Preparation method and application of lithium iron phosphate composite material

Through the hydrothermal reaction of polyvinyl alcohol-phytic acid microsphere template agent and iron salt and the calcination of lithium hydroxide, a carbon-coated lithium iron phosphate composite material is formed, which solves the problem of low conductivity and diffusivity of lithium iron phosphate cathode material. problem, significantly improving the specific capacity and cycle stability of lithium-ion batteries.

CN117832427BActive Publication Date: 2024-10-08GUIZHOU SHENGZEWEI CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311728874.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-15
Publication Date
2024-10-08
Estimated Expiration
2043-12-15

AI Technical Summary

Technical Problem

Lithium iron phosphate cathode material has low electronic conductivity and ion diffusivity, which limits its promotion and application in lithium-ion batteries.

Method used

Using polyvinyl alcohol as the carbon source, lithium iron phosphate is coated and modified through carbothermal reduction method to improve its conductivity and cycle stability. Specific steps include using polyvinyl alcohol-phytic acid microsphere template agent and iron salt for hydrothermal reaction to generate microspherical iron phosphate precursor, which is then calcined with lithium hydroxide after ultrasonic vibration treatment to form carbon-coated microspheres. Spherical lithium iron phosphate composite material.

Benefits of technology

It significantly improves the actual specific capacity and cycle stability of lithium iron phosphate composite materials, enhances charge transport and lithium ion deintercalation capabilities, and improves the battery performance of lithium ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117832427B_ABST
    Figure CN117832427B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of lithium iron phosphate, and discloses a preparation method and application of a lithium iron phosphate composite material, with lithium hydroxide as a lithium source. Polyvinyl alcohol microspheres are used as a carbon source, and a carbon-coated microspherical lithium iron phosphate composite material is obtained through a carbon thermal reduction method. As the positive electrode of a lithium ion battery, after carbon coating modification, the lithium iron phosphate composite material has higher conductivity, promotes the transfer of charges and the deintercalation of lithium ions during battery charging and discharging, and improves the specific capacity of the positive electrode material. In addition, the microspherical lithium iron phosphate has a high specific surface area and can provide more lithium ion deintercalation sites. The lithium iron phosphate composite material prepared by the present invention has a higher specific capacity and capacity retention rate as a positive electrode material for lithium ion batteries, and has excellent cycle stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium iron phosphate, and in particular to a preparation method and application of a lithium iron phosphate composite material. Background Art

[0002] The positive electrode materials of lithium-ion batteries mainly include lithium iron phosphate, nickel cobalt oxide, and lithium nickel cobalt manganese oxide. Among them, lithium iron phosphate positive electrode materials have the advantages of high specific capacity and good thermal stability, and are the most promising positive electrode materials for lithium-ion batteries. However, lithium iron phosphate positive electrode materials have low electronic conductivity and ion diffusion chamber coefficient, which hinders their promotion and application. At present, the modification methods of lithium iron phosphate positive electrode materials mainly include carbon coating, metal ion doping, etc., which can effectively improve the actual specific capacity and cycle stability of lithium iron phosphate positive electrode materials. Carbon materials have high conductivity, low density, and light weight, and are widely used in lithium-ion battery electrode materials. At present, the raw materials for carbon coating modification of lithium iron phosphate mainly include glucose, microorganisms, graphene, etc. Polyvinyl alcohol is a degradable green and environmentally friendly material. The present invention aims to use polyvinyl alcohol as a carbon source to achieve coating modification of lithium iron phosphate by carbon thermal reduction method to improve the actual specific capacity and cycle stability of positive electrode materials. Summary of the invention

[0003] The technical problem solved by the present invention is: to provide a method for preparing a novel carbon-coated lithium iron phosphate composite material, which, as a positive electrode material for lithium-ion batteries, has higher actual specific capacity and cycle stability.

[0004] The technical solution of the present invention:

[0005] A preparation method of lithium iron phosphate composite material:

[0006] Step (1): Add polyvinyl alcohol-phytic acid microsphere template into water, place in an ultrasonic oscillator, perform ultrasonic dispersion treatment, then add an aqueous solution of iron salt, add into a hydrothermal reactor to react, cool, filter, wash the filter cake with deionized water, and dry to obtain a microspherical polyvinyl alcohol microsphere-loaded iron phosphate precursor.

[0007] Step (2): polyvinyl alcohol microspheres loaded with iron phosphate precursor and lithium hydroxide are added to water, placed in an ultrasonic oscillator, and ultrasonically dispersed. The solution is then placed in a tube furnace, argon gas is introduced, the temperature is increased, calcined, cooled, the calcined product is washed with deionized water, and dried to obtain a lithium iron phosphate composite material.

[0008] Furthermore, the iron salt includes ferric chloride, ferric sulfate, and ferric nitrate.

[0009] Furthermore, the mass ratio of the polyvinyl alcohol-phytic acid microsphere template agent and the iron salt is 1:(0.2-0.6).

[0010] Furthermore, the reaction in step (1) is carried out at 100-140° C. for 6-12 h.

[0011] Furthermore, in step (2), the mass ratio of the polyvinyl alcohol microspheres loaded with iron phosphate precursor and lithium hydroxide is 1:(0.12-0.18).

[0012] Furthermore, the heating rate of calcination in step (2) is 3-10°C / min, firstly heating to 350-450°C, keeping the temperature for 2-4 h, then heating to 650-750°C, keeping the temperature for 3-5 h.

[0013] Furthermore, the polyvinyl alcohol-phytic acid microsphere template is prepared according to the following method: polyvinyl alcohol is added to water, heated and stirred to dissolve, then phytic acid is added, poured into a hydrothermal reactor for hydrothermal reaction, cooled, filtered, the filter cake is washed with deionized water, and dried to obtain the polyvinyl alcohol-phytic acid microsphere template.

[0014] Furthermore, the mass ratio of polyvinyl alcohol to phytic acid is 1:0.8-2.

[0015] Further, the hydrothermal reaction is carried out at 80-110° C. for 3-8 h.

[0016] The technical effect of the present invention is as follows: the present invention uses phytic acid as a cross-linking agent to cross-link with polyvinyl alcohol to obtain a polyvinyl alcohol-phytic acid microsphere template; under hydrothermal reaction conditions, the phosphate groups in the polyvinyl alcohol-phytic acid microspheres react with iron salts to generate iron phosphate precursors, and at the same time, the polyvinyl alcohol-phytic acid microspheres are used as templates to make the iron phosphate precursor grow in situ on the surface of the polyvinyl alcohol-phytic acid microspheres to obtain microspherical polyvinyl alcohol microspheres loaded with iron phosphate precursors, and finally lithium hydroxide is used as a lithium source. The polyvinyl alcohol microspheres are used as a carbon source, and a carbon-coated microspherical lithium iron phosphate composite material is obtained through a carbon thermal reduction method.

[0017] The lithium iron phosphate composite material is used as the positive electrode of the lithium ion battery. After being modified by carbon coating, the lithium iron phosphate composite material has higher conductivity, promotes the transmission of charge and the deintercalation of lithium ions during battery charging and discharging, and improves the specific capacity of the positive electrode material. In addition, the microspherical lithium iron phosphate has a high specific surface area and can provide more lithium ion deintercalation sites. The lithium iron phosphate composite material prepared by the present invention is used as a positive electrode material for lithium ion batteries, has higher specific capacity and capacity retention rate, and has excellent cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is the first charge and discharge curve of a lithium-ion battery.

[0019] Figure 2 It is a lithium-ion battery cycle performance curve. Implementation

[0020] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example

[0021] Add 1 g of polyvinyl alcohol to 15 mL of water, heat and stir to dissolve, then add 0.8 g of phytic acid, pour into a hydrothermal reactor for hydrothermal reaction, react at 100° C. for 8 h, cool, filter, wash the filter cake with deionized water, and dry to obtain a polyvinyl alcohol-phytic acid microsphere template agent.

[0022] 3 g of polyvinyl alcohol-phytic acid microsphere template agent was added to 60 mL of water, placed in an ultrasonic oscillator, and ultrasonically dispersed. Then, 10 mL of an aqueous solution containing 0.6 g of ferric chloride was added and added to a hydrothermal reactor. The mixture was reacted at 100 ° C for 12 h, cooled, filtered, the filter cake was washed with deionized water, and dried to obtain a microspherical polyvinyl alcohol microsphere-loaded iron phosphate precursor.

[0023] 3 g of microspherical polyvinyl alcohol microspheres loaded with iron phosphate precursor and 0.36 g of lithium hydroxide were added to water and placed in an ultrasonic oscillator for ultrasonic dispersion treatment. The solution was then placed in a tubular furnace and introduced with argon gas. The heating rate was 3°C / min, first raised to 350°C and kept warm for 4 h, then raised to 750°C and calcined for 3 h. The mixture was cooled, the calcined product was washed with deionized water, and dried to obtain a microspherical lithium iron phosphate composite material. Example

[0024] Add 1 g of polyvinyl alcohol into 15 mL of water, heat and stir to dissolve, then add 1.3 g of phytic acid, pour into a hydrothermal reactor for hydrothermal reaction, react at 80°C for 8 h, cool, filter, wash the filter cake with deionized water, and dry to obtain a polyvinyl alcohol-phytic acid microsphere template agent.

[0025] 3 g of polyvinyl alcohol-phytic acid microsphere template was added to 60 mL of water, placed in an ultrasonic oscillator, and ultrasonically dispersed. Then, 15 mL of an aqueous solution containing 1.2 g of ferric nitrate was added and added to a hydrothermal reactor. The reaction was carried out at 140 ° C for 8 h, cooled, filtered, the filter cake was washed with deionized water, and dried to obtain a microspherical polyvinyl alcohol microsphere-loaded iron phosphate precursor.

[0026] 3 g of microspherical polyvinyl alcohol microspheres loaded with iron phosphate precursor and 0.45 g of lithium hydroxide were added to water, placed in an ultrasonic oscillator, and ultrasonically dispersed. Then the solution was placed in a tubular furnace, argon gas was introduced, the heating rate was 3°C / min, the temperature was first raised to 400°C, kept warm for 3 hours, then raised to 650°C, kept warm for 4 hours, cooled, the calcined product was washed with deionized water, and dried to obtain a microspherical lithium iron phosphate composite material. Example

[0027] Add 1 g of polyvinyl alcohol to 15 mL of water, heat and stir to dissolve, then add 2 g of phytic acid, pour into a hydrothermal reactor for hydrothermal reaction, react at 110° C. for 3 h, cool, filter, wash the filter cake with deionized water, and dry to obtain a polyvinyl alcohol-phytic acid microsphere template.

[0028] 3 g of polyvinyl alcohol-phytic acid microsphere template was added to 60 mL of water, placed in an ultrasonic oscillator, and ultrasonically dispersed. Then, 30 mL of an aqueous solution containing 1.8 g of ferric sulfate was added and added to a hydrothermal reactor. The reaction was carried out at 140 ° C for 6 h, cooled, filtered, the filter cake was washed with deionized water, and dried to obtain a microspherical polyvinyl alcohol microsphere-loaded iron phosphate precursor.

[0029] 3 g of microspherical polyvinyl alcohol microspheres loaded with iron phosphate precursor and 0.54 g of lithium hydroxide were added to water and placed in an ultrasonic oscillator for ultrasonic dispersion treatment. The solution was then placed in a tubular furnace and introduced with argon gas. The heating rate was 10°C / min, first raised to 450°C and kept warm for 2 h, then raised to 700°C and calcined for 5 h. The mixture was cooled, the calcined product was washed with deionized water, and dried to obtain a microspherical lithium iron phosphate composite material.

[0030] Comparative Example 1

[0031] 1.3 g of phytic acid microsphere template was added to 60 mL of water, placed in an ultrasonic oscillator, and ultrasonically dispersed. Then, 10 mL of an aqueous solution containing 0.6 g of ferric chloride was added and added to a hydrothermal reactor. The mixture was reacted at 100 ° C for 12 h, cooled, filtered, the filter cake was washed with deionized water, and dried to obtain an iron phosphate precursor.

[0032] 2.3 g of iron phosphate precursor and 0.36 g of lithium hydroxide were added to water, placed in an ultrasonic oscillator, and ultrasonically dispersed. The solution was then placed in a tubular furnace, and argon gas was introduced. The heating rate was 3°C / min, first raised to 350°C, kept warm for 4 hours, then raised to 800°C, kept warm for calcination for 3 hours, cooled, and the calcined product was washed with deionized water and dried to obtain lithium iron phosphate.

[0033] Comparative Example 2

[0034] 1.3 g of phytic acid microsphere template was added to 60 mL of water, placed in an ultrasonic oscillator, and ultrasonically dispersed. Then, 10 mL of an aqueous solution containing 0.6 g of ferric chloride was added and added to a hydrothermal reactor. The mixture was reacted at 100 ° C for 12 h, cooled, filtered, the filter cake was washed with deionized water, and dried to obtain an iron phosphate precursor.

[0035] 0.7 g of polyvinyl alcohol, 2.3 g of iron phosphate precursor, and 0.36 g of lithium hydroxide were added to water, placed in an ultrasonic oscillator, and ultrasonically dispersed. Then the solution was placed in a tubular furnace, argon was introduced, and the heating rate was 3°C / min. The temperature was first raised to 350°C and kept warm for 4 h, then raised to 800°C and calcined for 3 h. The mixture was cooled, the calcined product was washed with deionized water, and dried to obtain a lithium iron phosphate composite material.

[0036] Lithium iron phosphate, acetylene black and polytetrafluoroethylene were added to N-methylpyrrolidone in a mass ratio of 80:12:8, ground and mixed evenly, the slurry was coated on the surface of aluminum foil, and dried at 110°C for 24 hours to obtain a positive electrode sheet. A metal lithium sheet was used as the negative electrode, a polypropylene microporous membrane was used as the diaphragm, and a 1 mol / L LiPF6 dimethyl carbonate + ethylene carbonate solution was used as the electrolyte. The battery was assembled in a glove box. A battery charge and discharge tester was used for constant current charge and discharge cycle testing. The scanning voltage range was 2.0 to 4.5 V. The current density of the test was 0.1 C.

[0037] manual Figure 1 and Figure 2 The test results are shown in the following table.

[0038] Table 1 Lithium-ion battery first charge and discharge and cycle performance test table

[0039]

[0040] When the current density is 0.1 C, the initial specific capacity of Example 3 reaches 163.7 mAg / h, and after 100 cycles, the capacity retention rate of Example 2 reaches 95.55%, which has excellent cycle stability.

[0041] The initial specific capacity of Comparative Example 1 was only 131.2 mAg / h, and the capacity retention rate was only 83.69%.

[0042] The initial specific capacity of Comparative Example 2 was only 126.0 mAg / h, and the capacity retention rate was only 77.06%.

[0043] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a lithium iron phosphate composite material, characterized in that: The lithium iron phosphate composite material is prepared according to the following method: Step (1): adding polyvinyl alcohol-phytic acid microsphere template agent to water, placing in an ultrasonic oscillator, ultrasonic dispersion treatment, then adding an aqueous solution of iron salt, adding to a hydrothermal reactor for reaction, cooling, filtering, washing the filter cake with deionized water, and drying to obtain a polyvinyl alcohol microsphere-loaded iron phosphate precursor; Step (2): polyvinyl alcohol microspheres loaded with iron phosphate precursor and lithium hydroxide are added to water, placed in an ultrasonic oscillator, and ultrasonically dispersed. The solution is then placed in a tube furnace, argon gas is introduced, the temperature is increased, calcined, cooled, the calcined product is washed with deionized water, and dried to obtain a lithium iron phosphate composite material.

2. The method for preparing the lithium iron phosphate composite material according to claim 1, characterized in that: The iron salts include ferric chloride, ferric sulfate and ferric nitrate.

3. The method for preparing the lithium iron phosphate composite material according to claim 1, characterized in that: The mass ratio of the polyvinyl alcohol-phytic acid microsphere template agent to the iron salt is 1:(0.2-0.6).

4. The method for preparing the lithium iron phosphate composite material according to claim 1, characterized in that: The reaction in step (1) is carried out at 100-140° C. for 6-12 h.

5. The method for preparing the lithium iron phosphate composite material according to claim 1, characterized in that: In the step (2), the mass ratio of the polyvinyl alcohol microspheres loaded with iron phosphate precursor and lithium hydroxide is 1:(0.12-0.18).

6. The method for preparing the lithium iron phosphate composite material according to claim 1, characterized in that: The heating rate of calcination in step (2) is 3-10°C / min, firstly heating to 350-450°C, keeping the temperature for 2-4 hours, then heating to 650-750°C, keeping the temperature for 3-5 hours.

7. The method for preparing the lithium iron phosphate composite material according to claim 1, characterized in that: The polyvinyl alcohol-phytic acid microsphere template agent is prepared according to the following method: polyvinyl alcohol is added to water, heated and stirred to dissolve, then phytic acid is added, poured into a hydrothermal reactor for hydrothermal reaction, cooled, filtered, the filter cake is washed with deionized water, and dried to obtain the polyvinyl alcohol-phytic acid microsphere template agent.

8. The method for preparing the lithium iron phosphate composite material according to claim 7, characterized in that: The mass ratio of the polyvinyl alcohol to phytic acid is 1:0.8-2.

9. The method for preparing the lithium iron phosphate composite material according to claim 7, characterized in that: The hydrothermal reaction is carried out at 80-110° C. for 3-8 h.

10. Use of the lithium iron phosphate composite material according to any one of claims 1 to 9 in a positive electrode of a lithium ion battery.