Offline batch activation device and activation method for membrane electrode

By designing an offline batch activation device, using the principle of electrochemical hydrogen pump and the insulating plate fixing structure, the rapid and simple batch activation of membrane electrodes is achieved, and the problems of low activation efficiency and complex operation in the prior art are solved, which significantly improves the problem of high-quality membrane electrode activation efficiency and significant improvements in the existing technology. The performance and efficiency of the membrane electrode after activation are achieved.

CN117855539BActive Publication Date: 2024-11-05SINOHYKEY TECHNOLOGY (GUANGZHOU) CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410107302.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-25
Publication Date
2024-11-05
Estimated Expiration
2044-01-25

AI Technical Summary

Technical Problem

The prior art is difficult to achieve rapid and batch activation of membrane electrodes, and the online activation method requires stack or battery assembly, which is complex in operation and is inconvenient for large-scale production.

Method used

An offline batch activation device is designed, including an activation chamber, an intake passage, an outlet passage and an external power supply. The membrane electrode is activated through the principle of electrochemical hydrogen pump, and the membrane electrode is fixed by insulating plates and conductive collector plates to simplify operation. and improve activation efficiency.

Benefits of technology

The rapid and simple batch activation of membrane electrodes is achieved, which reduces hydrogen input demand, reduces costs, and significantly improves the performance of membrane electrodes after activation, and shortens the online activation time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117855539B_ABST
    Figure CN117855539B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of fuel cells, and provides an offline activation device and activation method for a membrane electrode, wherein the offline activation device comprises an activation chamber, an air inlet channel, an air outlet channel and an external power supply, wherein the air inlet channel and the air outlet channel are connected through the activation chamber, and the external power supply is electrically connected to the membrane electrode; an upper insulating plate and a lower insulating plate are connected in the activation chamber, and a plurality of membrane electrode fixing positions are arranged between the upper insulating plate and the lower insulating plate, and each membrane electrode fixing position is provided with a first conductive current collecting plate and a second conductive current collecting plate, and the first conductive current collecting plate and the second conductive current collecting plate are closely attached to both sides of the membrane electrode. Advantages: (1) There is no need to assemble the membrane electrode into a battery or a stack and then perform electrochemical hydrogen pump activation, which has a simple structure, is easy to operate, and improves the activation efficiency. (2) There is no need to divide the activation chamber into a cathode chamber and an anode chamber, and the hydrogen generated by the cathode catalyst layer can be supplied to the anode catalyst layer, thereby reducing the use of hydrogen and reducing costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of fuel cells, and more specifically, to an off-line batch activation device and an activation method for a membrane electrode. Background Art

[0002] Fuel cells, as a clean and efficient energy conversion technology, rely on electrochemical reactions at the membrane electrode (MEA) interface. The membrane electrode, as the core component of the fuel cell, needs to be activated before it is put into practical use. This is because the initial electrode material and structure usually need further regulation to optimize the catalytic activity, material transfer capacity and three-phase reaction interface of the membrane electrode so that it can achieve optimal performance during operation. Among the many activation methods of fuel cell membrane electrodes, electrochemical hydrogen pump is a very promising activation method because it can save time and hydrogen costs, increase catalyst utilization and battery performance. This method uses the principle of electrochemistry to pass humidified hydrogen into the anode, humidified inert gas or no ventilation into the cathode, and apply voltage or current at both ends of the fuel cell to oxidize the hydrogen at the anode into hydrogen ions, which are reduced to hydrogen through the proton exchange membrane to the cathode.

[0003] CN200610090751.2 discloses a fuel cell membrane electrode activation method using an electrochemical hydrogen pump. The patent introduces water into the cathode side of the membrane electrode, so that the water plays a certain sealing role, so that the hydrogen generated by the cathode produces a certain resistance in the process of outward diffusion, opens the closed pores and semi-closed pores in the catalyst layer, and makes the pore structure of the membrane electrode more connected. CN202310800150.X discloses a fuel cell stack rapid activation method combining electrochemical humidification and electrochemical hydrogen pump, which can improve the catalyst layer structure, activate the catalyst activity, remove impurities and oxides on the catalyst surface, and open the proton conduction channel, so that the fuel cell performance is restored.

[0004] Although the above electrochemical hydrogen pump methods have good activation effects, they are all based on single cell equipment or battery stack equipment online, and require separate chamber processing for the anode and cathode, which is not conducive to rapid and batch activation of membrane electrodes. Therefore, there is an urgent need for a simple offline method that can activate membrane electrodes in batches. Summary of the invention

[0005] The present invention aims to overcome at least one defect (shortcoming) of the above-mentioned prior art and provide an offline batch activation device and activation method for membrane electrodes, so as to improve the activation efficiency when the membrane electrodes are activated by adopting the principle of electrochemical hydrogen pump.

[0006] One object of the present invention is to provide an off-line batch activation device for a membrane electrode, comprising an activation chamber, an air inlet channel, an air outlet channel and an external power supply, wherein the air inlet channel and the air outlet channel are connected through the activation chamber, and the external power supply is electrically connected to the membrane electrode; an upper insulating plate and a lower insulating plate are connected in the activation chamber, a plurality of membrane electrode fixing positions are arranged between the upper insulating plate and the lower insulating plate, each membrane electrode fixing position is provided with a first conductive current collecting plate and a second conductive current collecting plate, and the first conductive current collecting plate and the second conductive current collecting plate are closely attached to both sides of the membrane electrode.

[0007] In the present technical solution, the activation chamber is the place where the membrane electrode is activated; during electrochemical activation, the air inlet channel is the channel for gas to enter the activation chamber, and the air outlet channel is the channel for gas to be discharged from the activation chamber; the upper insulating plate is a plate placed in a horizontal direction and connected to the upper part of the activation chamber; the lower insulating plate is a plate placed in a horizontal direction and connected to the lower part of the activation chamber; the membrane electrode fixing position is used to fix the membrane electrode to be tested, which can be a structure provided on the upper insulating plate and the lower insulating plate to fix the membrane electrode. The membrane electrode to be tested is electrically connected to the power supply through the first conductive current collecting plate and the second conductive current collecting plate.

[0008] This solution provides an offline batch activation device for membrane electrodes, which can be activated without assembling the membrane electrodes into a stack or battery, is simple to operate, and improves the activation efficiency; at the same time, other component structures of the stack and battery are omitted, and more membrane electrode fixing positions can be set, that is, more membrane electrodes can be activated at the same time, further improving the activation efficiency and realizing batch activation. In addition, the hydrogen generated by the cathode of the membrane electrode can be supplied to the anode catalyst layer of the adjacent membrane electrode, which greatly reduces the input of hydrogen and reduces the cost.

[0009] Furthermore, the upper insulating plate is provided with a plurality of upper slots, the lower insulating plate is provided with lower slots corresponding to the upper slots one by one, each corresponding upper slot and lower slot forms a membrane electrode fixing position, the first conductive current collecting plate is provided on one side of the notch of the upper slot and the lower slot, and the second conductive current collecting plate is provided on the other side of the notch of the upper slot and the lower slot.

[0010] In this technical solution, the upper clamping groove is a structure for limiting the upper edge of the membrane electrode; the lower clamping groove is a structure for limiting the lower edge of the membrane electrode; the first conductive current collecting plate and the second conductive current collecting plate clamp the membrane electrode tightly at the notch. The membrane electrode fixing position is a clamping groove, which has a good fixing effect on the membrane electrode, and only needs to be set on the upper insulating plate and the lower insulating plate, without adding additional fixing parts. The structure is simple and suitable for mass production. At the same time, it also saves more space for the membrane electrode and further improves the activation efficiency.

[0011] Furthermore, the distance between two adjacent card slots is 1 mm to 300 mm.

[0012] In this technical solution, if the distance between two adjacent slots is too close, so that the distance between the two membrane electrodes to be tested is too close, then the source of hydrogen in the catalyst layer of the anode of the middle membrane electrode basically only comes from the cathode of the adjacent membrane electrode, which affects the activation efficiency. In addition, it will also cause the problem of contact between the two adjacent conductive collector plates; if the distance between the two membrane electrodes to be tested is too far, the hydrogen generated by the cathode of the adjacent membrane electrode will be dispersed, reducing the hydrogen reaching the anode of the adjacent membrane electrode, and at the same time it will also reduce the space utilization rate, reduce the number of membrane electrodes to be tested, affect the activation efficiency, and increase the volume of the activation chamber, increasing the use of hydrogen. Therefore, the appropriate distance between the two adjacent slots can improve the activation efficiency, provide sufficient space for the conductive collector plate, and reduce the use of hydrogen, reducing costs.

[0013] Furthermore, the distance between both ends of the upper insulating plate and the lower insulating plate and the inner wall of the activation chamber is 0 mm to 100 mm.

[0014] In the present technical solution, the distance is preferably 10 mm to 60 mm, and an appropriate distance is left between the two ends of the insulating plate and the inner wall of the activation chamber, so that the hydrogen diffused to the top and bottom can enter the anode catalyst layer of the middle membrane electrode through the gap between the insulating plate and the inner wall, that is, the hydrogen contacted by the middle membrane electrode can be the hydrogen passing through the insulating plate from the top and bottom and the hydrogen generated by the cathode of the adjacent membrane electrode, thereby ensuring the hydrogen supply to the anode catalyst layer of the middle membrane electrode and preventing gas shortage, thereby ensuring the activation efficiency; furthermore, such a setting avoids excessive pressure near the air inlet channel, causing pressure difference and resulting in damage to the membrane electrode; at the same time, the appropriate distance also saves space and reduces the volume of the activation chamber.

[0015] Furthermore, the membrane electrodes are connected in parallel and / or in series. In this technical solution, the connection mode of the membrane electrodes is flexible and can adapt to different practical needs.

[0016] Another object of the present invention is to provide a batch activation method for membrane electrodes, using the above-mentioned batch activation device, comprising the following steps:

[0017] S1, placing the membrane electrode to be activated into the membrane electrode fixing position of the activation chamber, and connecting the membrane electrode to the external power supply;

[0018] S2, introducing humidified hydrogen into the activation chamber through the air inlet channel to detect the air tightness of the activation chamber;

[0019] S3, turning on the external power supply to activate the membrane electrode by electrochemical hydrogen pump;

[0020] S4. After the activation is completed, nitrogen is introduced into the activation chamber through the air inlet channel for purging.

[0021] The above method has simple steps and good operability.

[0022] Furthermore, in step S2, the temperature of the activation chamber is maintained at 25-85°C, and the relative humidity of the hydrogen is 20-300%. In this technical solution, too low a temperature will slow down the reaction rate, resulting in poor activation effect or prolonged activation time; too high a temperature will increase energy consumption and may cause damage to the MEA material. Too low a humidity is not conducive to the wetting of the proton membrane and ionomer, resulting in poor activation effect; too high a humidity will cause serious deformation of the MEA.

[0023] Further, in step S3, the electrochemical hydrogen pump activation is to activate the membrane electrode at a constant potential or constant current by an external power supply for a preset time; the constant potential is 0.001V-0.25V; the constant current is 10-2000mA / cm 2 .

[0024] Furthermore, the preset time is 5 to 300 minutes.

[0025] In the present technical solution, the preset time can be set according to actual needs, for example, according to the number of membrane electrodes to be activated; appropriate preset time setting can ensure sufficient activation of the membrane electrodes and avoid waste of resources due to too long activation time.

[0026] Furthermore, in step S4, the relative humidity of the nitrogen is 0%-100%, and the nitrogen purge time is 5-200 minutes.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] (1) The present invention is based on the principle of electrochemical hydrogen pump and can be activated without assembling the membrane electrode into a stack or battery. The operation is simple and the activation efficiency is improved. At the same time, other component structures of the stack and the battery are omitted, and more membrane electrode fixing positions can be set, that is, more membrane electrodes can be activated at the same time, further improving the activation efficiency and realizing batch activation.

[0029] (2) The hydrogen produced by the cathode of the membrane electrode can be supplied to the anode catalyst layer of the adjacent membrane electrode, greatly reducing the input of hydrogen and lowering costs.

[0030] (3) The present invention utilizes the principle of electrochemical hydrogen pump, which helps to activate the catalyst, remove impurities and oxides on the catalyst surface, dredge the material transmission channel, and maximize the three-phase reaction interface, thereby improving the performance of the membrane electrode before and after online activation.

[0031] (4) When the off-line batch activation device and method of the present invention is used as a pretreatment before online activation, it can significantly reduce the online activation time of the membrane electrode and improve the performance of the membrane electrode after activation. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 Schematic diagram of the membrane electrode parallel structure of the batch activation device in Example 1.

[0033] Figure 2 This is a schematic diagram of the membrane electrode series structure of the batch activation device in Example 1.

[0034] Figure 3 The polarization curve performance comparison of the membrane electrode of comparative example 1 and embodiment 2.

[0035] Figure 4 The polarization curve of comparative example 1 changes with activation time.

[0036] Figure 5 This is the change of the polarization curve of Example 2 with activation time.

[0037] Figure 6 This is a comparison of the final polarization curve performance of the membrane electrode of Example 1 and Example 2 after complete hydrogen / air online activation.

[0038] Figure numerals: activation chamber 100, upper insulating plate 110, upper slot 111, lower insulating plate 120, lower slot 112, air inlet channel 200, air outlet channel 300, external power supply 400, membrane electrode 500, first conductive current collecting plate 600, second conductive current collecting plate 700. DETAILED DESCRIPTION

[0039] The drawings of the present invention are only for illustrative purposes and should not be construed as limiting the present invention. In order to better illustrate the following embodiments, some parts of the drawings may be omitted, enlarged or reduced, and do not represent the size of the actual product; it is understandable to those skilled in the art that some well-known structures and their descriptions in the drawings may be omitted.

[0040] Example 1

[0041] refer to Figure 1 and Figure 2This embodiment provides an off-line batch activation device for a membrane electrode 500, comprising an activation chamber 100, an air inlet channel 200, an air outlet channel 300 and an external power supply 400, wherein the air inlet channel 200 and the air outlet channel 300 are connected through the activation chamber 100, and the external power supply 400 is electrically connected to the membrane electrode 500; an upper insulating plate 110 and a lower insulating plate 120 are connected in the activation chamber 100, and a plurality of membrane electrode fixing positions are arranged between the upper insulating plate 110 and the lower insulating plate 120, and each membrane electrode fixing position is provided with a second conductive current collecting plate 700 and a second conductive current collecting plate, and the second conductive current collecting plate 700 and the second conductive current collecting plate are closely attached to both sides of the membrane electrode 500. Specifically, a notch is arranged at the front side of the activation chamber 100, and a closed door is movably connected to the notch, and the closed door can close the notch, and the membrane electrode 500 to be tested is taken and placed through the notch. The upper insulating plate 110 and the lower insulating plate 120 may be made of nylon, glass fiber, epoxy resin, PP or PE.

[0042] The upper insulating plate 110 is provided with a plurality of upper slots 111, and the lower insulating plate 120 is provided with lower slots 112 corresponding to the upper slots 111 one by one, and each corresponding upper slot 111 and lower slot 112 form a membrane electrode fixing position, and the second conductive current collecting plate 700 is provided on one side of the notch of the upper slot 111 and the lower slot 112, and the second conductive current collecting plate is provided on the other side of the notch of the upper slot 111 and the lower slot 112. That is, one upper slot 111 corresponds to one lower slot 112, and the membrane electrode 500 to be tested is placed in the membrane electrode fixing position.

[0043] In this embodiment, the activation chamber 100 is provided with openings on both sides, the two openings are connected to the air inlet channel 200 and the air outlet channel 300 respectively, and the two openings are provided between the upper insulating plate 110 and the lower insulating plate 120. The membrane electrode 500 to be tested is placed in the membrane electrode fixing position, and its cathode catalyst layer is all facing the air outlet channel 300. The second conductive collector plate 700 is closely attached to the cathode gas diffusion layer on the membrane electrode 500, and the second conductive collector plate is closely attached to the anode gas diffusion layer on the membrane electrode 500.

[0044] The distance between two adjacent slots is 1 mm to 300 mm, preferably 20 mm to 100 mm. The distance between the two ends of the upper insulating plate 110 and the lower insulating plate 120 and the inner wall of the activation chamber 100 is 0 mm to 100 mm, preferably 10 mm to 60 mm.

[0045] The membrane electrodes 500 are connected in parallel and / or in series. That is, the membrane electrodes 500 are connected in parallel, or the membrane electrodes 500 are connected in series, or the membrane electrodes 500 are connected in a mixed manner of parallel and series. A temperature controller is also provided in the activation chamber 100, and the temperature controller is used to control the temperature in the activation chamber 100.

[0046] Example 2

[0047] This embodiment provides a batch activation method for a membrane electrode, using the off-line batch activation device provided in Embodiment 1, and the batch activation method comprises the following steps:

[0048] S1. Place the membrane electrode to be activated in the membrane electrode fixing position of the activation chamber, connect the positive electrode of the external power supply to the anode of the membrane electrode, and connect the negative electrode of the external power supply to the cathode of the membrane electrode;

[0049] S2. Introduce humidified hydrogen into the activation chamber through the air inlet channel to detect the air tightness of the activation chamber; the temperature of the activation chamber is maintained at 40° C., and the relative humidity of the hydrogen is 150%.

[0050] S3, the electrochemical hydrogen pump activation is to activate the membrane electrode at a constant potential by an external power supply for a preset time; the constant potential is 0.06 V and the preset time is 120 minutes.

[0051] S4. After the activation is completed, nitrogen is introduced into the activation chamber through the air inlet channel for purging. The relative humidity of the nitrogen is 50%, and the purging time is 30 minutes.

[0052] Example 3

[0053] This embodiment provides a batch activation method for a membrane electrode, using the off-line batch activation device provided in Embodiment 1, and the batch activation method comprises the following steps:

[0054] S1. Place the membrane electrode to be activated in the membrane electrode fixing position of the activation chamber, connect the positive electrode of the external power supply to the anode of the membrane electrode, and connect the negative electrode of the external power supply to the cathode of the membrane electrode;

[0055] S2. Introduce humidified hydrogen into the activation chamber through the air inlet channel to detect the air tightness of the activation chamber; the temperature of the activation chamber is maintained at 85° C., and the relative humidity of the hydrogen is 250%.

[0056] S3, the electrochemical hydrogen pump activation is to activate the membrane electrode at a constant potential by an external power supply for a preset time; the constant potential is 0.25 V and the preset time is 5 minutes.

[0057] S4. After the activation is completed, nitrogen is introduced into the activation chamber through the air inlet channel for purging. The relative humidity of the nitrogen is 100%, and the purging time is 200 minutes.

[0058] Comparative Example 1

[0059] This comparative example is a membrane electrode that has not been activated offline.

[0060] The membrane electrode after offline activation in Example 2 and the membrane electrode without offline activation were assembled into a single cell for electrical performance testing. Figure 3 As shown, according to the test results, it can be seen that the pre-activation of the membrane electrode by the activation method of the present invention can improve the performance of the membrane electrode. The membrane electrode after offline activation in Example 3 and the membrane electrode that have not been offline activated are assembled into a single cell for electrical performance testing. The results are similar to those of Example 2. Compared with Comparative Example 1, its membrane electrode performance is significantly improved. In summary, it can be understood that the present invention can achieve pre-activation of the membrane electrode through a simple activation device and simple operation.

[0061] The membrane electrode without electrochemical hydrogen pump offline activation was assembled into a single cell at 2A / cm 2 The membrane electrode provided in Example 2 was assembled into a single cell and the current density was 2A / cm 2 Hydrogen / air online activation was carried out under a current density of 1.5 %. Before the activation began, the membrane electrode was initially evaluated for performance, and then a polarization curve test was performed every 30 minutes of activation. The activation was completed when the polarization curve was stable. Figure 4 and Figure 5 The polarization curves of comparative example 1 and example 2 change with activation time. As can be seen from the figure, when the online activation time is ≥90min, the polarization curve of comparative example 1 will no longer change with the extension of activation time, indicating that the online activation time for stable performance output of comparative sample 1 is 90min; when the online activation time is ≥60min, the polarization curve of example 2 will no longer change with the extension of activation time, indicating that the online activation time for stable performance output of the example is 60min. The online activation time of example 2 is significantly shorter than that of the comparative example, indicating that the use of the device and method of the present invention helps to shorten the online activation time, save test resources, and improve activation efficiency.

[0062] The final performance comparison between Comparative Example 1 and Example 2 after activation was performed. The results are as follows: Figure 6 As shown in the figure, it can be seen that the polarization curve performance of Example 2 after online activation is significantly better than that of the comparative example, indicating that the electrochemical hydrogen pump activation treatment of the membrane electrode in advance using the device and method of the present invention is beneficial to activating the catalyst, removing impurities and oxides on the catalyst surface, and opening up the material transmission path, thereby improving the final battery performance after the membrane electrode activation is completed.

[0063] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the technical solution of the present invention, and are not intended to limit the specific implementation methods of the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the claims of the present invention shall be included in the protection scope of the claims of the present invention.

Claims

1. An off-line batch activation device for a membrane electrode, characterized in that: It comprises an activation chamber, an air inlet channel, an air outlet channel and an external power supply, wherein the air inlet channel and the air outlet channel are connected through the activation chamber, and the external power supply is electrically connected to the membrane electrode; An upper insulating plate and a lower insulating plate are connected in the activation chamber, a plurality of membrane electrode fixing positions are arranged between the upper insulating plate and the lower insulating plate, each membrane electrode fixing position is provided with a first conductive current collecting plate and a second conductive current collecting plate, and the first conductive current collecting plate and the second conductive current collecting plate are closely attached to both sides of the membrane electrode; The upper insulating plate is provided with a plurality of upper slots, and the lower insulating plate is provided with lower slots corresponding to the upper slots one by one, and each corresponding upper slot and lower slot form a membrane electrode fixing position, the first conductive current collecting plate is provided on one side of the slot openings of the upper slots and the lower slots, and the second conductive current collecting plate is provided on the other side of the slot openings of the upper slots and the lower slots; the distance between two adjacent slots is 1mm to 300mm; the distance between both ends of the upper insulating plate and the lower insulating plate and the side inner wall of the activation chamber is 0mm to 100mm.

2. The off-line batch activation device of membrane electrode according to claim 1, characterized in that: The membrane electrodes are connected in parallel and / or in series.

3. A method for batch activation of a membrane electrode, using the off-line batch activation device for a membrane electrode according to any one of claims 1 or 2, characterized in that: The following steps are involved: S1, placing the membrane electrode to be activated into the membrane electrode fixing position of the activation chamber, and connecting the membrane electrode to the external power supply; S2, introducing humidified hydrogen into the activation chamber through the air inlet channel to detect the air tightness of the activation chamber; S3, turning on the external power supply to activate the membrane electrode by electrochemical hydrogen pump; S4. After the activation is completed, nitrogen is introduced into the activation chamber through the air inlet channel for purging.

4. The batch activation method according to claim 3, characterized in that: In step S2, the temperature of the activation chamber is maintained at 25-85°C, and the relative humidity of the hydrogen is 20-300%.

5. The batch activation method according to claim 4, characterized in that: In step S3, the electrochemical hydrogen pump activation is to activate the membrane electrode at a constant potential or constant current for a preset time by an external power supply; the constant potential is 0.001V-0.25V; the constant current is 10-2000mA / cm 2 .

6. The batch activation method according to claim 5, characterized in that: The preset time is 5 to 300 minutes.

7. The batch activation method according to any one of claims 3 to 6, characterized in that: In step S4, the relative humidity of the nitrogen is 0%-100%, and the nitrogen purge time is 5-200 minutes.

Citation Information

Cited By

  • Device for activating salt corrosion electrode

    CN120709420A