A polyethylene material with high-efficiency flame retardant performance and preparation method thereof
By rationally configuring inorganic flame retardants and synergists in polyethylene materials, the problem of degradation of performance when the flame retardant performance is improved in the prior art is solved, and high-efficiency flame retardant, good mechanical properties and corrosion resistance are achieved, which is suitable for industrial production .
Patent Information
- Application Number
- CN202311573128.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-23
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-11-23
AI Technical Summary
While improving flame retardant properties, existing polyethylene materials usually reduce their mechanical properties or cause environmental pollution problems, making it difficult to significantly improve flame retardant properties while maintaining other properties.
Use aluminum hydroxide, zinc borate, antimony oxide, zirconium oxide, tin oxide or molybdenum oxide as flame retardants, graphene, carbon nanotubes or montmorillonite as synergists, oxidized polyethylene wax, basalt fibers and titanate As other additives, by reasonably configuring these components, polyethylene materials with high efficiency flame retardant properties are prepared.
It realizes the efficient flame retardant properties of polyethylene materials, while maintaining good comprehensive mechanical properties, corrosion resistance and waterproof properties. It has a simple process and is suitable for industrial production.
Smart Images

Figure BDA0004566112330000151 
Figure BDA0004566112330000161 
Figure BDA0004566112330000171
Abstract
Description
Technical Field
[0001] The invention relates to the field of polyethylene materials, and in particular to a polyethylene material with high-efficiency flame retardant properties and a preparation method thereof. Background Art
[0002] Polyethylene is a common polymer material. It is widely used in packaging, building materials, power cables, automotive parts, etc. due to its excellent processing performance, electrical insulation, chemical stability and low cost. However, polyethylene is easy to burn in a fire and will produce toxic gases, which endangers human life and safety. Therefore, it is of great significance to improve the flame retardant properties of polyethylene.
[0003] In the past, people have developed a variety of flame retardants for polyethylene materials, such as inorganic fillers, halogen-containing flame retardants, phosphorus-containing flame retardants, etc. However, while these flame retardants improve the flame retardant properties, they often reduce the mechanical properties or other properties of polyethylene materials, or cause environmental pollution problems. Therefore, it is of great significance to develop a polyethylene material and a preparation method that can effectively improve the flame retardant properties of polyethylene materials without significantly reducing other properties. Summary of the invention
[0004] The object of the present invention is to provide a polyethylene material with high-efficiency flame retardant properties and a preparation method thereof, which aims to overcome the above-mentioned problems existing in the prior art.
[0005] The present invention solves the technical problem by adopting the following technical solutions.
[0006] The present invention provides a polyethylene material with high-efficiency flame retardant performance, which is made of a variety of raw materials, and the various raw materials include, by weight:
[0007] Polyethylene 90-110 parts;
[0008] Flame retardant 15-25 parts;
[0009] 10-20 parts of synergist; and
[0010] 4-19 parts of other additives;
[0011] Wherein, the flame retardant includes at least one of aluminum hydroxide, zinc borate, antimony oxide, zirconium oxide, tin oxide or molybdenum oxide;
[0012] The synergist includes at least one of graphene, carbon nanotubes or montmorillonite;
[0013] The other additives include oxidized polyethylene wax, basalt fiber and titanate.
[0014] Further, in a preferred embodiment of the present invention, the flame retardant includes the aluminum hydroxide, the zinc borate, the antimony oxide, the zirconium oxide, the tin oxide and the molybdenum oxide;
[0015] The synergist includes the graphene, the carbon nanotube and the montmorillonite.
[0016] Furthermore, in a preferred embodiment of the present invention, the mass ratio of the oxidized polyethylene wax, the basalt fiber and the titanate is 2:2:1.
[0017] Furthermore, in a preferred embodiment of the present invention, the plurality of raw materials are made of the following raw materials in parts by weight:
[0018] 95-105 parts of polyethylene;
[0019] 20-24 parts of the flame retardant;
[0020] 15-19 parts of the synergist; and
[0021] The other additives are 10-16 parts.
[0022] Further, in a preferred embodiment of the present invention, the weight portion of the flame retardant is 22 parts, and the flame retardant comprises, by weight:
[0023] 5 parts of the aluminum hydroxide;
[0024] 4 parts of the zinc borate;
[0025] 2 parts of the antimony oxide;
[0026] 2 parts of the zirconium oxide;
[0027] 3 parts of tin oxide; and
[0028] Described molybdenum oxide 6 parts.
[0029] Further, in a preferred embodiment of the present invention, the weight portion of the synergist is 18 parts, and the synergist comprises, by weight:
[0030] 5 parts of the graphene;
[0031] 6 parts of the carbon nanotubes; and
[0032] 7 parts of the montmorillonite.
[0033] Furthermore, in a preferred embodiment of the present invention, the weight proportion of the other additives in the plurality of raw materials is 19 parts.
[0034] Furthermore, in a preferred embodiment of the present invention, the other additives also include sodium tungstate, cerium nitrate and titanium dioxide;
[0035] The weight ratio of the oxidized polyethylene wax, the basalt fiber, the titanate, the sodium tungstate, the cerium nitrate and the titanium dioxide in the other additives is 4:4:2:5:1:3.
[0036] The present invention also provides a method for preparing a polyethylene material with high-efficiency flame retardant performance, which comprises the following steps:
[0037] In parts by weight, 15-25 parts of a flame retardant, 10-20 parts of a synergist and 4-19 parts of other additives are dried and mixed uniformly to obtain a first mixture; wherein the flame retardant is a mixture of one or more of aluminum hydroxide, zinc borate, antimony oxide, zirconium oxide, tin oxide or molybdenum oxide, the synergist is a mixture of one or more of graphene, carbon nanotubes or montmorillonite, and the other additives include oxidized polyethylene wax, basalt fiber and titanate;
[0038] Melt blending the first mixture with 90-110 parts of polyethylene to obtain a second mixture;
[0039] The second mixture is extruded into granules through an extrusion device, cooled and dried, and then screened to obtain the polyethylene material with high-efficiency flame retardant performance.
[0040] Furthermore, in a preferred embodiment of the present invention, in the process of obtaining the first mixture, the other additives also include sodium tungstate, cerium nitrate and titanium dioxide;
[0041] When the first mixture and the polyethylene are melt-blended, the melting temperature is 150-190° C. and the time is 20-35 min;
[0042] During the cooling and drying, the cooling rate is controlled at 9°C / hour.
[0043] The beneficial effects of a polyethylene material with high-efficiency flame retardant performance and a preparation method thereof according to an embodiment of the present invention are as follows: by reasonably configuring an inorganic flame retardant in polyethylene, the polyethylene material has high-efficiency flame retardant performance; by reasonably configuring a synergist in polyethylene, the polyethylene material has high-efficiency flame retardant performance while also having good comprehensive mechanical properties, corrosion resistance and waterproof properties; by reasonably configuring other additives in polyethylene, the various properties of the polyethylene material are further improved and strengthened, especially the mechanical strength and waterproof and anti-corrosion properties of the polyethylene material are significantly improved. Therefore, the polyethylene material provided by the embodiment of the present invention not only has high-efficiency flame retardant performance, but also has excellent other properties (such as comprehensive mechanical properties, waterproofness and corrosion resistance, etc.); in addition, the preparation method of the above-mentioned polyethylene material provided by the embodiment of the present invention has a simple process, low pollution, and can efficiently prepare the above-mentioned polyethylene material of high quality, which is suitable for industrial production. DETAILED DESCRIPTION
[0044] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0045] The polyethylene material with high-efficiency flame retardant performance and the preparation method thereof according to the embodiment of the present invention are described in detail below.
[0046] The embodiment of the present invention provides a polyethylene material with high-efficiency flame retardant performance, which is made of a variety of raw materials, which include, by weight: 90-110 parts of polyethylene, 15-25 parts of flame retardant, 10-20 parts of synergist and 4-19 parts of other additives. Preferably, in a preferred embodiment of the present invention, the multiple raw materials include, by weight: 95-105 parts of polyethylene, 20-24 parts of flame retardant, 15-19 parts of synergist and 10-16 parts of other additives.
[0047] Furthermore, the flame retardant may optionally include at least one of aluminum hydroxide, zinc borate, antimony oxide, zirconium oxide, tin oxide or molybdenum oxide, and preferably the flame retardant is aluminum hydroxide, zinc borate, antimony oxide, zirconium oxide, tin oxide and molybdenum oxide. It should be noted that the flame retardant provided in the embodiment of the present invention is preferably aluminum hydroxide, zinc borate, antimony oxide, zirconium oxide, tin oxide and molybdenum oxide because it can be configured in organic polyethylene to play a synergistic role in improving its flame retardancy. Secondly, it should be specifically stated that aluminum hydroxide, as one of the flame retardant components provided in the embodiment of the present invention, has the advantages of high flame retardant efficiency, small addition amount, wide application range, etc. At the same time, it can reduce the generation of toxic and harmful substances, has good environmental performance, and it is reasonably compounded with other components of the flame retardant in the above proportion, showing a flame retardant performance improvement of 1+1>2; in addition, zinc borate as an environmental The shape-preserving non-halogen flame retardant is non-toxic, low in water solubility, high in thermal stability, small in particle size, small in specific gravity, and good in dispersibility. It is compounded with antimony oxide, zirconium oxide, tin oxide, and molybdenum oxide, which not only greatly improves the flame retardancy of polyethylene materials, but also ensures that the comprehensive mechanical properties of polyethylene materials are not reduced. The reasonable proportion of antimony oxide, zirconium oxide, tin oxide, and molybdenum oxide not only improves the flame retardancy of polyethylene materials to a certain extent, but also balances the processability and strength of polyethylene materials, so that the polyethylene materials can still maintain the expected toughness and strength under the condition of good processability, so that the comprehensive performance of polyethylene materials reaches the best under balanced conditions. It should be emphasized that the polyethylene material provided in the embodiment of the present invention can reasonably configure inorganic flame retardants with the characteristics of environmental protection, low water solubility, high in thermal stability, small in particle size, small in specific gravity, and good in dispersibility in polyethylene in a certain proportion, so that the flame retardant can play a synergistic role in polyethylene to exert efficient flame retardant properties.Specifically, the flame retardants of the embodiment of the present invention are preferably configured as aluminum hydroxide, zinc borate, antimony oxide, zirconium oxide, tin oxide and molybdenum oxide, achieving a five-level flame retardant effect, wherein the first level of flame retardancy is that when the polyethylene material is first heated, aluminum hydroxide, zinc borate, antimony oxide and molybdenum oxide will decompose, absorb a large amount of heat, and reduce the fuel temperature, thereby playing the first level of basic flame retardant effect; the second level of flame retardancy is based on the first level of flame retardancy, and the flame retardant effect is mainly played by zirconium oxide in coordination, that is, zirconium oxide produces oxygen ions at high temperature, so that the flame that gradually begins to be generated is quickly extinguished, thereby playing a secondary flame retardant effect of dilution and isolation; the third level of flame retardancy is that at the same time as the secondary flame retardancy, antimony oxide will form a glassy coating layer and promote the carbonization of the polymer, while zirconium oxide will Provide lattice oxygen to promote the oxidation of carbon in the combustion product, thereby playing a purely chemical mechanism of flame retardancy; the fourth level of flame retardancy is that tin oxide and molybdenum oxide will generate crystal water under high temperature conditions with further increased temperature, thereby further absorbing heat, reducing the fuel temperature, and inhibiting the formation of molten droplets of combustion products; the fifth level of flame retardancy is both interspersed in the first four levels of flame retardancy and further extended and strengthened by the fourth level of flame retardancy. First, aluminum hydroxide, zinc borate, antimony oxide, zirconium oxide, tin oxide and molybdenum oxide work together to play a flame retardant function of cooling, oxygen ion dilution and covering. Secondly, when the crystal water is further vaporized into water vapor, the oxygen in the air can be further diluted, thereby delaying the thermal degradation rate of the polymer, inhibiting the combustion of the polymer, and promoting carbonization and inhibiting the formation of smoke as a whole. Therefore, the preferred formula of the above flame retardant compounded in the polyethylene material provided in this application complements each other and realizes the efficient flame retardant performance of the polyethylene material. In addition, since the flame retardant provided in the present application is mainly composed of inorganic metal oxides, it provides a relatively neat and orderly material organizational structure for the polyethylene material as a whole, and provides a good organizational structure adaptation basis for other substances (such as enhancers and other additives) to simultaneously exert other properties (such as excellent mechanical properties and waterproof and anti-corrosion properties, etc.), which is beneficial for the polyethylene material provided in the present application to maintain the overall improvement of various performances.
[0048] Further optionally, the synergist includes at least one of graphene, carbon nanotubes or montmorillonite, and preferably, the synergist includes the graphene, the carbon nanotubes and the montmorillonite. It should be noted that the reasonable configuration of graphene and montmorillonite further enhances the flame retardancy, processability and thermal stability of the polyethylene material on the basis of low cost, and the carbon nanotubes have excellent thermal conductivity and electrical conductivity, and are dispersed in the polyethylene material, and their large specific surface area further synergistically improves the flame retardancy and mechanical properties of the polyethylene material. Specifically, by preferably configuring graphene, carbon nanotubes and montmorillonite, carbon nanotubes with a large specific surface area can be easily attached to the surface of the graphene tissue. At the same time, montmorillonite and graphene form an intercalated structure in the tissue. Therefore, the mutually embedded + attached and filled layer network structure formed by the three not only improves the mechanical strength, processability and thermal stability from the structural level, but also forms a dense barrier layer on its surface during combustion, thereby blocking combustion and achieving a good flame retardant effect.
[0049] Further optionally, in some embodiments of the present invention, the other additives include oxidized polyethylene wax, basalt fiber and titanate. Preferably, the oxidized polyethylene wax, the basalt fiber and the titanate are in a mass ratio of 2:2:1. It should be noted that the reasonable configuration of other additives is mainly to enhance the water resistance and processability of the polyethylene material on the basis of synergistically improving the mechanical strength of the polyethylene material. It should also be emphasized that by limiting the mass ratio of oxidized polyethylene wax, basalt fiber and titanate, the oxidized polyethylene wax can be well attached to the basalt fiber and filled with titanate, and then can be nested with the organizational structure formed by the synergist, synergistically improving the water resistance and processability of the polyethylene material and the mechanical properties, so that the above-mentioned properties of the polyethylene material provided in this application can be balanced.
[0050] Further, in a preferred embodiment of the present invention, the weight of the flame retardant is 22 parts, and the flame retardant includes, by weight: 5 parts of aluminum hydroxide, 4 parts of zinc borate, 2 parts of antimony oxide, 2 parts of zirconium oxide, 3 parts of tin oxide, and 6 parts of molybdenum oxide. In addition, preferably, the weight of the synergist is 18 parts, and the synergist includes, by weight: 5 parts of graphene, 6 parts of carbon nanotubes, and 7 parts of montmorillonite.
[0051] Furthermore, in a preferred embodiment of the present invention, the weight proportion of the other additives in the multiple raw materials is 19 parts, and more preferably, the other additives also include sodium tungstate, cerium nitrate and titanium dioxide, and the weight proportion of the oxidized polyethylene wax, the basalt fiber, the titanate, the sodium tungstate, the cerium nitrate and the titanium dioxide in the other additives is 4:4:2:5:1:3. It should be noted that in the preferred scheme of the embodiment of the present invention, sodium tungstate and cerium nitrate are reasonably configured so that the polytungsten anions formed by tungstate ions can react with the cations of rare earth cerium to form a coordination chemical reaction, thereby forming a chelate or complex with a larger molecular weight. These chelates or complexes are dispersed in the polyethylene material in a certain proportion, and finally form a dense film in the polyethylene material, thereby hindering the occurrence of chemical or electrochemical reactions of the polyethylene material in a complex environment, and further improving the corrosion resistance of the polyethylene material. The configuration of titanium dioxide can adhere to the above-mentioned complex or / and the organizational structure of the polyethylene material through its physical properties (high melting point, strong adhesion and stable chemical properties), thereby cooperating with sodium tungstate and cerium nitrate to further improve the strength and corrosion resistance of the polyethylene material.
[0052] The embodiment of the present invention also provides a method for preparing a polyethylene material with high-efficiency flame retardant performance. The preparation process is simple, pollution-free, and the high-quality polyethylene material can be efficiently prepared. The method is suitable for industrial production, and specifically includes the following steps:
[0053] S1. Dry and mix 15-25 parts of flame retardant, 10-20 parts of synergist and 4-19 parts of other additives by weight to obtain a first mixture; wherein the flame retardant is a mixture of one or more of aluminum hydroxide, zinc borate, antimony oxide, zirconium oxide, tin oxide or molybdenum oxide, the synergist is a mixture of one or more of graphene, carbon nanotubes or montmorillonite, and the other additives include oxidized polyethylene wax, basalt fiber and titanate. It should be noted that in a preferred embodiment of the present invention, in the process of obtaining the first mixture, the other additives also include sodium tungstate, cerium nitrate and titanium dioxide.
[0054] S2. Melt-blending the first mixture with 90-110 parts of polyethylene to obtain a second mixture. It should be noted that when the first mixture is melt-blended with the polyethylene, the melting temperature is 150-190°C and the time is 20-35 minutes; it should be emphasized that the temperature and time during melt blending are reasonably limited because it is necessary to ensure the uniformity and sufficiency of the mixing of the components in the polyethylene material and the relative stability of the physical and chemical properties of the components in the polyethylene material. Too high or too low a temperature, too long or too short a time, are not conducive to the realization of the above two purposes.
[0055] S3, extruding the second mixture through an extrusion device for granulation, cooling and drying, and then screening to obtain the polyethylene material with efficient flame retardant properties. It should be noted that during the cooling and drying, the cooling rate is controlled at 9°C / hour; it should be emphasized that the reason why the cooling rate is precisely limited is that the applicant found in the research and development process that the cooling rate still has a certain influence on the structure and performance of the polyethylene material of the intended target of this application. By controlling the cooling rate at 9°C / hour, it is well ensured that the stress release of the polyethylene material during the cooling process is as complete as possible, and at the same time, it is prevented that the cooling rate is too slow to cause grain growth, so that the final polyethylene material has a relatively stable organizational structure, ensuring the high flame retardancy, good processability and comprehensive mechanical properties and waterproof and anti-corrosion properties of the polyethylene material provided in the embodiment of the present invention.
[0056] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0057] Example 1
[0058] This embodiment provides a polyethylene material with high-efficiency flame retardant performance, which is made of a variety of raw materials, which include, by weight: 100g polyethylene, 22g flame retardant, 18g synergist and 19g other additives. Specifically, the flame retardant is 5g aluminum hydroxide, 4g zinc borate, 2g antimony oxide, 2g zirconium oxide, 3g tin oxide and 6g molybdenum oxide, the synergist is 5g graphene, 6g carbon nanotubes and 7g montmorillonite, and the other additives are 4g oxidized polyethylene wax, 4g basalt fiber, 2g titanate, 5g sodium tungstate, 1g cerium nitrate and 3g titanium dioxide.
[0059] This embodiment also provides a method for preparing a polyethylene material with high-efficiency flame retardant properties, which comprises the following steps:
[0060] S1. Dry and mix the flame retardant, synergist and other additives of the above specific components and proportions in this embodiment in parts by weight to obtain a first mixture;
[0061] S2, melt-blending the first mixture with 100 g of polyethylene to obtain a second mixture; wherein the melting temperature is 150-190° C. and the melting time is 20-35 min;
[0062] S3, extruding the second mixture through a twin-screw extruder to granulate, cooling and drying through a blast drying oven, and then screening to obtain a polyethylene material with high efficiency flame retardant performance. It should be noted that the cooling rate during the cooling process is controlled at 9°C / hour.
[0063] Example 2
[0064] The polyethylene material with high-efficiency flame retardant performance and the preparation method thereof provided in this embodiment are substantially the same as those in Example 1, except that the raw materials in this embodiment include 95g polyethylene, 20g flame retardant, 15g synergist and 10g other additives. It should be noted that the corresponding specific components in the flame retardant, synergist and other additives are the same as those in Example 1, and the specific mass of each component can be adaptively adjusted according to the mass ratio of the components in Example 1. For example, the mass of aluminum hydroxide in the flame retardant in this embodiment is 5*20 / 22=4.55g, and the mass of other corresponding components is similar, and the subsequent related embodiments will not be given examples for further description.
[0065] Example 3
[0066] The polyethylene material with high-efficiency flame retardant performance and the preparation method thereof provided in this embodiment are substantially the same as those in Example 1, except that, in the raw materials of this embodiment, there are 105g polyethylene, 24g flame retardant, 19g synergist and 16g other additives. It should be noted that the corresponding specific components of the flame retardant, synergist and other additives are the same as those in Example 1, and the specific mass of each component can be adaptively adjusted according to the mass ratio of the components in Example 1.
[0067] Example 4
[0068] The polyethylene material with high-efficiency flame retardant performance and the preparation method thereof provided in this embodiment are substantially the same as those in Example 1, except that the raw materials in this embodiment include 90g polyethylene, 15g flame retardant, 10g synergist and 4g other additives. It should be noted that the corresponding specific components in the flame retardant, synergist and other additives are the same as those in Example 1, and the specific mass of each component can be adaptively adjusted according to the mass ratio of the components in Example 1.
[0069] Example 5
[0070] The polyethylene material with high-efficiency flame retardant performance and the preparation method thereof provided in this embodiment are substantially the same as those in Example 1, except that, in the raw materials of this embodiment, there are 110 g of polyethylene, 25 g of flame retardant, 20 g of synergist and 19 g of other additives. It should be noted that the corresponding specific components of the flame retardant, synergist and other additives are the same as those in Example 1, and the specific mass of each component can be adaptively adjusted according to the mass ratio of the components in Example 1.
[0071] Example 6
[0072] The polyethylene material with high-efficiency flame retardant performance and the preparation method thereof provided in this embodiment are substantially the same as those in Example 1, except that, among the raw materials in this embodiment, the flame retardant component is only zinc borate.
[0073] Example 7
[0074] The polyethylene material with high-efficiency flame retardant performance and the preparation method thereof provided in this embodiment are substantially the same as those in Example 1, except that, in the raw materials of this embodiment, the flame retardant component is only tin oxide.
[0075] Example 8
[0076] The polyethylene material with high-efficiency flame retardant properties and its preparation method provided in this embodiment are roughly the same as those in Example 1, except that among the raw materials in this embodiment, the flame retardant components are only antimony oxide and tin oxide, and the corresponding masses can be adaptively adjusted according to the mass ratio of the components in Example 1.
[0077] Example 9
[0078] The polyethylene material with high-efficiency flame retardant properties and its preparation method provided in this embodiment are roughly the same as those in Example 1, except that among the raw materials in this embodiment, the flame retardant components are only aluminum hydroxide and molybdenum oxide, and the corresponding masses can be adaptively adjusted according to the mass ratio of the components in Example 1.
[0079] Example 10
[0080] The polyethylene material with high-efficiency flame retardant properties and its preparation method provided in this embodiment are roughly the same as those in Example 1, except that among the raw materials in this embodiment, the flame retardant components are only aluminum hydroxide, zirconium oxide and molybdenum oxide, and the corresponding masses can be adaptively adjusted according to the mass ratio of the components in Example 1.
[0081] Embodiment 11
[0082] The polyethylene material with high-efficiency flame retardant properties and its preparation method provided in this embodiment are roughly the same as those in Example 1, except that among the raw materials in this embodiment, the flame retardant components are only zinc borate, antimony oxide and zirconium oxide, and the corresponding masses can be adaptively adjusted according to the mass ratio of the components in Example 1.
[0083] Example 12
[0084] The polyethylene material with high-efficiency flame retardant properties and its preparation method provided in this embodiment are roughly the same as those in Example 1, except that among the raw materials in this embodiment, the flame retardant components only include aluminum hydroxide, zinc borate, antimony oxide and zirconium oxide, and the corresponding masses can be adaptively adjusted according to the mass ratio of the components in Example 1.
[0085] Embodiment 13
[0086] The polyethylene material with high-efficiency flame retardant properties and its preparation method provided in this embodiment are roughly the same as those in Example 1, except that among the raw materials in this embodiment, the flame retardant components are only zinc borate, molybdenum oxide, antimony oxide and zirconium oxide, and the corresponding masses can be adaptively adjusted according to the mass ratio of the components in Example 1.
[0087] Embodiment 14
[0088] The polyethylene material with high-efficiency flame retardant properties and its preparation method provided in this embodiment are roughly the same as those in Example 1, except that, among the raw materials in this embodiment, the flame retardant components include five kinds of aluminum hydroxide, zinc borate, molybdenum oxide, tin oxide and zirconium oxide, and the corresponding masses can be adaptively adjusted according to the mass ratio of the components in Example 1.
[0089] Embodiment 15
[0090] The polyethylene material with high-efficiency flame retardant properties and its preparation method provided in this embodiment are roughly the same as those in Example 1, except that, in the raw materials of this embodiment, the flame retardant components include five kinds of aluminum hydroxide, zinc borate, molybdenum oxide, antimony oxide and zirconium oxide, and the corresponding masses can be adaptively adjusted according to the mass ratio of the components in Example 1.
[0091] Example 16
[0092] The polyethylene material with high-efficiency flame retardant properties and the preparation method thereof provided in this embodiment are substantially the same as those in Example 1, except that, among the raw materials in this embodiment, the synergist component is only graphene.
[0093] Embodiment 17
[0094] The polyethylene material with high-efficiency flame retardant performance and the preparation method thereof provided in this embodiment are substantially the same as those in Example 1, except that, among the raw materials in this embodiment, the synergist component is only carbon nanotubes.
[0095] Embodiment 18
[0096] The polyethylene material with high-efficiency flame retardant properties and its preparation method provided in this embodiment are substantially the same as those in Example 1, except that among the raw materials in this embodiment, the synergist components are only graphene and carbon nanotubes, and the corresponding masses can be adaptively adjusted according to the mass ratio of the components in Example 1.
[0097] Embodiment 19
[0098] The polyethylene material with high-efficiency flame retardant properties and its preparation method provided in this embodiment are substantially the same as those in Example 1, except that among the raw materials in this embodiment, the synergist components are only graphene and montmorillonite, and the corresponding masses can be adaptively adjusted according to the mass ratio of the components in Example 1.
[0099] Embodiment 20
[0100] The polyethylene material with high-efficiency flame retardant properties and its preparation method provided in this embodiment are roughly the same as those in Example 1, except that among the raw materials in this embodiment, the other additives only include oxidized polyethylene wax, basalt fiber and titanate, and the corresponding masses can be adaptively adjusted according to the mass ratio of the components in Example 1.
[0101] Comparative Example
[0102] A comparison sample was made of HDPE polyethylene commonly used in the market, and prepared to be compared with Examples 1-20 as test examples.
[0103] Test example
[0104] First, the above-mentioned Examples 1-20 and the comparative example were subjected to flame retardancy test and mechanical strength (including tensile strength, bending strength and impact strength, etc.) performance tests under the same conditions, and the test results are shown in Table 1. It should be noted that one of the methods for the flame retardancy test is a combustion method. Specifically, according to the same standard, Examples 1-20 and the comparative example were made into 21 standard samples, and then the 21 standard samples were placed in a combustion device, and their combustion conditions were observed after ignition, and parameters such as the combustion time and the state after combustion were recorded.
[0105] Table 1 Test results of flame retardant properties and mechanical properties
[0106]
[0107]
[0108]
[0109]
[0110] It can be seen from Table 1 that the polyethylene material samples of Examples 1-20 provided by the present invention in the test examples have high-efficiency flame retardant properties, and their burning rate relative to the samples of the comparative examples is only about one-third of that of the comparative examples. In other words, the flame retardant property of the polyethylene material provided by the embodiments of the present invention is about 3 times that of the comparative examples of the prior art, showing a very excellent flame retardant effect, and the flame retardant temperature is also much higher than that of the polyethylene material provided by the comparative examples of the prior art; in addition, from the test index of the oxygen index (the oxygen index refers to the minimum oxygen concentration when the material just maintains flame combustion in a mixed gas of O2 and N2 at room temperature under the prescribed test conditions, expressed as a percentage of volume. A high oxygen index indicates that the material is not easy to burn, a low oxygen index indicates that the material is easy to burn, and the higher the oxygen index indicates that the flame retardant property is better), the oxygen index of the polyethylene material provided by the embodiments of the present invention is about twice that of the comparative examples, therefore, the comprehensive flame retardant property of the polyethylene material provided by the embodiments of the present invention is very excellent. At the same time, it can also be seen that the polyethylene material provided in the embodiment of the present invention not only has excellent flame retardant properties and good environmental protection, but also has outstanding mechanical properties. Its tensile strength, bending strength and impact strength are also higher than those of the control example, showing excellent comprehensive mechanical properties, which makes it have a basis for wide application in multiple scenarios.
[0111] Furthermore, the above-mentioned Examples 1-20 and the comparative example were subjected to simulation tests under the same conditions. Specifically, 21 portions of NaCl solution with a mass concentration of 5% were prepared, each portion of NaCl solution was placed in a 1000ml beaker according to an amount of 1000ml, and each sample was completely immersed in the NaCl solution. After soaking for 21 days, the samples were taken out and rinsed with deionized water, and the water resistance and corrosion resistance of each test sample were observed and analyzed. It should be noted that in the test of the present invention, in addition to direct observation and analysis, the corrosion resistance of the test samples can also be evaluated by the weight loss method, and the water resistance of the test samples can be tested by a waterproof tester. The above test was repeated three times and the average was taken. The test results obtained are shown in Table 2:
[0112] Table 2 Comparative test results of anti-corrosion and waterproof performance
[0113]
[0114]
[0115]
[0116] It can be seen from Table 2 that the polyethylene material samples with high-efficiency flame retardant properties of Examples 1-20 provided by the present invention in the test examples are superior to the samples of the comparative examples in terms of water resistance and corrosion resistance as a whole, among which the polyethylene material sample of Example 1 has the best water resistance and corrosion resistance, with a corrosion inhibition efficiency of 99.99% and a water resistance rate of 99.98%. In addition, it should be noted that, from a horizontal comparison of the samples of Examples 1-20, it can be found that the other additives, sodium tungstate, cerium nitrate and titanium dioxide, still have a certain influence on the corrosion resistance and water resistance of the polyethylene material. Compared with Example 20 in which sodium tungstate, cerium nitrate and titanium dioxide are not added, the polyethylene material samples of Examples 1-19 to which sodium tungstate, cerium nitrate and titanium dioxide are added have more excellent corrosion resistance and water resistance, among which the corrosion resistance efficiency is above 99%, and the water resistance efficiency is basically above 99.50%.
[0117] In summary, the embodiment of the present invention provides a polyethylene material with high-efficiency flame retardant properties. By reasonably configuring an inorganic flame retardant in polyethylene, the polyethylene material has high-efficiency flame retardant properties; by reasonably configuring a synergist in polyethylene, the polyethylene material has high-efficiency flame retardant properties while also having good comprehensive mechanical properties as well as corrosion resistance and waterproof properties; by reasonably configuring other additives in polyethylene, the mechanical properties and anti-corrosion and waterproof properties of the polyethylene material are further improved and strengthened. Therefore, the polyethylene material provided by the embodiment of the present invention not only has high-efficiency flame retardant properties, but also has excellent other properties; in addition, the preparation method of the above-mentioned polyethylene material provided by the embodiment of the present invention has a simple process, low pollution, and can efficiently prepare the above-mentioned polyethylene material of high quality, which is suitable for industrial production.
[0118] The embodiments described above are part of the embodiments of the present invention, rather than all of the embodiments. The detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
Claims
1. A polyethylene material with high efficiency flame retardant properties, characterized in that: It is made of a variety of raw materials, which include by weight: Polyethylene 90-110 parts; Flame retardant 15-25 parts; 10-20 parts of synergist; and 4-19 parts of other additives; The flame retardant comprises aluminum hydroxide, zinc borate, antimony oxide, zirconium oxide, tin oxide and molybdenum oxide; the mass ratio of aluminum hydroxide, zinc borate, antimony oxide, zirconium oxide, tin oxide and molybdenum oxide is 5:4:2:2:3:6; The synergist includes at least one of graphene, carbon nanotubes and montmorillonite; The other additives include oxidized polyethylene wax, basalt fiber and titanate, and the mass ratio of the oxidized polyethylene wax, the basalt fiber and the titanate is 2:2:
1.
2. The polyethylene material with high efficiency flame retardant performance according to claim 1, characterized in that: The various raw materials are made of the following raw materials in parts by weight: 95-105 parts of polyethylene; 20-24 parts of the flame retardant; 15-19 parts of the synergist; and The other additives are 10-16 parts.
3. The polyethylene material with high-efficiency flame retardant performance according to claim 2, characterized in that: The weight portion of the flame retardant is 22 parts, and the flame retardant includes, by weight: 5 parts of the aluminum hydroxide; 4 parts of the zinc borate; 2 parts of the antimony oxide; 2 parts of the zirconium oxide; 3 parts of tin oxide; and Described molybdenum oxide 6 parts.
4. The polyethylene material with high efficiency flame retardant performance according to claim 2, characterized in that: The weight portion of the synergist is 18 parts, and the synergist comprises, by weight: 5 parts of the graphene; 6 parts of the carbon nanotubes; and 7 parts of the montmorillonite.
5. The polyethylene material with high-efficiency flame retardant performance according to claim 1, characterized in that: The weight portion of the other additives in the plurality of raw materials is 19 parts.
6. The polyethylene material with high efficiency flame retardant performance according to claim 5, characterized in that: The other additives also include sodium tungstate, cerium nitrate and titanium dioxide; The weight ratio of the oxidized polyethylene wax, the basalt fiber, the titanate, the sodium tungstate, the cerium nitrate and the titanium dioxide in the other additives is 4:4:2:5:1:
3.
7. A method for preparing the polyethylene material with high efficiency flame retardant properties as claimed in claim 1, characterized in that: It includes the following steps: By weight, 15-25 parts of flame retardant, 10-20 parts of synergist and 4-19 parts of other additives are dried and mixed uniformly to obtain a first mixture; Melt blending the first mixture with 90-110 parts of polyethylene to obtain a second mixture; The second mixture is extruded into granules through an extrusion device, cooled and dried, and then screened to obtain the polyethylene material with high-efficiency flame retardant performance.
8. The method for preparing a polyethylene material with high-efficiency flame retardant properties according to claim 7, characterized in that: In the process of obtaining the first mixture, the other additives also include sodium tungstate, cerium nitrate and titanium dioxide; When the first mixture and the polyethylene are melt-blended, the melting temperature is 150-190° C. and the time is 20-35 min; During the cooling and drying, the cooling rate is controlled at 9°C / hour.