Long-term elastic stability of stainless steel materials for deep-sea robots
By adjusting the chemical composition of Fe-Cr-Ni stainless steel and using vacuum induction smelting and electroslag remelting dual processes, deep-sea long-term elastic and stable stainless steel materials with extremely high elastic stability and excellent mechanical properties were prepared, and the existing solutions were solved The problem of insufficient material performance meets the requirements of service of deep-sea robots.
Patent Information
- Application Number
- CN202311565822.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-22
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-11-22
AI Technical Summary
The existing deep-sea long-term elastic and stable stainless steel materials have problems such as low metallurgy quality, poor comprehensive performance, poor dimensional tolerance, poor surface quality and poor batch quality stability, and cannot meet the service requirements of deep-sea robots.
Adjust chemical composition based on Fe-Cr-Ni, increase chromium content and reduce nickel content, combine vacuum induction smelting and electroslag remelting dual processes, and after hot processing, cold processing and deep cold treatment, extremely elastic and stable performance are prepared and stainless steel materials with excellent mechanical properties.
It has achieved extremely high elastic stability, excellent mechanical properties and good seawater corrosion resistance of stainless steel materials for deep-sea robots, meeting the requirements of service of deep-sea robots.
Smart Images

Figure CN117845128B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of metal materials, and in particular relates to a stainless steel material with long-term elastic stability for deep-sea robots. Background Art
[0002] With the utilization and development of marine resources, countries around the world have increased their research and development of marine equipment. The springs and components required for underwater exploration robots, marine excavation equipment, deep-sea submersibles, underwater search and rescue equipment, etc. require materials with good elastic properties and seawater corrosion resistance in the deep sea.
[0003] Usually springs and spring components are required to have the following properties: After 720 hours of loading with a displacement compression load of 10%, the change rate of the spring free length is less than 1%. Long-term elastic stability: The change rate of the spring free length is less than 2%. The tensile strength of the spring wire is Rm ≥ 1280MPa, Rp0.2 ≥ 765MPa, A ≥ 3%, Z ≥ 20%, HV ≥ 380, E ≥ 190GPa; after 1000 hours of long-term static clamping (elastic deformation of the element is 10%), the dimensional change rate (elastic stability of 10% elastic deformation) is ≤ 0.5% (the ratio of the change in size to the original size), and the long-term elastic stability (free length change rate) after the limit load is less than 2%. After 60 days of seawater immersion, the tensile strength meets Rm ≥ 1250MPa, and has good seawater corrosion resistance.
[0004] The elastic components include spiral elastic retaining rings, expansion rings, clamping rings, locking rings, etc.
[0005] At present, deep-sea long-term elastic stability stainless steel materials generally have problems such as low raw material metallurgical quality, poor comprehensive performance, poor wire and flat wire dimensional tolerance, unsatisfactory surface quality, poor batch quality stability and consistency, etc. Compared with the international advanced level, there is still a large gap and it cannot meet the service requirements of deep-sea robots. The main reasons are:
[0006] (1) Weak composition optimization design and control capabilities. The composition of stainless steel for springs has developed from 15-7, 17-7, 18-8 to a new series of stainless steel materials with long-term elastic stability, and hundreds of grades have been formed. Elements such as C, N, Si, Mn, Mo, Cu, and Nb in the alloy have a huge impact on the strength, toughness, plasticity, and corrosion resistance of the material. Many companies are not good at composition design, especially micro-alloying; in addition, many manufacturers are unable to achieve full-process production and process control, resulting in low elastic performance and stability of the stainless steel materials produced.
[0007] (2) Poor metallurgical quality control. Metallurgical purity and composition uniformity are one of the main gaps between domestic and foreign high-performance metal material products. The poor metallurgical quality of domestic stainless steel is the main reason for poor material performance, poor uniformity, and poor performance. In addition, large non-metallic inclusions will also have a significant impact on the performance and quality of precision strip.
[0008] (3) The cold processing technology of deep-sea long-term elastic stability stainless steel is much more difficult than that of ordinary steel. It involves a series of key process technologies, including cold-rolled plate shape and dimensional tolerance control technology, micro-defect detection and removal technology, protective atmosphere continuous annealing technology, high-precision rolling technology, microstructure and performance regulation heat treatment technology, precision striping technology, and other spring round wire and special-shaped wire drawing technologies, which require good hardware basic conditions and, more importantly, rely on long-term technical accumulation.
[0009] Chinese scientists have studied the elastic relaxation of stainless steel materials with long-term elastic stability. The study shows that the instability of the organization and mechanical properties of stainless steel, iron-based stainless steel with long-term elastic stability, and nickel-based stainless steel with long-term elastic stability is the main reason for the instability of elastic relaxation. Summary of the invention
[0010] The purpose of the present invention is to provide a stainless steel material with long-term elastic stability for deep-sea robots. The material has the properties of elastic materials, filling the gap in this type of material in my country, filling the deficiency of similar foreign materials that have excessive displacement changes after long-term use, resulting in attenuation of elastic properties, and meeting the urgent needs of national key projects. Compared with existing stainless steel structural materials with long-term elastic stability, the material of the present invention has extremely high elastic stability, excellent mechanical properties, corrosion resistance, and good machining performance. The material of the present invention has excellent comprehensive mechanical properties, seawater corrosion resistance, intergranular corrosion resistance and other corrosion resistance properties.
[0011] The technical solution of the present invention is:
[0012] The material of the present invention adjusts the chemical composition on the basis of Fe-Cr-Ni, increases the chromium content and reduces the nickel content, so as to meet the performance requirements of long-term elastic stability for deep-sea robots: after long-term static clamping (elastic deformation of the element 10%) for 1000 hours, the dimensional change rate (elastic stability of 10% elastic deformation) is ≤0.5% (the ratio of the dimensional change to the original size).
[0013] The weight percentage of each component of the long-term elastic stability stainless steel material for deep-sea robots is:
[0014] C 0.040~0.055; Cr 17.0~20.0; Ni 3.0~4.5; Cu 1.0~2.5; Nb 0.2~0.40; Mn≤0.7; Mo 0.8~2.00; Si≤1.0; P≤0.006; S≤0.006; N 0.2~0.4, and the rest is Fe.
[0015] A better technical solution is that the weight percentage of each component of the material is:
[0016] C 0.042~0.054; Cr 17.79~19.5; Ni 3.2~4.4; Cu 1.3~2.43; Nb 0.25~0.35; Mn 0.2~0.6; Mo 1.0~1.8; Si 0.2~0.4; P0.0017~0.00336; S 0.0008~0.0016; N 0.25~0.35, and the rest is Fe.
[0017] The application of the above-mentioned stainless steel material in the preparation of structural parts for deep-sea robot substrates.
[0018] The material of the present invention is melted by vacuum induction, and then undergoes an electroslag remelting double process to obtain an alloy ingot, and then undergoes hot working and cold working to obtain a bar, slab, strip or wire, etc. The material finally needs to be cryogenically treated.
[0019] 1) Vacuum induction melting adopts a two-step refining process; the first refining is at a temperature of (1530-1560) ±5°C, the vacuum degree is controlled at 3-8Pa, and the refining is for 10-20 minutes; the second refining is at a temperature of (1530-1560) ±5°C, the vacuum degree is controlled at 1-2×10 -1 Pa or above, refining for 10 minutes to control component segregation, and then electromagnetic stirring;
[0020] 2) Casting and melting electrode rod
[0021] The molten steel after the second refining is uniformly poured at a medium speed in a thin stream, the pouring time is 12 to 18 seconds, and the pouring temperature is controlled to (1530 to 1560) ± 5°C to obtain the remelted electrode rod; the pouring is carried out at a low temperature and uniform speed as much as possible;
[0022] 3) Obtained by electroslag remelting
[0023] The CaF-CaO-Al2O3-MgF quaternary slag system is used for electroslag remelting to further deoxidize and desulfurize, improve the morphology of inclusions, and improve the metallurgical quality of the steel ingot.
[0024] 4) Homogenization heat treatment
[0025] Before forging, the electroslag rod is subjected to homogenization heat treatment at 1140°C. For electroslag rods with a diameter greater than 200mm, the total insulation time is determined by 1.5min for 1mm; for electroslag rods with a diameter less than 200mm, the insulation time is 5h.
[0026] 5) Processing
[0027] The electroslag rod is processed into bars, slabs, strips and wires through homogenization heat treatment, forging, finishing, hot rolling, cold rolling, cold drawing and other processes. Among them, the hot working temperature is 1130℃~900℃; solid solution treatment is required during the cold working process to eliminate cold work hardening. The solid solution treatment system is the holding temperature of 980~1080℃, the holding time of 60~100 minutes, and water quenching.
[0028] When elastic elements such as springs are made of the material described in the present invention, they need to undergo conventional aging heat treatment at 420-490° C.×4h.
[0029] After the conventional aging of the material, deep cold aging treatment is required. The material is placed in a mixture of dry ice + ethanol at a temperature of -60 to -80 degrees Celsius for 16 hours.
[0030] The method of the present invention performs property transformation + conventional aging treatment + deep cold aging heat treatment on stainless steel materials with long-term elastic stability to stabilize the structure and form spring components of stainless steel materials with long-term elastic stability; strips, foils, spring round wires and special-shaped wires are formed into elastic components, and telescopic arms and spring components for deep-sea robots are manufactured by performing stabilization heat treatment.
[0031] The functions of each element in the material of the present invention are as follows:
[0032] Chromium Cr is a signature element of stainless steel. Its primary function is to improve corrosion resistance and make it "rust-proof". An appropriate amount of chromium can make the alloy have good corrosion resistance in a variety of media, especially in oxidizing environments. When the ratio of Cr and Ni is appropriate, the corrosion resistance is even better. However, as the Cr content increases to a certain level, intermetallic compounds such as σ phase will form in the alloy, which will have an adverse effect on strength and plasticity.
[0033] Nickel Ni is the main element that forms austenite in stainless steel. It stabilizes the austenite structure and improves the toughness of the alloy. It is also beneficial for inhibiting the precipitation of harmful phases such as σ, μ, and Laves, which can prevent the occurrence of brittleness and improve the stability of the metal.
[0034] On the one hand, carbon C is a strong austenite-forming element, and its degree of action is 30 times that of nickel. It also has a solid solution strengthening effect, and a small amount of it can significantly enhance the strength of austenitic alloys; on the other hand, it has a great affinity with chromium and can form a series of complex carbides with chromium, which will lead to chromium depletion at the grain boundaries. Therefore, although excessive carbon content is beneficial to improving strength, it will greatly enhance the stability of austenite, making it difficult for deformation-induced martensitic phase transformation, and at the same time it will aggravate chromium depletion at the grain boundaries, which is not conducive to intergranular corrosion. From the perspective of strength and corrosion resistance, the role of carbon in stainless steel is contradictory.
[0035] The ability of nitrogen N to form austenite is comparable to that of carbon, and it also has a strong solid solution strengthening effect, which can significantly increase the strength of austenitic stainless steel without significantly reducing its toughness and plasticity. In addition, nitrogen can improve the local corrosion resistance of steel in a variety of media, including intergranular corrosion, pitting corrosion and crevice corrosion. Therefore, nitrogen has increasingly become an important alloying element for chromium-nickel austenitic stainless steel.
[0036] Manganese Mn In chromium-nickel austenitic stainless steel, the Mn content is generally specified not to exceed 2%, and is mostly controlled at around 1.5% in normal production. Mn is a relatively weak austenite-forming element, but has a strong effect of stabilizing austenite. Studies have shown that when the Mn content in steel is less than 2%, the change in Mn content has no significant effect on the structure (including the stability of austenite) of commonly used chromium-nickel austenitic stainless steel. In addition to deoxidation, the role of Mn in chromium-nickel austenitic stainless steel is to stabilize austenite, improve the thermoplasticity of steel, and form manganese sulfide with the help of the strong affinity of Mn and S, which is beneficial to the removal of S in steel and the elimination of the harmful effects of residual S in steel. However, further studies have shown that the presence of Mn in steel often leads to a decrease in the resistance of chromium-nickel austenitic stainless steel to chloride pitting corrosion and crevice corrosion due to the formation of manganese sulfide. The measured values of Mn content (Wt%) in ЭИ708А alloy are 0.23% and 0.18%. The values in relevant data show that the range of Mn is Mn<0.3%. In order to control the formation of manganese sulfide in the alloy and ensure the corrosion resistance of the alloy, the research team believes that the Mn content should be controlled below 0.3% (Mn<0.3%).
[0037] Silicon (Si) is an element that shrinks the γ phase. A certain amount of silicon can deoxidize and purify the alloy, but when the Si content is too high, it will increase the brittleness of the alloy material and reduce the processing performance of the material. Therefore, it is usually regarded as a permanent impurity element in general stainless steel. However, because Si is beneficial to resist the corrosion of oxidizing media, stainless steel containing silicon has been developed.
[0038] Copper (Cu) can significantly reduce the cold hardening tendency of chromium-nickel austenitic stainless steel, improve cold working formability, and is beneficial to local corrosion resistance. Copper is added to the material of the present invention to improve the seawater corrosion resistance of the alloy material and also play a secondary hardening effect in the long-term elastic stability alloy.
[0039] The role of molybdenum (Mo) in long-term elastic stability stainless steel, adding molybdenum can increase tempering stability and strengthen the secondary hardening effect, improve corrosion resistance, and increase the strength of steel without reducing toughness. However, too high molybdenum will promote the formation of ferrite, which has an adverse effect on the alloy. To prevent the transformation to ferrite, the range of molybdenum is controlled at 0.8-2.0%.
[0040] The role of niobium (Nb) is generally to add Nb to long-term elastic stability stainless steel in order to improve the strength of the alloy material. The material of the present invention adds a small amount of niobium to significantly improve the tensile strength of the alloy, improve the toughness and corrosion resistance of the alloy material, reduce the brittle transition of the alloy material, and make the alloy material have good welding performance and forming performance. Niobium is generally added in a small amount to long-term elastic stability stainless steel materials. When the niobium content exceeds 5%, the hot working performance of the alloy material decreases.
[0041] Phosphorus and sulfur (P, S) affect the mechanical properties of deep-sea long-term elastic stability stainless steel and should be strictly controlled as harmful elements.
[0042] The applicant's experimental verification shows that as the telescopic arm spring material, after deformation + aging: Rm ≥ 1280MPa, Rp0.2 ≥ 765MPa, A ≥ 3%, Z ≥ 20%, HV ≥ 380, E ≥ 190GPa;
[0043] The material of the present invention has good mechanical properties and elastic stability. The room temperature tensile property Rm is 1360-1750MPa, A≥4%, and the hardness HV is 420-490. The room temperature elastic modulus is 212GPa≥E≥190GPa. After long-term static clamping (elastic deformation of the element is 10%) for 1000 hours, the dimensional change rate (elastic stability of 10% elastic deformation) is ≤0.3% (ratio of dimensional change to original size), and the long-term elastic stability (free length change rate) after the limit load is less than 2%. After 60 days of seawater immersion, the tensile strength meets Rm 1360-1750MPa, and has good seawater corrosion resistance. It can be used to make plates, rods, narrow strips, rods, wires, micro-filaments and their products.
[0044] The elastic properties of the material of the present invention are as follows: when the spring is loaded with a displacement compression load of 10%, after 720 hours, the free length change rate of the spring made of the material of the present invention is ≤0.3%, and after extreme compression, the size change rate is ≤1.0%. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 This is a schematic diagram of a spring wound with the material described in the present invention. DETAILED DESCRIPTION
[0046] Embodiment 1: According to the chemical composition (Wt%) C 0.042; Cr 17.79; Ni 3.2; Cu 1.30; Nb 0.25; Mn 0.3; Mo 1.0; Si 0.2; N 0.25, and the balance Fe is used to control the ingredients, and the steel ingot is manufactured by a double process of vacuum melting and electroslag remelting, and is hot-processed and cold-processed into plates and strips. The material can be used to make structural parts for deep-sea robot substrates, and can be widely used in navigation, petrochemical, machinery, and automobile industries.
[0047] Embodiment 2: According to the chemical composition (Wt%) of C 0.049; Cr 18.22; Ni 3.8; Cu 1.85; Nb 0.3; Mn 0.2; Mo 1.5; Si 0.3; N 0.3, and the balance Fe, a steel ingot is manufactured by a double process of vacuum melting and electroslag remelting, is hot-processed and cold-processed into a precision narrow strip, and then is made into parts such as deep-sea robot telescopic arm springs through a special rolling process (the winding direction and the width direction of the flat wire cross section are kept in the same horizontal plane), which can be widely used in functional components such as deep-sea springs.
[0048] Example 3: C 0.053; Cr 19.5; Ni 4.4; Cu 2.45; Nb 0.35; Mo 1.8; Si 0.4; N 0.35, the balance Fe controls the ingredients, and the steel ingot is manufactured by vacuum melting and electroslag remelting double process, and is hot-processed and cold-processed into wires and micro-wires of various specifications. It is used to make telescopic springs for deep-sea robots, various elastic elements, and stainless steel materials with long-term elastic stability required by instrumentation, aerospace, and petrochemical industries.
[0049] The steel of the present invention was charged with dozens of furnaces (30 kg per furnace) of material for performance testing. The grade of the steel was named SHSS (ShenHai Spring Steel, wherein SHSS1 is the material described in Example 1; SHSS2 is the material described in Example 2; SHSS3 is the material described in Example 3), and its typical chemical composition analysis values are shown in Table 1.
[0050] Table 1 Chemical composition of invention steel (wt%)
[0051]
[0052] Compared with domestic and foreign materials, the stainless steel material of the present invention has excellent properties
[0053] The deformation form of the invented material and the mechanical properties of domestic and foreign long-term elastic stability stainless steel are shown in Table 2.
[0054] Table 2
[0055]
[0056] The material of the present invention is subjected to stabilization heat treatment at a temperature of 420-490° C. after being prepared into parts, so as to release excess internal stress and maintain long-term elastic stability.
[0057] The mechanical properties of the invented material and domestic and foreign long-term elastic stability stainless steel after deformation + stabilization heat treatment are shown in Table 3.
[0058] Table 3 Comparison of mechanical properties of the material of the present invention and domestic and foreign stainless steel (deformation + stabilization heat treatment)
[0059]
[0060] The rate of change of free length of the spring in the table is the rate of change of free length of the elastic element after 1000h when the load of the elastic element is 10% (displacement deformation), in order to examine the long-term elastic stability.
[0061] Corrosion resistance test of the material of the present invention
[0062] Artificial seawater uniform corrosion test
[0063] The invented materials SHSS-1, SHSS-2 and SHSS-3 have good corrosion resistance, which is better than that of SUS304, SUS316 and NS113 materials.
[0064] The invention material and the comparative material were subjected to intergranular corrosion tests according to GB / T4334.5-2000 "Corrosion of Metals and Alloys - Test Methods for Intergranular Corrosion of Stainless Steel". After 560 hours of testing, the results showed that there were no cracks caused by intergranular corrosion.
[0065] After 1440 hours of testing according to GB / T 6384 “Test methods for seawater corrosion of metallic materials for ships and marine engineering in natural environments”, the changes in mechanical properties of the invention material and the comparative material after deformation + stabilization heat treatment are shown in Table 4.
[0066] Table 4
[0067]
[0068] After being corroded by natural seawater, the mechanical properties of the invented material are more consistent than those of other comparative materials.
[0069] According to GB / T10124 “Metallic Materials Laboratory Uniform Corrosion Full Immersion Test Method”, after 560 hours of testing, the corrosion rates R (mm / a) of the invention material and the comparative material are shown in Table 5.
[0070] Table 5
[0071]
[0072] After the invention material and the comparative material were subjected to a neutral salt spray test for 48 hours according to GJB150.11 "Salt spray test for environmental test methods for military equipment", the test comparison results are shown in Table 6.
[0073] Table 6 Test results of samples after 24h neutral salt spray test
[0074]
[0075] Long-term stability of the elastic properties of the invented material
[0076] The inventive material is processed into a wire with a diameter of 4.0 mm by cold deformation, and then wound into a spring with an outer diameter of 31.5 mm, a pitch of 5 mm, an effective number of turns of 5, and a free length of 45 mm. Figure 1 The standard spring specimens processed as shown are subjected to stabilization heat treatment at 420-490℃×4h to test the long-term stability of the spring.
[0077] Inventive material with long-term elastic stability.
[0078] The existing spring material design at home and abroad requires that the spring load is 30% of the ultimate load, and the long-term elastic stability (free length change rate) is less than 2%. The dimensional stability of the invented material is far better than this level. Table 7 is the long-term elastic stability test analysis of the invented material.
[0079] Table 7 Analysis of long-term elastic stability test of inventive materials
[0080]
Claims
1. A stainless steel material with long-term elastic stability for deep-sea robots, characterized in that: The weight percentage of each component of this material: C 0.042~0.054, Cr 17.79~19.5, Ni 3.2~4.4, Cu 1.3~2.43, Nb 0.25~0.35, Mn0.2~0.6, Mo 1.0~1.8, Si 0.2~0.4, P 0.0017~0.00336, S 0.0008~0.0016, N 0.25~0.35, the rest is Fe; The long-term elastic stability: the change rate of the spring free length is less than 2%, the tensile strength of the spring wire is Rm≥1280MPa, Rp0.2≥765MPa, A≥3%, Z≥20%, HV≥380, E≥190GPa; after long-term static clamping for 1000 hours, the dimensional change rate is ≤0.5%, the long-term elastic stability after the limit load is less than 2%, and after immersion in seawater for 60 days, the tensile strength meets Rm≥1250MPa, and it has good resistance to seawater corrosion.
2. The stainless steel material according to claim 1, characterized in that: The weight percentage of each component of this material: C 0.042, Cr 17.79, Ni 3.2, Cu 1.30, Nb 0.25, Mn0.3, Mo 1.0, Si 0.2, N 0.25, P0.0033, S 0.00011, balance Fe.
3. The stainless steel material according to claim 1, characterized in that: The weight percentage of each component of this material: C 0.049, Cr 18.22, Ni 3.8, Cu 1.85, Nb 0.3, Mn0.2, Mo 1.5, Si 0.3, N 0.3, P0.0028, S 0.0008, balance Fe.
4. The stainless steel material according to claim 1, characterized in that: The weight percentage of each component of this material: C 0.054, Cr 19.5, Ni 4.4, Cu 2.45, Nb 0.35, Mn0.6, Mo 1.8, Si 0.4, N 0.35, P0.0017, S 0.0016, balance Fe.
5. Use of the stainless steel material according to any one of claims 1 to 4 in preparing structural parts for a deep-sea robot substrate.
Citation Information
Patent Citations
Multielement composite heat-resistant steel
CN104651743A
Stainless steel for bridge pile with high strength corrosion resistance
CN111088459A
High-temperature-resistant concentrated sulfuric acid corrosion austenitic stainless steel with excellent hot working performance and hot perforating method thereof
CN113201697A
Austian iron-based stainless steel
CN115997042A
Austenitic stainless steel of improved stress corrosion resistance
GB1216550A