A process for preparing silicon nitride ceramic microspheres

Through gas-phase chemical reaction and multiple sintering processes, high-density and high-strength silicon nitride ceramic microspheres were prepared, solving the problem of insufficient density and impact resistance of the spherical body in traditional processes, and achieving rapid molding and performance improvement.

CN117843375BActive Publication Date: 2024-11-01HENGYANG KAIXIN SPECIAL MATERIAL TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410009748.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-03
Publication Date
2024-11-01
Estimated Expiration
2044-01-03

AI Technical Summary

Technical Problem

The strength and impact resistance of existing silicon nitride ceramic balls are insufficient, and the traditional manufacturing process is complex and time-consuming, making it difficult to quickly form dense spheres.

Method used

Ultrafine silicon nitride powder is prepared by gas-phase chemical reaction, combined with carbon fiber, MgO powder and Y2O3-Al2O3 powder, and three sintering processes of high-temperature and high-pressure, discharge plasma and microwave sintering to form high-density and stable silicon nitride ceramic microspheres .

Benefits of technology

The rapid molding of high-density and high-strength silicon nitride ceramic microspheres has been achieved, which improves the densification degree and performance of the sphere, simplifies the process flow, and reduces the mechanical processing needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117843375B_ABST
    Figure CN117843375B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of silicon nitride ceramic balls, and discloses a process for preparing silicon nitride ceramic microspheres, including: step one, preparation of silicon nitride powder, synthesis of ultrafine silicon nitride powder by gas phase chemical reaction; step two, preparation of raw material preparation for silicon nitride ceramic microspheres; step three, raw material mixing and molding, mixing the prepared silicon nitride powder, carbon fiber, MgO powder, Y2O3-Al2O3 powder, pressurizing and molding, obtaining silicon nitride ceramic microsphere embryos; step four, drying, rapid evaporation of water, so as to carry out the next step of operation; step five, sintering, preliminary sintering, after the preliminary sintering is completed, secondary sintering is carried out, and finally, microwave sintering is adopted; step six, processing. Silicon nitride of the present invention is made into silicon nitride powder by gas phase chemical reaction, and the powder particle size is less than 1 μm, which is more conducive to forming a uniform and good organizational structure; high temperature and high pressure sintering, discharge plasma sintering, microwave sintering are adopted for three times, and high-density and high-strength silicon nitride ceramic microspheres are made.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of silicon nitride ceramic balls, and in particular relates to a process for preparing silicon nitride ceramic microspheres. Background Art

[0002] Silicon nitride, with the chemical formula Si3N4, is an important structural ceramic material. It is a superhard material that has lubricity and wear resistance, and is an atomic crystal; it is resistant to oxidation at high temperatures. It can also resist thermal shocks, and will not break even if it is heated to more than 1000°C in air, cooled rapidly, and then heated rapidly. It is precisely because of the excellent properties of silicon nitride ceramics that they are often used to manufacture mechanical components such as bearings, turbine blades, mechanical seal rings, and permanent molds.

[0003] Silicon nitride ceramic balls are precision ceramics sintered at high temperature in a non-oxidizing atmosphere. They have high strength, high wear resistance, high temperature resistance, corrosion resistance, acid and alkali resistance, can be used in seawater for a long time, and have good electrical and magnetic insulation properties. They have a low density, almost 1 / 3 the weight of bearing steel, and have low centrifugal force when rotating, which can achieve high-speed operation. They are also self-lubricating and can be used in environments with high pollution without lubricating media, making them the preferred balls for ceramic bearings and hybrid ceramic ball bearings. However, the strength and impact resistance of silicon nitride ceramic balls still need to be improved.

[0004] Silicon nitride ceramic bearing balls have extremely high requirements for dimensional accuracy. In the current manufacturing technology, the commonly used silicon nitride ball manufacturing processes include: pressureless sintering, hot pressing sintering, hot isostatic pressing sintering, cold isostatic pressing technology, etc. In the production of bearing parts, hot isostatic pressing is currently considered to be the best process for manufacturing silicon nitride blank balls, because this process is directly applicable to sealing preforming or part of the sintering production method, and can produce 100% dense materials. However, its process is complicated. The hot isostatic pressing method requires glass powder to spray the ball blank to form a porous shell, which is then placed in a vacuum special furnace for heating to remove the trapped air from the material and melt the glass. After controlled cooling, the glass layer becomes a sealing layer. After the hot pressing stage is completed, the pressure is reduced to promote the removal of glass from the ball. This will cause certain pollution to the silicon nitride ceramic ball. The preparation of silicon nitride ceramic balls by pressureless sintering cannot reach the degree of densification used, and hot pressing sintering takes too long. Cold isostatic pressing technology has the advantages of stability, uniformity and high density of green blanks, but cold isostatic pressing generally uses rubber molds, and the sphericity of the blanks is poor, resulting in a large amount of machining and grinding required for the sintered ball blanks to meet the requirements of bearing balls. Therefore, it is necessary to find a rapid prototyping process for preparing dense silicon nitride balls. Summary of the invention

[0005] The object of the present invention is to provide a process for preparing silicon nitride ceramic microspheres to solve at least one of the problems raised in the above background technology.

[0006] In order to solve the above technical problems, the specific technical solutions of the present invention are as follows:

[0007] In some embodiments of the present application, a process for preparing silicon nitride ceramic microspheres is provided, comprising:

[0008] Step 1, preparation of silicon nitride powder, using silane and ammonia as raw materials, synthesizing ultrafine silicon nitride powder in a fluidized bed reactor through gas phase chemical reaction, and screening and grading the silicon nitride powder to ensure uniform particle size;

[0009] Step 2, preparing raw materials for silicon nitride ceramic microspheres, preparing silicon nitride powder, carbon fiber, MgO powder, and Y2O3-Al2O3 powder;

[0010] Step 3, mixing and molding the raw materials, mixing the prepared silicon nitride powder, carbon fiber, MgO powder, and Y2O3-Al2O3 powder, placing them into a spherical mold for pressure molding, and obtaining a silicon nitride ceramic microsphere embryo;

[0011] Step 4: Drying: Place the formed silicon nitride ceramic microspheres in an oven for heating to quickly evaporate the water in the silicon nitride ceramic microspheres for the next step;

[0012] Step 5: sintering, subjecting the dried silicon nitride ceramic microspheres to high temperature and pressure treatment to form a dense structure; first, placing the silicon nitride ceramic microsphere embryo into a furnace body, and preliminarily sintering the silicon nitride ceramic microspheres under high temperature and high pressure conditions, and cooling the silicon nitride ceramic microspheres to room temperature after the preliminarily sintering is completed; placing the silicon nitride ceramic microsphere embryo into the furnace body again, raising the temperature, and subjecting the silicon nitride ceramic microspheres to secondary sintering by discharge plasma under high temperature conditions, and cooling the silicon nitride ceramic microspheres to room temperature after the secondary sintering is completed; finally, subjecting the silicon nitride ceramic microspheres to microwave sintering under high temperature conditions, and obtaining silicon nitride ceramic microspheres after sintering;

[0013] Step six, processing, cutting, drilling and polishing the formed and sintered silicon nitride ceramic microspheres to obtain silicon nitride ceramic microspheres of desired shape and size.

[0014] Preferably, in the preferred embodiment of the above process for preparing silicon nitride ceramic microspheres, the reaction temperature in the fluidized bed reactor in step 1 is 600-850°C.

[0015] Preferably, in the preferred embodiment of the above-mentioned process for preparing silicon nitride ceramic microspheres, the flow rate of the raw gas through the fluidized bed reactor in the step 1 is 20-40 cm / s.

[0016] Preferably, in the preferred embodiment of the above-mentioned process for preparing silicon nitride ceramic microspheres, the particle size of the silicon nitride powder is less than 1 μm, which is more conducive to the subsequent work.

[0017] Preferably, in the preferred embodiment of the above-mentioned process for preparing silicon nitride ceramic microspheres, the weight proportions of the silicon nitride powder, carbon fiber, MgO powder, and Y2O3-Al2O3 powder are as follows:

[0018] Silicon nitride powder 70-80,

[0019] Carbon fiber 5-20,

[0020] MgO powder 5-10,

[0021] Y2O3-Al2O3 powder 5-10.

[0022] Preferably, in the preferred embodiment of the above process for preparing silicon nitride ceramic microspheres, the drying temperature in step 4 is 50-60°C.

[0023] Preferably, in the preferred embodiment of the above-mentioned process for preparing silicon nitride ceramic microspheres, in the step five, the high temperature and high pressure conditions for the preliminary sintering are a temperature of 1400-1550°C and a pressure of 5-10MPa, a temperature of the secondary sintering is 1400-1600°C, and a temperature of the microwave sintering is 1500-1700°C.

[0024] Preferably, in the preferred embodiment of the above-mentioned process for preparing silicon nitride ceramic microspheres, the time for the initial sintering in step five is 2-3 hours, the time for the secondary sintering is 5-6 hours, and the time for the microwave sintering is 3-5 hours.

[0025] Preferably, in the preferred embodiment of the above-mentioned process for preparing silicon nitride ceramic microspheres, the processing method of step six is ​​mechanical processing, electric spark processing and laser processing.

[0026] Through the above technical scheme, it can be known that compared with the prior art, the beneficial effects of the present invention are: the silicon nitride of the present invention is made into silicon nitride powder through gas phase chemical reaction, and the powder particle size is less than 1μm, which is more conducive to the subsequent work. The finer the raw materials used before sintering, the better the sintering characteristics and the performance of the sintered ceramic balls are, and it is more conducive to forming a uniform and good organizational structure; high-temperature and high-pressure sintering, spark plasma sintering, and microwave sintering are used for three sintering to make high-density and stable silicon nitride ceramic microspheres. The spark plasma sintering has a fast heating rate and a low heating temperature. The high degree of heating and uniform heating can realize the rapid sintering of dense sintered bodies. Microwave sintering is carried out after spark plasma sintering. Microwaves directly interact with material particles (molecules, ions). The special band of microwaves is coupled with the basic microstructure of the material to generate heat. The dielectric loss of the material heats the material as a whole to the sintering temperature to achieve densification, which is beneficial to increase the densification speed. Through the effect of three different sintering on the structure of silicon nitride ceramic microspheres, the process of preparing dense silicon nitride ceramic microspheres through rapid prototyping can obtain high-density and high-strength silicon nitride ceramic microspheres. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0028] Figure 1 The present invention is a process flow chart for preparing silicon nitride ceramic microspheres; DETAILED DESCRIPTION

[0029] The specific implementation of the present invention is further described in detail below in conjunction with the accompanying drawings and examples. The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention.

[0030] In the description of the present application, it should be understood that the terms "center", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.

[0031] The terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, unless otherwise specified, "plurality" means two or more.

[0032] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0033] In order to better understand the purpose, structure and function of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings.

[0034] See also Figure 1 As shown, a process for preparing silicon nitride ceramic microspheres according to an embodiment of the present application is described, comprising:

[0035] Step 1, preparation of silicon nitride powder, using silane and ammonia as raw materials, synthesizing ultrafine silicon nitride powder in a fluidized bed reactor through gas phase chemical reaction, and screening and grading the silicon nitride powder to ensure uniform particle size;

[0036] Step 2, preparing raw materials for silicon nitride ceramic microspheres, preparing silicon nitride powder, carbon fiber, MgO powder, and Y2O3-Al2O3 powder;

[0037] Step 3, mixing and molding the raw materials, mixing the prepared silicon nitride powder, carbon fiber, MgO powder, and Y2O3-Al2O3 powder, placing them into a spherical mold for pressure molding, and obtaining a silicon nitride ceramic microsphere embryo;

[0038] Step 4: Drying: Place the formed silicon nitride ceramic microspheres in an oven for heating to quickly evaporate the water in the silicon nitride ceramic microspheres for the next step;

[0039] Step 5: sintering, subjecting the dried silicon nitride ceramic microspheres to high temperature and pressure treatment to form a dense structure; first, placing the silicon nitride ceramic microsphere embryo into a furnace body, and preliminarily sintering the silicon nitride ceramic microspheres under high temperature and high pressure conditions, and cooling the silicon nitride ceramic microspheres to room temperature after the preliminarily sintering is completed; placing the silicon nitride ceramic microsphere embryo into the furnace body again, raising the temperature, and subjecting the silicon nitride ceramic microspheres to secondary sintering by discharge plasma under high temperature conditions, and cooling the silicon nitride ceramic microspheres to room temperature after the secondary sintering is completed; finally, subjecting the silicon nitride ceramic microspheres to microwave sintering under high temperature conditions, and obtaining silicon nitride ceramic microspheres after sintering;

[0040] Step six, processing, cutting, drilling and polishing the formed and sintered silicon nitride ceramic microspheres to obtain silicon nitride ceramic microspheres of desired shape and size.

[0041] To further optimize the above technical solution, the reaction temperature in the fluidized bed reactor in step 1 is 600-850°C.

[0042] To further optimize the above technical solution, the flow rate of the raw gas through the fluidized bed reactor in step 1 is 20-40 cm / s.

[0043] In order to further optimize the above technical solution, the particle size of silicon nitride powder is less than 1 μm, which is more conducive to the subsequent work.

[0044] Specifically, by controlling the temperature of the reactor and the flow rate of the raw gas, the silicon nitride ceramic powder undergoes a gas phase chemical reaction, making the powder particle size less than 1μm, which is more conducive to subsequent work. The finer the raw materials used before sintering, the better the sintering characteristics and performance of the sintered ceramic balls, and the more conducive to forming a uniform and good organizational structure.

[0045] To further optimize the above technical solution, the weight proportions of silicon nitride powder, carbon fiber, MgO powder, and Y2O3-Al2O3 powder are as follows:

[0046] Silicon nitride powder 70-80,

[0047] Carbon fiber 5-20,

[0048] MgO powder 5-10,

[0049] Y2O3-Al2O3 powder 5-10.

[0050] To further optimize the above technical solution, the drying temperature in step 4 is 50-60°C.

[0051] Specifically, the silicon nitride ceramic microsphere embryo is quickly dried by a heating and drying method.

[0052] To further optimize the above technical solution, in step five, the high temperature and high pressure conditions for the initial sintering are 1400-1550°C and 5-10MPa, the temperature for the secondary sintering is 1400-1600°C, and the temperature for the microwave sintering is 1500-1700°C.

[0053] To further optimize the above technical solution, the time for the initial sintering in step five is 2-3 hours, the time for the secondary sintering is 5-6 hours, and the time for the microwave sintering is 3-5 hours.

[0054] It should be noted that high-temperature and high-pressure sintering, spark plasma sintering, and microwave sintering are used to form high-density and stable silicon nitride ceramic microspheres. The spark plasma sintering has a fast heating rate, high heating temperature, and uniform heating, which can achieve rapid sintering of dense sintered bodies. Microwave sintering is performed after spark plasma sintering. Microwaves directly interact with material particles (molecules, ions), and utilize the special waveband of microwaves to couple with the basic fine structure of the material to generate heat. The dielectric loss of the material causes the material to be heated to the sintering temperature as a whole to achieve densification, which is beneficial to increasing the densification speed. Through the effects of three different sinterings on the structure of silicon nitride ceramic microspheres, and through the process of preparing dense silicon nitride ceramic microspheres through rapid prototyping, high-density and high-strength silicon nitride ceramic microspheres are obtained.

[0055] In order to further optimize the above technical solution, the processing methods in step six are mechanical processing, electrical discharge processing and laser processing.

[0056] Embodiment 1

[0057] Step 1, preparation of silicon nitride powder, using silane and ammonia as raw gas, synthesizing ultrafine silicon nitride powder in a fluidized bed reactor through gas phase chemical reaction, the reaction temperature in the fluidized bed reactor is 600°C, the flow rate of the raw gas through the reactor is 20cm / s, the silicon nitride powder is subjected to a phase chemical reaction, and the silicon nitride powder generated after the reaction is screened and graded to ensure uniform particle size;

[0058] Step 2, preparing raw materials for silicon nitride ceramic microspheres, preparing silicon nitride powder, carbon fiber, MgO powder, and Y2O3-Al2O3 powder;

[0059] Step 3: Mix and shape the raw materials. Mix 70 parts of the prepared silicon nitride powder, 20 parts of carbon fiber, 5 parts of MgO powder, and 5 parts of Y2O3-Al2O3 powder, put them into a spherical mold for pressure molding, and obtain a silicon nitride ceramic microsphere embryo;

[0060] Step 4: Drying: Place the formed silicon nitride ceramic microspheres in an oven for heating to quickly evaporate the water in the silicon nitride ceramic microspheres for the next step;

[0061] Step 5: sintering, subjecting the dried silicon nitride ceramic microspheres to high temperature and pressure treatment to form a dense structure; first, placing the silicon nitride ceramic microsphere embryo into a furnace body, and preliminarily sintering the silicon nitride ceramic microspheres at a temperature of 1400° C. and a pressure of 5 MPa for 2 hours. After the preliminary sintering is completed, the silicon nitride ceramic microspheres are cooled to room temperature; placing the silicon nitride ceramic microsphere embryo into the furnace body again, raising the temperature, and performing secondary sintering of the silicon nitride ceramic microspheres at a temperature of 1400° C. by using discharge plasma for 5 hours. After the secondary sintering is completed, the silicon nitride ceramic microspheres are cooled to room temperature; finally, the silicon nitride ceramic microspheres are sintered at a temperature of 1500° C. by using microwave sintering for 3 hours. After the sintering is completed, silicon nitride ceramic microspheres are obtained;

[0062] Step six, processing, cutting, drilling and polishing the formed and sintered silicon nitride ceramic microspheres to obtain silicon nitride ceramic microspheres of desired shape and size.

[0063] The prepared silicon nitride ceramic microspheres have a density of 99.3%, a hardness of 41 GPa at room temperature, a strength of 850 MPa at room temperature, a hardness of 39 GPa at high temperature, and a strength of 850 MPa.

[0064] Embodiment 2

[0065] Step 1, preparation of silicon nitride powder, using silane and ammonia as raw gas, synthesizing ultrafine silicon nitride powder in a fluidized bed reactor through gas phase chemical reaction, the reaction temperature in the fluidized bed reactor is 720°C, the flow rate of the raw gas through the reactor is 30 cm / s, the silicon nitride powder is subjected to a phase chemical reaction, and the silicon nitride powder generated after the reaction is screened and graded to ensure uniform particle size;

[0066] Step 2, preparing raw materials for silicon nitride ceramic microspheres, preparing silicon nitride powder, carbon fiber, MgO powder, and Y2O3-Al2O3 powder;

[0067] Step 3, mixing and molding the raw materials: 75 parts of the prepared silicon nitride powder, 5 parts of carbon fiber, 10 parts of MgO powder, and 10 parts of Y2O3-Al2O3 powder are mixed, and put into a spherical mold for pressure molding to obtain a silicon nitride ceramic microsphere embryo;

[0068] Step 4: Drying: Place the formed silicon nitride ceramic microspheres in an oven for heating to quickly evaporate the water in the silicon nitride ceramic microspheres for the next step;

[0069] Step 5: sintering, subjecting the dried silicon nitride ceramic microspheres to high temperature and pressure treatment to form a dense structure; first, placing the silicon nitride ceramic microsphere embryo into a furnace body, and performing preliminary sintering on the silicon nitride ceramic microspheres at a temperature of 1500° C. and a pressure of 8 MPa for 2.5 hours. After the preliminary sintering is completed, the silicon nitride ceramic microspheres are cooled to room temperature; placing the silicon nitride ceramic microsphere embryo into the furnace body again, raising the temperature, and performing secondary sintering on the silicon nitride ceramic microspheres at a temperature of 1500° C. by using discharge plasma for 5.5 hours. After the secondary sintering is completed, the silicon nitride ceramic microspheres are cooled to room temperature; finally, the silicon nitride ceramic microspheres are sintered by microwave sintering at a temperature of 1600° C. for 4 hours. After the sintering is completed, silicon nitride ceramic microspheres are obtained;

[0070] Step six, processing, cutting, drilling and polishing the formed and sintered silicon nitride ceramic microspheres to obtain silicon nitride ceramic microspheres of desired shape and size.

[0071] The prepared silicon nitride ceramic microspheres have a density of 99.5%, a hardness of 43 GPa at room temperature, a strength of 900 MPa at room temperature, a hardness of 41 GPa at high temperature, and a strength of 870 MPa.

[0072] Embodiment 3

[0073] Step 1, preparation of silicon nitride powder, using silane and ammonia as raw gas, synthesizing ultrafine silicon nitride powder in a fluidized bed reactor through gas phase chemical reaction, the reaction temperature in the fluidized bed reactor is 850°C, the flow rate of the raw gas through the reactor is 40cm / s, the silicon nitride powder is subjected to a phase chemical reaction, and the silicon nitride powder generated after the reaction is screened and graded to ensure uniform particle size;

[0074] Step 2, preparing raw materials for silicon nitride ceramic microspheres, preparing silicon nitride powder, carbon fiber, MgO powder, and Y2O3-Al2O3 powder;

[0075] Step 3, mixing and molding the raw materials, mixing 80 parts of the prepared silicon nitride powder, 6 parts of carbon fiber, 7 parts of MgO powder, and 7 parts of Y2O3-Al2O3 powder, putting them into a spherical mold for pressure molding, and obtaining a silicon nitride ceramic microsphere embryo;

[0076] Step 4: Drying: Place the formed silicon nitride ceramic microspheres in an oven for heating to quickly evaporate the water in the silicon nitride ceramic microspheres for the next step;

[0077] Step 5, sintering, subjecting the dried silicon nitride ceramic microspheres to high temperature and pressure treatment to form a dense structure; first, placing the silicon nitride ceramic microsphere embryo into a furnace body, and preliminarily sintering the silicon nitride ceramic microspheres at a temperature of 1550° C. and a pressure of 10 MPa for 3 hours. After the preliminary sintering is completed, the silicon nitride ceramic microspheres are cooled to room temperature; the silicon nitride ceramic microsphere embryo is placed into the furnace body again, the temperature is increased, and the silicon nitride ceramic microspheres are secondary sintered by discharge plasma at a temperature of 1600° C. for 6 hours. After the secondary sintering is completed, the silicon nitride ceramic microspheres are cooled to room temperature; finally, the silicon nitride ceramic microspheres are sintered by microwave sintering at a temperature of 1700° C. for 5 hours. After the sintering is completed, the silicon nitride ceramic microspheres are obtained;

[0078] Step six, processing, cutting, drilling and polishing the formed and sintered silicon nitride ceramic microspheres to obtain silicon nitride ceramic microspheres of desired shape and size.

[0079] The prepared silicon nitride ceramic microspheres have a density of 99.8%, a hardness of 45 GPa at room temperature, a strength of 1000 MPa at room temperature, a hardness of 44 GPa at high temperature, and a strength of 890 MPa.

[0080] Comparative Example 1

[0081] Step 1: Prepare raw materials for silicon nitride ceramic microspheres, including silicon nitride powder, carbon fiber, MgO powder, and Y2O3-Al2O3 powder;

[0082] Step 2: Mixing and molding the raw materials: 75 parts of the prepared silicon nitride powder, 5 parts of carbon fiber, 10 parts of MgO powder, and 10 parts of Y2O3-Al2O3 powder are mixed, and put into a spherical mold for pressure molding to obtain a silicon nitride ceramic microsphere embryo;

[0083] Step 3: Drying: Place the formed silicon nitride ceramic microspheres in an oven for heating to quickly evaporate the water in the silicon nitride ceramic microspheres for the next step;

[0084] Step 4: sintering: subjecting the dried silicon nitride ceramic microspheres to high temperature and pressure treatment to form a dense structure; placing the silicon nitride ceramic microsphere embryos into a furnace; sintering the silicon nitride ceramic microspheres at a temperature of 1500° C. and a pressure of 8 MPa; the sintering time is 9 hours; and after sintering, silicon nitride ceramic microspheres are obtained;

[0085] Step five: processing, cutting, drilling and polishing the formed and sintered silicon nitride ceramic microspheres to obtain silicon nitride ceramic microspheres of desired shape and size.

[0086] The prepared silicon nitride ceramic microspheres have a density of 95%, a hardness of 33 GPa at room temperature, a strength of 650 MPa at room temperature, a hardness of 30 GPa at high temperature, and a strength of 610 MPa.

[0087] Comparative Example 2

[0088] Step 1: Prepare raw materials for silicon nitride ceramic microspheres, including silicon nitride powder, carbon fiber, MgO powder, and Y2O3-Al2O3 powder;

[0089] Step 2: Mixing and molding the raw materials: 75 parts of the prepared silicon nitride powder, 5 parts of carbon fiber, 10 parts of MgO powder, and 10 parts of Y2O3-Al2O3 powder are mixed, and put into a spherical mold for pressure molding to obtain a silicon nitride ceramic microsphere embryo;

[0090] Step 3: Drying: Place the formed silicon nitride ceramic microspheres in an oven for heating to quickly evaporate the water in the silicon nitride ceramic microspheres for the next step;

[0091] Step 4: sintering, subjecting the dried silicon nitride ceramic microspheres to high temperature and pressure treatment to form a dense structure; first, placing the silicon nitride ceramic microsphere embryo into a furnace body, and preliminarily sintering the silicon nitride ceramic microspheres at a temperature of 1500° C. and a pressure of 8 MPa for 4 hours. After the preliminary sintering is completed, the silicon nitride ceramic microspheres are cooled to room temperature; the silicon nitride ceramic microsphere embryo is placed into the furnace body again, the temperature is increased, and the silicon nitride ceramic microspheres are secondary sintered by discharge plasma at a temperature of 1500° C. for 6 hours. After the sintering is completed, the silicon nitride ceramic microspheres are obtained;

[0092] Step five: processing, cutting, drilling and polishing the formed and sintered silicon nitride ceramic microspheres to obtain silicon nitride ceramic microspheres of desired shape and size.

[0093] The prepared silicon nitride ceramic microspheres have a density of 96%, a hardness of 37 GPa at room temperature, a strength of 800 MPa at room temperature, a hardness of 32 GPa at high temperature, and a strength of 770 MPa.

[0094] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.

[0095] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A process for preparing silicon nitride ceramic microspheres, characterized in that: include: Step 1, preparation of silicon nitride powder, using silane and ammonia as raw materials, synthesizing ultrafine silicon nitride powder in a fluidized bed reactor through gas phase chemical reaction, and screening and grading the silicon nitride powder to ensure uniform particle size; Step 2, preparing raw materials for silicon nitride ceramic microspheres, including silicon nitride powder, carbon fiber, MgO powder, and Y2O3-Al2O3 powder; Step 3: Mixing and molding the raw materials: mixing the prepared silicon nitride powder, carbon fiber, MgO powder, and Y2O3-Al2O3 powder, and putting them into a spherical mold for pressure molding to obtain a silicon nitride ceramic microsphere green body; Step 4: Drying: Place the formed silicon nitride ceramic microspheres in an oven for heating to evaporate the water in the silicon nitride ceramic microspheres quickly for the next step; Step 5: sintering, subjecting the dried silicon nitride ceramic microspheres to high temperature and pressure treatment to form a dense structure; first, placing the silicon nitride ceramic microsphere green body into a furnace body, and preliminarily sintering the silicon nitride ceramic microspheres under high temperature and high pressure conditions, and cooling the silicon nitride ceramic microspheres to room temperature after the preliminarily sintering is completed; placing the silicon nitride ceramic microsphere green body into the furnace body again, raising the temperature, and subjecting the silicon nitride ceramic microspheres to secondary sintering by discharge plasma under high temperature conditions, and cooling the silicon nitride ceramic microspheres to room temperature after the secondary sintering is completed; finally, subjecting the silicon nitride ceramic microspheres to microwave sintering under high temperature conditions, and obtaining silicon nitride ceramic microspheres after sintering; Step six, processing, cutting, drilling, and polishing the formed and sintered silicon nitride ceramic microspheres to obtain silicon nitride ceramic microspheres of desired shape and size; The weight proportions of the silicon nitride powder, carbon fiber, MgO powder, and Y2O3-Al2O3 powder are as follows: Silicon nitride powder 70-80, Carbon fiber 5-20, MgO powder 5-10, Y2O3-Al2O3 powder 5-10; In the step 5, the high temperature and high pressure conditions for the primary sintering are 1400-1550°C and 5-10MPa, the temperature for the secondary sintering is 1400-1600°C, and the temperature for the microwave sintering is 1500-1700°C; In the step 5, the time for the primary sintering is 2-3 hours, the time for the secondary sintering is 5-6 hours, and the time for the microwave sintering is 3-5 hours.

2. A process for preparing silicon nitride ceramic microspheres according to claim 1, characterized in that: In the step 1, the reaction temperature in the fluidized bed reactor is 600-850°C.

3. A process for preparing silicon nitride ceramic microspheres according to claim 1, characterized in that: In the step 1, the flow rate of the raw gas through the fluidized bed reactor is 20-40 cm / s.

4. A process for preparing silicon nitride ceramic microspheres according to claim 1, characterized in that: The silicon nitride powder has a particle size of less than 1 μm, which is more conducive to subsequent work.

5. A process for preparing silicon nitride ceramic microspheres according to claim 1, characterized in that: The drying temperature in step 4 is 50-60°C.

Citation Information

Patent Citations

  • Preparation method of silicon nitride-based conductive ceramic and molding method of silicon nitride-based conductive ceramic cutting tool

    CN104609865A

  • Single-phase silicon nitride ceramic material and microwave sintering preparation method thereof

    CN107963891A

  • Compact high-hardness high-strength silicon nitride ceramic ball as well as preparation method and application thereof

    CN113461426A

  • High-toughness silicon nitride ceramic material and preparation method thereof

    CN115536403A

  • High-hardness and high-toughness silicon nitride bearing ball as well as preparation method and application thereof

    CN115636674A