A fluorinated ionomer with high oxygen permeability and moisture retention, its preparation method and application
By grafting inorganic anionic clusters onto the side chains of perfluorosulfonic acid resin, fluorinated ionomers with high oxygen permeability and moisture retention were prepared, solving the problem of poor oxygen permeability in fuel cells and improving the mass transfer and kinetic performance of fuel cells.
Patent Information
- Application Number
- CN202311657375.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-04
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-12-04
AI Technical Summary
In existing proton exchange membrane fuel cells, poor oxygen permeability leads to local transport resistance, which is dominant, and sulfonic acid group adsorption occupies catalytic sites, reducing oxygen permeability and fuel cell performance.
By grafting inorganic anionic clusters onto the side chains of perfluorosulfonyl resin through a substitution reaction, fluorinated ionomers with high oxygen permeability and moisture retention are prepared, improving the interface between the catalyst and the ionomer and reducing local transport impedance.
It improves oxygen permeability, releases more Pt catalytic active sites, and enhances the kinetic and mass transfer performance of fuel cells, especially exhibiting superior battery output performance under low humidity conditions.
Smart Images

Figure CN117843850B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of new energy technology, specifically to a fluorinated ionomer with high oxygen permeability and moisture retention, its preparation method, and its application. Background Technology
[0002] Proton exchange membrane fuel cells (PEMFCs) are considered one of the most promising automotive power systems due to their high energy conversion efficiency, zero pollution, and short refueling time. However, the high cost limits the large-scale commercial application of PEMFCs. The cost of the precious metal Pt catalyst accounts for approximately 40% of the total stack cost, and reducing the Pt loading is the most effective way to reduce fuel cell costs. When the Pt loading is reduced, the mass transfer polarization caused by oxygen permeation resistance in the cathode catalyst layer accounts for more than 50% of the total polarization loss. Oxygen diffusion in the catalyst layer occurs in two processes: first, oxygen diffuses through the pores between secondary catalyst aggregates via Fick diffusion; second, oxygen diffuses through the ionomer film to the catalyst surface and undergoes an oxygen reduction reaction. The oxygen transport resistance in this process is called the local transport resistance (R0). local Because the catalyst layer is thin at low Pt loadings, the resistance to Fick diffusion within the catalyst layer can be ignored. This means that the oxygen transport resistance within the catalyst layer is R. local It plays a dominant role. Currently, reducing R... local There are two main approaches: First, introducing cyclic molecules into the main chain structure of perfluorosulfonic acid ionomers. This can break the crystallinity of the polytetrafluoroethylene (PTFE) main chain, allowing the polymer to gain a larger free volume and providing favorable conditions for oxygen transport. Second, improving the interface between the catalyst and the ionomer. It is well known that sulfonic acid groups on the side chains of perfluorosulfonic acid resins specifically adsorb onto the surface of phosphoric acid (Pt). This not only occupies catalytic sites on Pt and reduces the oxygen reduction kinetics of the catalyst, but also causes the ionomer main chain to aggregate, forming a physical barrier layer on the Pt surface and reducing oxygen permeability. Therefore, developing ionomers with high oxygen permeability is of great significance for improving the mass transfer performance of PEMFCs. Summary of the Invention
[0003] One of the objectives of this invention is to provide a method for preparing a fluorinated ionomer with high oxygen permeability and moisture retention. This method involves grafting inorganic anionic clusters onto the side chains of a perfluorosulfonyl resin via a substitution reaction, followed by protonation of the ionomer, thus successfully preparing a fluorinated ionomer with high oxygen permeability and moisture retention.
[0004] The second objective of this invention is to provide a fluorinated ionomer with high oxygen permeability and moisture retention, which has high oxygen permeability, reduces the local transport impedance of fuel cells, and improves mass transfer polarization under high current density.
[0005] The third objective of this invention is to provide an application of a fluorinated ionomer with high oxygen permeability and moisture retention.
[0006] One of the solutions adopted to achieve the objective of this invention is: a method for preparing a fluorinated ionomer with high oxygen permeability and moisture retention, comprising the following steps:
[0007] 1) Prepare precursor materials of amino-modified anionic clusters by reacting anionic clusters with tris(hydroxymethyl)aminomethane under solvent conditions;
[0008] 2) The precursor material of the amino-modified anionic clusters obtained in step 1) is subjected to cation exchange to obtain counterionic anionic clusters;
[0009] 3) The counterionic anionic clusters obtained in step 2) are subjected to a substitution reaction with perfluorosulfonyl fluoride resin under the action of an acid-binding agent. After the reaction is completed, the reaction solution is concentrated and the polymer is precipitated in the solvent to obtain the counterionic resin.
[0010] 4) Protonate the counterion resin obtained in step 3) to obtain the high oxygen permeability and moisture-retaining fluorinated ionomer.
[0011] Preferably, in step 1), the molar ratio of the anionic cluster to tris(hydroxymethyl)aminomethane is 1:1 to 3; the amino-modified anionic cluster is [N(C4H9)4]3[MMo6O 18 {(OCH2)3CNH2}2], [N(C4H9)4]3[NH2C(CH2O)3MMo6O 18 [(OH)3]、[N(C4H9)4]2[V6O 13 At least one of {(OCH2)3CNH2}2], wherein M is at least one of Mn, Cr, Fe, Al, Co, Ni, and Ga.
[0012] Preferably, in step 1), the solvent is at least one of water, acetonitrile, ethanol, and methanol.
[0013] Preferably, in step 2), the counterion includes Li + Na + K + Cs + NH4 + and at least one of organic ammonium salt ions.
[0014] The salts used for cation exchange are generally nitrates or perchlorates of the above counterions.
[0015] Preferably, in step 3), the perfluorosulfonyl fluoride resin and the counterionic anionic cluster are in a molar ratio of 1:1.2 to 3.
[0016] Preferably, in step 3), the acid-binding agent includes at least one of triethylamine, potassium carbonate, cesium carbonate, pyridine, N,N-diisopropylethylamine, and 4-dimethylaminopyridine; the perfluorosulfonyl fluoride resin is at least one of Nafion R-1100, 3M PFSO2F, and Aquivion PFSO2F; and the molar ratio of the acid-binding agent to the perfluorosulfonyl fluoride resin is 3 to 4:1.
[0017] Preferably, in step 3), the solvent is at least one of methanol, ethanol, and water.
[0018] Preferably, in step 4), protonation is performed using an inorganic acid, wherein the inorganic acid is at least one of hydrochloric acid, sulfuric acid, phosphoric acid, nitric acid, and perchloric acid.
[0019] The second objective of this invention is achieved by preparing a fluorinated ionomer with high oxygen permeability and moisture retention using the aforementioned preparation method.
[0020] The solution adopted to achieve the third objective of this invention is: the application of a fluorinated ionomer with high oxygen permeability and moisture retention, wherein the fluorinated ionomer with high oxygen permeability and moisture retention is applied to the cathode catalyst layer of a proton exchange membrane fuel cell.
[0021] The present invention has the following advantages and beneficial effects:
[0022] 1) The preparation method of the present invention does not require an additional catalyst. The ionomer is simply obtained through a substitution reaction. The anionic clusters are readily soluble in water, and the post-processing is simple and convenient.
[0023] 2) The preparation method of the present invention is simple, low in cost, and can be mass-produced, making it suitable for industrial production.
[0024] 3) The ionomer prepared in this invention has higher oxygen permeability than the commonly used perfluorosulfonic acid resin Nafion, thus improving the mass transfer polarization of proton exchange membrane fuel cells. Simultaneously, due to the charge delocalization effect of the anionic clusters, their specific adsorption on the Pt surface is weakened, thereby releasing more oxygen reduction active sites of Pt and further improving the kinetic performance of the fuel cell.
[0025] 4) The anionic cluster molecules selected in this invention have very strong hydrophilicity, giving the membrane electrode excellent moisture retention, enabling the fuel cell to operate stably under low humidity conditions. Simultaneously, the high charge delocalization effect also facilitates proton dissociation.
[0026] 5) The ionomer prepared by this invention has high oxygen permeability, which reduces the local transport impedance of fuel cells and improves mass transfer polarization under high current density.
[0027] 6) The ionomer prepared by this invention exhibits an amazing peak power density in proton exchange membrane fuel cells, which greatly improves the mass transfer performance, especially under low humidity conditions, and has better battery output performance. Attached Figure Description
[0028] Figure 1 The bar chart shows the local oxygen transport impedance values for Example 1 and Comparative Example 1.
[0029] Figure 2 The graphs show the polarization curves and power density curves of Example 1 and Comparative Example 1 at 100% RH.
[0030] Figure 3 The graphs show the polarization curves and power density curves of Example 1 and Comparative Example 1 at 70% RH.
[0031] Figure 4 The graphs show the polarization curves and power density curves of Example 1 and Comparative Example 1 at 50% RH. Detailed Implementation
[0032] To better understand the present invention, the following embodiments are further illustrations of the present invention, but the content of the present invention is not limited to the following embodiments.
[0033] Example 1
[0034] 1) Na3[MnMo6O 18 Synthesis of {(OCH2)3CNH2}2] anionic clusters
[0035] 8g of [N(C4H9)4]4[Mo8O 26 A mixture of 1.49 g of Mn(CH3COO)3·2H2O and 1.56 g of (HOCH2)3CNH2 in 150 mL of acetonitrile was refluxed for 16 h. The orange solution was cooled to room temperature and filtered to remove very fine black solids. The filtrate was then poured into diethyl ether to give a pink precipitate, which was separated by filtration, washed with a small amount of acetonitrile and diethyl ether, and then dried under vacuum. The obtained product was [N(C4H9)4]3[MnMo6O]3. 18 [{(OCH2)3CNH2}2] was dissolved in 50 ml of acetonitrile. A 0.25 mol / L NaClO4 acetonitrile solution was added while stirring, and stirring continued for 30 min, resulting in a pink precipitate. The precipitate was washed several times with acetonitrile to obtain Na3[MnMo6O] 18 {(OCH2)3CNH2}2] anion cluster.
[0036] 2) Preparation of PFSN-MnMo6-D ionomers
[0037] Nafion R-1100 and Na3[MnMo6O] were mixed in a molar ratio of 2:1. 18 [{(OCH2)3CNH2}2] was dissolved in 40 ml of dry DMF, and then 1.6 mol of triethylamine was added. The mixture was refluxed at 80 °C for 3 days. At the end of the reaction, the reaction solution was concentrated, and the polymer was precipitated by dropwise addition to ethanol at room temperature. The solid polymer was collected by filtration, washed with deionized water, and dried under vacuum at 80 °C to obtain the ionomer Na. + Salt form. Finally, the ionomer was protonated in an acidic aqueous solution at 80°C, then filtered under vacuum, washed with a large amount of ultrapure water, and dried to obtain the final PFSN-MnMo6-D ionomer.
[0038] 3) Fabrication of membrane electrode (MEA)
[0039] Weigh the PFSN-MnMo6-D ionomer and commercial Pt / C catalyst according to a ionomer:catalyst mass ratio of 1:3.33. Wet the catalyst with a trace amount of water, then add an appropriate amount of isopropanol:water mixed solvent (4:1), and then add the weighed ionomer solution to prepare an ink with a mass concentration of 3 mg / ml. After ultrasonic dispersion at room temperature for 60 minutes, spray the uniformly dispersed ink onto both sides of the proton exchange membrane to obtain the CCM electrode. Assemble the CCM electrode and the commercial gas diffusion layer together to obtain the membrane electrode assembly.
[0040] 4) Testing of local oxygen transport resistance of PFSN-MnMo6-D ionomer in fuel cells
[0041] Assemble the membrane electrode assembly, flow field plate, and end plate from process 3) into a single fuel cell. At a cell temperature of 80°C, 100% RH, and an open-circuit voltage (OCV) of 0.15V, inject N2 / O2 (X) into the cathode at a flow rate of 600 mL / min. O2 A mixture of 1%, 2%, 3%, and 4% hydrogen gas was injected into the anode at a flow rate of 600 mL / min, and the oxygen transport impedance was determined using the linear sweep voltammetry (LSV) method with a flow-limited method.
[0042] 5) Performance testing of PFSN-MnMo6-D ionomer in fuel cells
[0043] The membrane electrode assembly, flow field plate, and end plate from process 3) are assembled into a single fuel cell. The fuel cell is tested at a cell temperature of 80°C, with pure oxygen at the cathode, pure hydrogen at the anode, and a gas flow rate of 600 mL / min for both, without external back pressure. Polarization curves and power density curves are measured under different humidity levels.
[0044] Example 2
[0045] 1) Na3[NH2C(CH2O)3MnMo6O 18 Synthesis of [OH)3]
[0046] 1.76g of (NH4)3[MnMo6O 24 [N(C4H9)4]3[NH2C(CH2O)3MMo6O] and 0.272 g of H2NC(CH2OH)3 were dissolved in 8 ml of deionized water and refluxed for 3 h. Then, 1.45 g of tetrabutylammonium bromide was added and stirred for 10 min, producing a large amount of precipitate. The precipitate was filtered, washed with deionized water and dried to obtain [N(C4H9)4]3[NH2C(CH2O)3MMo6O]3. 18 [OH)3] was dissolved in 20 ml of acetonitrile, and a 0.25 mol / L NaClO4 acetonitrile solution was added while stirring. Stirring was continued for 30 min, resulting in a pink precipitate. The precipitate was washed several times with acetonitrile to obtain Na3[NH2C(CH2O)3MnMo6O] 18 [OH)3] anionic cluster.
[0047] 2) Preparation of PFSN-MnMo6-M ionomers
[0048] Nafion R-1100 and Na3[NH2C(CH2O)3MnMo6O] were mixed in a molar ratio of 1:1.1. 18 [OH)3] was dissolved in 40 ml of dry DMF, and then 1.6 mol of triethylamine was added. The mixture was refluxed at 80 °C for 3 days. At the end of the reaction, the reaction solution was concentrated, and the polymer was precipitated by dropwise addition to ethanol at room temperature. The solid polymer was collected by filtration, washed with deionized water, and dried under vacuum at 80 °C to obtain the ionomer Na. + Salt form. Finally, the ionomer was protonated in an acidic aqueous solution at 80°C, then filtered under vacuum, washed with a large amount of ultrapure water, and dried to obtain the final PFSN-MnMo6-M ionomer.
[0049] 3) Fabrication of membrane electrode (MEA)
[0050] Weigh the PFSN-MnMo6-M ionomer and commercial Pt / C catalyst according to a ionomer:catalyst mass ratio of 1:3.33. Wet the catalyst with a trace amount of water, then add an appropriate amount of isopropanol:water mixed solvent (4:1), and then add the weighed ionomer solution to prepare an ink with a mass concentration of 3 mg / ml. After ultrasonic dispersion at room temperature for 60 minutes, spray the uniformly dispersed ink onto both sides of the proton exchange membrane to obtain the CCM electrode. Assemble the CCM electrode and the commercial gas diffusion layer together to obtain the membrane electrode assembly.
[0051] 4) Testing of local oxygen transport resistance of PFSN-MnMo6-M ionomer in fuel cells
[0052] Assemble the membrane electrode assembly, flow field plate, and end plate from process 3) into a single fuel cell. At a cell temperature of 80°C, 100% RH, and an open-circuit voltage (OCV) of 0.15V, inject N2 / O2 (X) into the cathode at a flow rate of 600 mL / min. O2 A mixture of 1%, 2%, 3%, and 4% hydrogen gas was injected into the anode at a flow rate of 600 mL / min, and the oxygen transport impedance was determined using the linear sweep voltammetry (LSV) method with a flow-limited method.
[0053] 5) Performance testing of PFSN-MnMo6-M ionomer in fuel cells
[0054] The membrane electrode assembly, flow field plate, and end plate from process 3) are assembled into a single fuel cell. The fuel cell is tested at a cell temperature of 80°C, with pure oxygen at the cathode, pure hydrogen at the anode, and a gas flow rate of 600 mL / min for both, without external back pressure. Polarization curves and power density curves are measured under different humidity levels.
[0055] Example 3
[0056] 1) Take 3.12g of [(n-C4H9)4N]3[H3V 10 O 28 [N(C4H9)4]2[V6O]2 was dissolved in 40 ml of N,N-dimethylacetamide. The mixture was stirred at 90 °C for 24 h. After the reaction was complete, the resulting solution was precipitated in diethyl ether, and 20 ml of acetonitrile was added to the precipitate. The insoluble matter was filtered off, and 10 ml of 6 mol / L HCl solution was added to the filtrate to form a precipitate. The precipitate was washed with water and acetonitrile and dried. The resulting solid was suspended in 10 ml of a mixed solvent of acetonitrile and N,N-dimethylformamide, and 3 ml of 1 mol / L tetrabutylammonium hydroxide was added to the solution to dissolve the solid completely. The solution was then precipitated in diethyl ether. 13The precipitate {(OCH2)3CNH2}2 was dissolved in 20 ml of acetonitrile. A 0.25 mol / L NaClO4 acetonitrile solution was added with stirring, and stirring continued for 30 min to obtain the precipitate. The precipitate was washed several times with acetonitrile to obtain Na2[V6O] 13 {(OCH2)3CNH2}2] anion cluster.
[0057] 2) Preparation of PFSN-V6-D ionomer
[0058] Nafion R-1100 and Na2[V6O] were mixed in a molar ratio of 2:1. 13 [{(OCH2)3CNH2}2] was dissolved in 40 mL of dry DMF, and then 1.6 mol of triethylamine was added. The mixture was refluxed at 80 °C for 3 days. At the end of the reaction, the reaction solution was concentrated, and the polymer was precipitated by dropwise addition to ethanol at room temperature. The solid polymer was collected by filtration, washed with deionized water, and dried under vacuum at 80 °C to obtain the ionomer Na. + Salt form. Finally, the ionomer was protonated in an acidic aqueous solution at 80°C, then filtered under vacuum, washed with a large amount of ultrapure water, and dried to obtain the final PFSN-V6-D ionomer.
[0059] 3) Fabrication of membrane electrodes
[0060] Weigh the PFSN-V6-D ionomer and commercial Pt / C catalyst according to a ionomer:catalyst mass ratio of 1:3.33. Wet the catalyst with a trace amount of water, then add an appropriate amount of isopropanol:water mixed solvent (4:1), and then add the weighed ionomer solution to prepare an ink with a mass concentration of 3 mg / ml. After ultrasonic dispersion at room temperature for 60 minutes, spray the uniformly dispersed ink onto both sides of the proton exchange membrane to obtain the CCM electrode. Assemble the CCM electrode and the commercial gas diffusion layer together to obtain the membrane electrode assembly.
[0061] 4) Testing of local oxygen transport resistance of PFSN-V6-D ionomer in fuel cells
[0062] Assemble the membrane electrode assembly, flow field plate, and end plate from process 3) into a single fuel cell. At a cell temperature of 80°C, 100% RH, and an open-circuit voltage (OCV) of 0.15V, inject N2 / O2 (X) into the cathode at a flow rate of 600 mL / min. O2 A mixture of 1%, 2%, 3%, and 4% hydrogen gas was injected into the anode at a flow rate of 600 mL / min, and the oxygen transport impedance was determined using the linear sweep voltammetry (LSV) method with a flow-limited method.
[0063] 5) Performance testing of PFSN-V6-D ionomer in fuel cells
[0064] The membrane electrode assembly, flow field plate, and end plate from process 3) are assembled into a single fuel cell. The fuel cell is tested at a cell temperature of 80°C, with pure oxygen at the cathode, pure hydrogen at the anode, and a gas flow rate of 600 mL / min for both, without external back pressure. Polarization curves and power density curves are measured under different humidity levels.
[0065] Comparative Example 1
[0066] 1) Fabrication of membrane electrodes using traditional Nafion ionomers
[0067] Weigh out the Nafion ionomer and commercial Pt / C catalyst according to a ionomer:catalyst mass ratio of 1:3.33. Wet the catalyst with a trace amount of water, then add an appropriate amount of isopropanol:water mixed solvent (4:1), and then add the weighed ionomer solution to prepare an ink with a mass concentration of 3 mg / ml. After ultrasonic dispersion at room temperature for 60 minutes, spray the uniformly dispersed ink onto both sides of the proton exchange membrane to obtain the CCM electrode. Assemble the CCM electrode and the commercial gas diffusion layer together to obtain the membrane electrode assembly.
[0068] 2) Testing of local oxygen transport resistance of Nafion ionomers in fuel cells
[0069] The membrane electrode assembly, flow field plate, and end plate from process 1) are assembled into a single fuel cell. At a cell temperature of 80°C, 100% RH, and an open-circuit voltage (OCV) of 0.15V, N2 / O2 (X) is injected into the cathode at a flow rate of 600 mL / min. O2 A mixture of 1%, 2%, 3%, and 4% hydrogen gas was injected into the anode at a flow rate of 600 mL / min, and the oxygen transport impedance was determined using the linear sweep voltammetry (LSV) method with a flow-limited method.
[0070] 3) Performance testing of Nafion ionomers in fuel cells
[0071] The membrane electrode assembly, flow field plate, and end plate from process 2) are assembled into a single fuel cell. The fuel cell is tested at a cell temperature of 80°C, with pure oxygen at the cathode, pure hydrogen at the anode, and a gas flow rate of 600 mL / min for both, without external back pressure. Polarization curves and power density curves are measured under different humidity levels.
[0072] Figure 1 The bar chart shows the local oxygen transport impedance values for Example 1 and Comparative Example 1. As can be seen from the figure, due to the good oxygen permeability of the PFSN-MnMo6-D ionomer, the local oxygen transport impedance value of the ionomer is 31.5 s / m, which is lower than that of the traditional commercial Nafion ionomer.
[0073] Figure 2The graphs show the polarization and power density curves of Example 1 and Comparative Example 1 at 100% RH. As can be seen from the graphs, when PFSN-MnMo6-D ionomer is used as a binder in the cathode catalyst layer of a fuel cell, under conditions of 100% RH, hydrogen at the anode, oxygen at the cathode, and no back pressure, the single cell exhibits an extremely high power density, with a peak power density of 1688 mW / cm³. 2 It is significantly higher than that of Nafion ionomers.
[0074] Figure 3 The graphs show the polarization curves and power density curves of Example 1 and Comparative Example 1 at 70% RH. As can be seen from the graphs, when the operating humidity of the fuel cell drops to 70% RH, the PFSN-MnMo6-D ionomer exhibits a superior peak power density compared to the Nagion ionomer, and the mass transfer polarization is significantly improved.
[0075] Figure 4 The graphs show the polarization curves and power density curves of Example 1 and Comparative Example 1 at 50% RH. As can be seen from the graphs, when the operating humidity of the fuel cell drops to 50% RH, the advantages of PFSN-MnMo6-D ionomer become more obvious. This is because the hydrophilicity of the anionic clusters improves the moisture retention of the membrane electrode, thus improving the battery performance of the fuel cell at low humidity.
[0076] The above description is merely a preferred embodiment of the present invention, and should not be construed as limiting the scope of the invention. It should be noted that those skilled in the art can make various improvements and modifications without departing from the principles of the present invention, and these improvements and modifications are also considered to be within the scope of protection of the present invention.
Claims
1. A method for preparing a fluorinated ionomer with high oxygen permeability and moisture retention, characterized in that, Includes the following steps: 1) A precursor material with an amino-modified anionic cluster was prepared by reacting anionic clusters with tris(hydroxymethyl)aminomethane under solvent conditions. The amino-modified anionic cluster was [N(C4H9)4]3[MMo6O 18 {(OCH2)3CNH2}2], [N(C4H9)4]3[NH2C(CH2O)3MMo6O 18 [(OH)3]、[N(C4H9)4]2[V6O 13 At least one of {(OCH2)3CNH2}2], wherein M is at least one of Mn, Cr, Fe, Al, Co, Ni, and Ga; 2) The precursor material of the amino-modified anionic clusters obtained in step 1) is subjected to cation exchange to obtain counterionic anionic clusters; 3) The counterionic anionic clusters obtained in step 2) are subjected to a substitution reaction with perfluorosulfonyl fluoride resin under the action of an acid-binding agent. After the reaction is completed, the reaction solution is concentrated and the polymer is precipitated in the solvent to obtain the counterionic resin. 4) Protonate the counterion resin obtained in step 3) to obtain the fluorinated ionomer with high oxygen permeability and moisture retention.
2. The method for preparing the fluorinated ionomer with high oxygen permeability and moisture retention according to claim 1, characterized in that: In step 1), the molar ratio of the anionic cluster to tris(hydroxymethyl)aminomethane is 1:1 to 3.
3. The method for preparing the fluorinated ionomer with high oxygen permeability and moisture retention according to claim 1, characterized in that: In step 1), the solvent is at least one of water, acetonitrile, ethanol, and methanol.
4. The method for preparing the fluorinated ionomer with high oxygen permeability and moisture retention according to claim 1, characterized in that: In step 2), the counterion includes Li + Na + K + Cs + NH4 + and at least one of organic ammonium salt ions.
5. The method for preparing the fluorinated ionomer with high oxygen permeability and moisture retention according to claim 1, characterized in that: In step 3), the perfluorosulfonyl fluoride resin and the counterionic anionic cluster are in a molar ratio of 1:1.2~3.
6. The method for preparing the fluorinated ionomer with high oxygen permeability and moisture retention according to claim 1, characterized in that: In step 3), the acid-binding agent includes at least one of triethylamine, potassium carbonate, cesium carbonate, pyridine, N,N-diisopropylethylamine, and 4-dimethylaminopyridine; the perfluorosulfonyl fluoride resin is at least one of Nafion R-1100, 3M PFSO2F, and Aquivion PFSO2F; and the molar ratio of the acid-binding agent to the perfluorosulfonyl fluoride resin is 3~4:
1.
7. The method for preparing the fluorinated ionomer with high oxygen permeability and moisture retention according to claim 1, characterized in that: In step 3), the solvent is at least one of methanol, ethanol and water.
8. The method for preparing the fluorinated ionomer with high oxygen permeability and moisture retention according to claim 1, characterized in that: In step 4), protonation is performed using an inorganic acid, which is at least one of hydrochloric acid, sulfuric acid, phosphoric acid, nitric acid, and perchloric acid.
9. A fluorinated ionomer with high oxygen permeability and moisture retention, characterized in that: It is prepared by any one of the preparation methods according to claims 1-8.
10. An application of the fluorinated ionomer with high oxygen permeability and moisture retention as described in claim 9, characterized in that: The fluorinated ionomer with high oxygen permeability and moisture retention is applied to the cathode catalyst layer of a proton exchange membrane fuel cell.
Citation Information
Patent Citations
Preparation method of multi-metal oxygen cluster hybrid polyelectrolyte semi-interpenetrating network membrane
CN114464856A
Polymer-based polyoxometallate composite proton exchange membrane material as well as preparation method and application thereof
CN116706176A