspect of the present invention, the gas pressure in the reaction chamber of the tubular furnace is 40Pa higher than the external atmospheric pressure.

[0020] According to one aspect of the present invention, the copper wire is subjected to a pre-reaction treatment, comprising:

[0021] The copper wire stays in a heating zone of a tubular furnace reaction chamber at 100° C. to 400° C. for 10 to 20 seconds to generate an oxide layer;

[0022] A mixed gas of inert gas and hydrogen is introduced into the reaction chamber of the tubular furnace, and the oxide layer is reduced by the hydrogen.

[0023] According to one aspect of the present invention, a copper wire is cleaned, comprising:

[0024] The copper wire is passed through the liquid seal, and the copper wire is cleaned by a solution in the liquid seal.

[0025] According to one aspect of the present invention, the compound having an aromatic ring structure is a nitrogen-containing aromatic compound, specifically one or a combination of aniline, pyrrole, nitrobenzene, phenylenediamine, phenylacetonitrile, benzidine, diazonium, quinoline, bipyridine or o-phenanthroline.

[0026] According to one aspect of the present invention, the process temperature for generating the graphene copper wire is controlled between 300 and 600° C., and the reaction time is controlled between 5 and 20 seconds.

[0027] According to one aspect of the present invention, after the graphene copper wire is generated, the wire is taken up; when the heating zone length of the tubular furnace reaction chamber is 1.2 m, the take-up speed is controlled to be 0.06-0.24 m / s.

[0028] A second aspect of the present invention provides a graphene copper wire, which is prepared using the above-mentioned method for preparing the graphene copper wire.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] The invention provides a graphene copper wire and a preparation method thereof. The invention adopts two means, namely, a liquid seal structure design and the introduction of a reducing atmosphere, to reduce the oxygen content of a reaction chamber, while maintaining the reaction chamber in a positive pressure state, thereby improving production efficiency and the quality of the graphene copper wire product. The liquid seal solution is a mixed solution of an organic solvent with a reducing ability and a low boiling point and a raw material with an aromatic ring structure, which can not only further reduce the oxygen content of the reaction chamber, but also clean the copper wire and provide a carbon source for generating graphene, so that the raw material can easily react to generate high-quality graphene. The conditions for low-temperature growth of graphene are adopted, the process temperature range is 300-600°C, and copper wire is directly used as a raw material for production, so that while producing high-quality graphene copper wire, the process complexity is reduced and the cost is saved. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:

[0032] Figure 1 This is the Raman spectrum of graphene on pristine copper wire;

[0033] Figure 2 This is the Raman spectrum of graphene without liquid seal positive pressure;

[0034] Figure 3 This is the Raman spectrum of graphene grown after wiping the surface with ethanol;

[0035] Figure 4 This is the Raman spectrum of graphene grown on copper wire after oxidation. DETAILED DESCRIPTION

[0036] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. Preferred embodiments of the present invention are given below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0037] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0038] This article relates to numerical ranges. Unless otherwise specified, the above numerical ranges are considered continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0039] The temperature parameters herein, unless otherwise specified, allow for both constant temperature treatment and treatment within a certain temperature range. The constant temperature treatment allows for temperature fluctuations within the precision range of instrument control.

[0040] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.

[0041] In a specific embodiment, the present invention provides a method for preparing a graphene copper wire, the method comprising the following steps:

[0042] S1. The copper wire is treated before reaction.

[0043] In some embodiments, the treatment includes a cleaning treatment, wherein the copper wire is cleaned by a reducing solution in a liquid sealing device provided in a tube furnace.

[0044] Preferably, an organic solvent with reducing ability and low boiling point such as ethanol or benzene is used as a liquid seal to clean the copper wire when the copper wire passes through the liquid seal.

[0045] In some embodiments, the copper wire is wiped with felt, cloth or other materials that can absorb liquid and can be used for wiping. The wiping material needs to be soaked in a solution such as ethanol or benzene that has a certain reducing ability, a low boiling point and does not react with copper.

[0046] In some embodiments, the copper wire is treated by oxidation-reduction means to produce a relatively uniform oxide layer on the surface of the copper wire to further protect the surface of the copper wire, and then the oxide layer is removed by reduction to completely expose the surface of the copper wire.

[0047] Specifically, the copper wire stays in a heating zone of a tubular furnace reaction chamber at 100°C to 400°C for 10 to 20 seconds to generate an oxide layer; a mixture of inert gas and hydrogen is introduced into the tubular furnace reaction chamber, and the oxide layer is reduced by the hydrogen. In some specific examples, the temperature may be 100°C, 200°C, 300°C or 400°C; the residence time may be 10 seconds, 11 seconds, 12 seconds, 13 seconds, 14 seconds, 15 seconds, 16 seconds, 17 seconds, 18 seconds, 19 seconds or 20 seconds.

[0048] Preferably, the copper wire stays in the heating zone of the tubular furnace reaction chamber at 200° C. for 10 seconds to generate an oxide layer.

[0049] By treating the copper wire, the antioxidants or additives that are beneficial to processing efficiency coated on the surface of the copper wire during processing, as well as the organic matter and dust in the air adsorbed during the placement process, are removed, so that the copper wire is completely exposed, even if the surface of the copper wire is not covered by any molecules.

[0050] S2. Control the gas pressure in the tubular furnace reaction chamber to be in a positive pressure state, and the oxygen content is less than 1ppm.

[0051] In some embodiments, the tube furnace is provided with a liquid sealing structure, and the liquid sealing solution of the liquid sealing structure has no oxidizing ability and does not react with copper, and can be, for example, water.

[0052] Preferably, the liquid seal structure solution adopts an organic solvent with reducing ability, and the reducing solvent is used as a liquid seal to reduce the oxygen in the reaction chamber of the tubular furnace.

[0053] Preferably, the organic solvent having reducing ability includes ethanol, benzene or a combination thereof.

[0054] Preferably, the liquid sealing solution of the liquid sealing structure can also adopt a mixed solution of the organic solvent with reducing ability and the compound with aromatic ring structure, so that the oxygen content in the reaction chamber can be reduced by the liquid sealing solution, the copper wire can be cleaned, and the carbon source for growing graphene can be attached to the surface of the copper wire, so that graphene can be more easily grown on the surface of the copper wire.

[0055] In some embodiments, a high-precision instrument for measuring the oxygen content in real time may be installed in the reaction chamber to determine that the oxygen content is less than 1 ppm.

[0056] In some embodiments, a mixture of inert gas and hydrogen is introduced into the tubular furnace reaction chamber, and the hydrogen with reducing ability reduces the oxygen in the tubular furnace reaction chamber.

[0057] Specifically, the inert gas is one or a combination of argon or nitrogen.

[0058] Specifically, the proportion of hydrogen in the mixed gas is 1% to 100%. In some specific examples, the proportion of hydrogen in the mixed gas can be 1%, 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90% or 100%. The hydrogen can neutralize the oxygen in the system, thereby reducing the oxygen content of the reaction environment to improve the quality of the generated graphene copper wire.

[0059] Specifically, the flow rate of the mixed gas of the inert gas and hydrogen is 1 to 1000 sccm, preferably, 5 to 60 sccm. In some specific examples, the flow rate of the mixed gas of the inert gas and hydrogen can be 1 sccm, 100 sccm, 200 sccm, 300 sccm, 400 sccm, 500 sccm, 600 sccm, 700 sccm, 800 sccm, 900 sccm or 1000 sccm.

[0060] In some embodiments, the entrance of the copper wire from the liquid seal into the tube furnace is set at 1 cm away from the liquid surface of the liquid seal. The farther the pipeline outlet is from the liquid surface, the greater the pressure difference between the reaction chamber of the tube furnace and the external atmospheric pressure.

[0061] In some embodiments, the gas pressure in the tubular furnace reaction chamber is 40 Pa higher than normal pressure, which reduces the requirements for reaction conditions, thereby simplifying the production process and improving production efficiency.

[0062] The present invention adopts a tubular furnace with a liquid sealing structure to produce graphene copper wires. The liquid sealing structure is used to maintain a micro-positive pressure environment of a reaction chamber of the tubular furnace. The copper wire is used as a raw material for production, so the production process is simpler, thereby improving production efficiency. By adding low-boiling-point and reducing reagents such as benzene and ethanol to a sealing solution, and introducing a mixed gas containing hydrogen, the oxygen content in the reaction chamber is reduced, the contact between the copper material and oxygen is reduced, and the quality of the prepared graphene copper material is improved.

[0063] S3. Using a raw material having an aromatic ring structure as a carbon source for generating graphene to generate graphene copper wire.

[0064] In some embodiments, the compound with an aromatic ring structure is a nitrogen-containing aromatic compound, specifically one or more of aniline, pyrrole, nitrobenzene, phenylenediamine, phenylacetonitrile, benzidine, diazonium, quinoline, bipyridine and o-phenanthroline and their derivatives. The use of compounds with an aromatic ring structure makes it easier to react to generate graphene. The use of nitrogen-containing aromatic compounds can make the generated graphene contain nitrogen elements, thereby increasing the conductivity of the graphene.

[0065] In some embodiments, the liquid seal structure may use a compound containing the above-mentioned aromatic ring structure as a liquid seal solution. When the copper wire passes through the liquid seal, the compound with the aromatic ring structure may adhere to its surface to make the subsequent reaction of generating graphene easier to proceed.

[0066] In some embodiments, a mixture of inert gas and hydrogen is introduced into the tubular furnace reaction chamber as a protective gas, and the compound having an aromatic ring structure is blown into the reaction chamber through the mixed gas, and reacts on the surface of the copper wire to generate graphene after contacting the copper wire.

[0067] In some embodiments, the oxide layer on the surface of the copper wire is reduced by the above hydrogen, and in the case where the reaction chamber has a compound with an aromatic ring structure, graphene is grown on the surface of the copper wire after the oxide layer is reduced.

[0068] In some embodiments, the conditions for low-temperature growth of graphene are adopted, the process temperature range is 300-600°C, and the reaction time is controlled within 5-20 seconds. In some specific examples, the process temperature can be 300°C, 400°C, 500°C or 600°C; the reaction time can be 5 seconds, 10 seconds, 15 seconds or 20 seconds. Among them, 300°C is the lowest temperature for graphene to grow on the surface of copper under normal pressure or slightly positive pressure, and 600°C is the limit temperature to prevent excessive changes in copper grain boundaries.

[0069] In some embodiments, a wire taking-up mechanism and a wire unwinding mechanism are provided at both ends of the tubular furnace. The wire is unwinded by the wire unwinding mechanism and wound up by the wire taking-up mechanism, so that the copper wire is routed in the tubular furnace to achieve the effect of continuous production of graphene copper wire.

[0070] It is well known to those skilled in the art that the heating temperature and reaction time are related to the routing speed and the reduction of the copper wire. When the routing speed is high, the copper wire stays in the heating zone of the tubular furnace reaction chamber for a shorter time, and the actual heating time is shorter. In this case, the preferred process temperature range is 400-500°C, for example, 400°C, 420°C, 440°C, 460°C, 480°C or 500°C, and 500°C is most preferred.

[0071] In some embodiments, after the graphene copper wire is generated, the wire is taken up; when the length of the heating zone of the tubular furnace reaction chamber is 1.2 m, the take-up speed is controlled to be 0.06 to 0.24 m / s.

[0072] Another embodiment of the present invention provides a graphene copper wire, which is prepared by the above-mentioned method for preparing the graphene copper wire.

[0073] In one example, the conductivity of the graphene copper wire was 105.25% IACS.

[0074] In one example, the conductivity of the graphene copper wire was 105.33% IACS.

[0075] It should be clear that the use of the process provided by the embodiment of the present invention or the replacement or change of conventional data all fall within the protection scope and disclosure scope of the present invention.

[0076] The present application is described below through specific embodiments.

[0077] Example 1

[0078] Use felt soaked in ethanol to clamp the copper wire and pass it through to clean the surface of the copper wire; after threading, pass nitrogen in the tube furnace, and control the gas flow rate at 30sccm to maintain a slightly positive pressure state in the furnace (greater than atmospheric pressure by about 40Pa); place o-phenanthroline in the non-heating area of ​​the cavity, and blow 30sccm of nitrogen into the reaction cavity; after the temperature of the reaction cavity is controlled to 400℃, start routing, and at this time, the surface of the copper wire is coated with graphene. The length of the heating zone of the reaction cavity is 1.2m, and the winding speed is controlled to be 0.12m / s.

[0079] Example 2

[0080] The copper wire surface was treated by oxidation at 200℃ for 10s; after threading, nitrogen-hydrogen mixed gas (hydrogen ratio 5%) was introduced into the tube furnace, and the gas flow rate was controlled at 30sccm to maintain a slightly positive pressure state in the furnace (greater than atmospheric pressure by about 40Pa); o-phenanthroline was placed in the non-heating area of ​​the cavity, and 30sccm of nitrogen-hydrogen mixed gas was blown into the reaction cavity; the temperature of the reaction cavity was controlled at 500℃ before the wire was routed, and the copper wire surface was reduced and coated with graphene. The length of the heating zone of the reaction cavity was 1.2m, and the winding speed was controlled to be 0.12m / s.

[0081] Example 3

[0082] Use felt soaked in ethanol to clamp the copper wire and pass it through, and use ethanol for secondary cleaning at the liquid seal; after threading, pass nitrogen in the tube furnace, and control the gas flow rate at 30sccm to maintain a slightly positive pressure state in the furnace (greater than atmospheric pressure by about 40Pa); place the gel containing nitrobenzene in the non-heating area of ​​the cavity, and blow 30sccm of nitrogen into the reaction cavity; after the temperature of the reaction cavity is controlled at 300℃, start routing, and the surface of the copper wire is coated with graphene. The length of the heating zone of the reaction cavity is 1.2m, and the winding speed is controlled to be 0.12m / s.

[0083] Example 4

[0084] The copper wire surface was treated by oxidation at 400℃ for 5s; after threading, nitrogen-hydrogen mixed gas (hydrogen ratio 5%) was introduced into the tubular furnace, and the gas flow rate was controlled at 30sccm to maintain a slightly positive pressure state in the furnace (greater than atmospheric pressure by about 40Pa); o-phenanthroline was placed in the non-heating area of ​​the cavity, and 30sccm of nitrogen-hydrogen mixed gas was blown into the reaction cavity; the temperature of the reaction cavity was controlled at 600℃ before the wire was routed, and the copper wire surface was reduced and coated with graphene. The length of the heating zone of the reaction cavity was 1.2m, and the winding speed was controlled to be 0.2m / s.

[0085] Figure 1 This is the Raman spectrum of graphene on pristine copper wire; Figure 2 This is the Raman spectrum of graphene without liquid seal positive pressure; Figure 3 This is the Raman spectrum of graphene grown after wiping the surface with ethanol; Figure 4 This is the Raman spectrum of graphene grown on copper wire after oxidation. Figure 1-Figure 4 The ordinate represents the Raman intensity, which can be expressed in any unit, and the abscissa represents the Raman frequency shift, in wavenumber cm -1 ,pass Figure 1-Figure 4 It can be seen that the graphene prepared by the preparation method provided by the present invention has better quality.

[0086] Taking 115μm copper wire as an example, the conductivity of the sample before and after graphene growth is shown in Table 1, the 200℃ anti-oxidation time is shown in Table 2, and the 1575 / 2117 Raman ratio is shown in Table 3:

[0087] Table 1

[0088]

[0089] Table 2

[0090]

[0091] Table 3

[0092]

[0093]

[0094] It can be seen from Tables 1, 2 and 3 that the preparation method of the graphene copper wire provided by the present invention can prepare a graphene copper wire with higher conductivity, and its anti-oxidation time and Raman ratio are also improved.

[0095] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a graphene copper wire, characterized in that: include: The reaction chamber of the tubular furnace is controlled to be in a positive pressure state, and the oxygen content is less than 1ppm; Using a compound with an aromatic ring structure as a carbon source for generating graphene, graphene copper wire is generated, and the reaction time is controlled within 5 to 20 seconds; The gas pressure of the tubular furnace reaction chamber is 40Pa higher than the external atmospheric pressure, the process temperature of generating graphene copper wire is controlled between 300 and 600°C, and the control of the tubular furnace reaction chamber to a positive pressure state and an oxygen content lower than 1ppm includes: The tubular furnace is provided with a liquid sealing structure, the liquid sealing solution of the liquid sealing structure has no oxidizing ability and does not react with copper, and the liquid sealing solution adopts a mixed solution of an organic solvent with reducing ability and a compound with an aromatic ring structure; A mixed gas of inert gas and hydrogen is introduced into the reaction chamber of the tubular furnace, and the oxygen in the reaction chamber of the tubular furnace is reduced by the hydrogen having reducing ability; The compound having an aromatic ring structure is a nitrogen-containing aromatic compound, and the nitrogen-containing aromatic compound is specifically one or a combination of aniline, pyrrole, nitrobenzene, phenylenediamine, phenylacetonitrile, benzidine, diazonium, quinoline, bipyridine or o-phenanthroline; the organic solvent having reducing ability includes one or a combination of ethanol and benzene.

2. The method for preparing graphene copper wire according to claim 1, characterized in that: The control of the tubular furnace reaction chamber to a positive pressure state and an oxygen content lower than 1 ppm includes: The inlet for the copper wire to enter the tube furnace from the liquid seal is set at 1 cm away from the liquid surface of the liquid seal.

3. The method for preparing graphene copper wire according to claim 2, characterized in that: The proportion of hydrogen in the mixed gas is 1% to 20%.

4. The method for preparing graphene copper wire according to claim 2, characterized in that: The gas flow rate of the mixed gas is 100-1000 sccm.

5. The method for preparing graphene copper wire according to claim 2, characterized in that: The gas flow rate of the mixed gas is 10-60 sccm.

6. The method for preparing graphene copper wire according to claim 1, characterized in that: The copper wire is treated before reaction, including: The copper wire stays in a heating zone of a tubular furnace reaction chamber at 100° C. to 400° C. for 10 to 20 seconds to generate an oxide layer; A mixed gas of inert gas and hydrogen is introduced into the reaction chamber of the tubular furnace, and the oxide layer is reduced by the hydrogen.

7. The method for preparing graphene copper wire according to claim 1, characterized in that: Cleaning of copper wires, including: The copper wire is passed through the liquid seal, and the copper wire is cleaned by a solution in the liquid seal.

8. The method for preparing graphene copper wire according to claim 1, characterized in that: After the graphene copper wire is generated, winding the wire; When the heating zone length of the tubular furnace reaction chamber is 1.2 m, the wire take-up speed is controlled to be 0.06 to 0.24 m / s.

9. A graphene copper wire, characterized in that: The graphene copper wire is prepared by the method for preparing the graphene copper wire according to any one of claims 1 to 8.