Connector and battery cell
By setting specific indentation areas on the laser injection surface of the pole column connecting part of the connecting sheet, the problem of high reflection in laser welding is solved, the welding efficiency and quality is improved, the mold life is extended, and the battery cell production cost is reduced.
Patent Information
- Application Number
- CN202410275971.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-12
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-03-12
AI Technical Summary
The existing connecting sheets have caused the welding equipment to be shut down due to high reflection problems during laser welding, which reduces welding quality and efficiency, and affects battery cell production.
A connecting piece is designed, which provides multiple indentation areas on the laser injection surface of the pole connecting part, and the indentation projection area and depth are between 0.04mm2≤S≤6mm2 and 0.1mm≤H≤0.5mm, and the pressure is The ratio of the trace area area to the laser injection surface area is between 35%≤N<80%, the spacing between the transverse and longitudinal directions is between 0.2mm≤X≤2mm and 0.2mm≤Y≤2mm, and the side wall is sandwiched with the laser injection surface. The angle is 45°≤Z≤85° to reduce high reflectance.
It effectively improves the energy absorption rate of the laser beam, avoids downtime of welding equipment, improves welding efficiency and quality, extends the service life of the mold, reduces production costs, and improves battery cell production efficiency and pass rate.
Smart Images

Figure CN117878540B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of power batteries, and in particular to a connecting sheet. The present invention also relates to a battery cell provided with the connecting sheet. Background Art
[0002] The connecting piece in the prior art is connected to the pole and the pole ear respectively, wherein the connecting piece is connected to the bottom plate of the pole by laser welding. Since the connecting piece is usually made of copper, when the laser beam is welding the connecting piece to the bottom plate of the pole, the laser beam directed to the connecting piece will have a high reflection (reflection) problem, so that part of the energy emitted by the laser beam is less absorbed by the connecting piece, which will reduce the penetration depth of the laser beam and reduce the welding quality and efficiency, resulting in poor welding effect between the negative electrode connecting piece and the pole. When the high reflection problem is serious, the welding equipment will shut down, making it impossible to weld the connecting piece, thereby affecting the production rhythm and production efficiency of the battery cell. Summary of the invention
[0003] In view of this, the present invention aims to provide a connecting sheet to improve the energy absorption rate of the laser beam and the laser welding efficiency.
[0004] To achieve the above object, the technical solution of the present invention is achieved as follows:
[0005] A connecting piece, comprising a pole ear connecting part and a pole connecting part which are connected to each other;
[0006] The pole connection part has a first welding surface connected to the pole welding, and a laser incident surface arranged opposite to the first welding surface, and an indentation area with multiple indentations is provided on the laser incident surface, and the projection area S of each indentation in the thickness direction of the pole connection part satisfies: 0.04mm 2 ≤S≤6mm 2 , the depth H of each indentation satisfies: 0.1mm≤H≤0.5mm; the area Q of the indentation region, the area M of the laser entrance surface, and the ratio N of the area Q of the indentation region to the area M of the laser entrance surface satisfy: 35%≤N<80%.
[0007] Furthermore, a lateral spacing X between two adjacent indentations in the width direction of the laser incident surface satisfies: 0.2 mm ≤ X ≤ 2 mm;
[0008] A longitudinal distance Y between two adjacent indentations in the length direction of the laser incident surface satisfies: 0.2 mm ≤ Y ≤ 2 mm.
[0009] Furthermore, an angle Z between the side wall of the indentation and the laser incident surface satisfies: 45°≤Z≤85°.
[0010] Furthermore, the cross-section of the indentation is at least one of square, circular, trapezoidal or triangular.
[0011] Further, the pole lug connection portion is in a "U" shape, and relative to the "U"-shaped opening, the pole connection portion is connected to the other end of the pole lug connection portion; and / or,
[0012] The tab connection portion has a second welding surface connected to the tab by welding. Relative to the second welding surface, the indentation area is also provided on the other side of the tab connection portion. The tab connection portion is connected to the tab by laser welding.
[0013] Furthermore, the pole connecting portion and the pole lug connecting portion are integrally formed; and / or,
[0014] The pole connecting part and the pole lug connecting part are both made of copper.
[0015] Furthermore, the pole connecting portion and the pole lug connecting portion are arranged on the same plane, or,
[0016] The pole connecting part and the pole lug connecting part are staggered and arranged at intervals up and down, and the pole connecting part is connected to the pole lug connecting part through an inclined connecting rib.
[0017] Further, the spacing distance L between the pole connection part and the lug connection part satisfies: L≥4mm; and / or,
[0018] The inclination angle α of the connecting rib satisfies: 0°<α<90°.
[0019] Compared with the prior art, the present invention has the following advantages:
[0020] The connecting piece of the present invention is provided with an indentation area having a plurality of indentations on the laser incident surface on the pole connecting part, and the projection area S of the indentations in the thickness direction of the pole connecting part satisfies: 0.04mm 2 ≤S≤6mm 2 The depth H of each indentation satisfies: 0.1mm≤H≤0.5mm, which is conducive to reducing the high reflection problem of the laser beam and effectively avoiding the shutdown of the welding equipment, thereby increasing the absorption rate of the pole connection part to the laser beam energy, and can effectively prevent the high reflection problem of the connecting piece during the laser welding process, thereby improving the efficiency and quality of laser welding, and then improving the assembly safety and reliability of the connecting piece, as well as the production efficiency, and also helping to reduce the production cost of the battery cell. At the same time, the setting of the projection area and depth of the indentation is also conducive to reducing the wear of the mold used for forming the indentation area, which is conducive to extending the service life of the mold and further reducing the production cost.
[0021] In addition, by setting the range of the lateral spacing X and the longitudinal spacing Y between two adjacent indentations, it is beneficial to arrange the indentations reasonably, thereby further reducing the occurrence of the laser beam high reflection problem. The setting of the range of the ratio N of the area Q of the indentation area to the area M of the laser entrance surface is beneficial to reducing the high reflection. The setting of the range of the angle Z between the side wall of the indentation and the laser entrance surface is beneficial to further prevent high reflection, and can increase the absorption effect of the laser beam energy. The cross section of the indentation is at least one of square, circular, trapezoidal or triangular, which is easy to process and shape, and has a good effect in preventing reflection.
[0022] In addition, the shape of the pole lug connection part is conducive to the connection with the pole lug, and the structure is simple and easy to process and form; the pole lug connection part is also connected to the pole lug by welding through the indentation area, and has good welding quality. The pole column connection part and the pole lug connection part are integrally formed, which is conducive to improving the processing efficiency of the connecting piece; the copper pole lug connection part and the pole column connection part are conducive to improving the electrical performance of the connecting piece. The pole column connection part and the pole lug connection part are coplanar or staggered and spaced apart, which can meet the use requirements of different battery cells. The setting of the spacing distance range between the pole column connection part and the pole lug connection part, as well as the setting of the inclination angle of the connecting rib, are conducive to improving the performance of the connecting piece.
[0023] In addition, another object of the present invention is to provide a battery cell, which includes the connecting sheet as described above.
[0024] The battery cell of the present invention is advantageously provided with the connecting sheet as described above to improve the production efficiency and qualified rate of the battery cell. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the accompanying drawings:
[0026] Figure 1 This is a schematic structural diagram of the first connecting sheet according to an embodiment of the present invention at a first viewing angle;
[0027] Figure 2 This is a schematic structural diagram of the first connecting sheet according to an embodiment of the present invention at a second viewing angle;
[0028] Figure 3 It is a partial structural schematic diagram of the indentation area according to an embodiment of the present invention;
[0029] Figure 4 A schematic diagram of the positions of the horizontal spacing and the vertical spacing according to an embodiment of the present invention;
[0030] Figure 5It is a schematic diagram of the position of the indentation depth and the angle Z according to an embodiment of the present invention;
[0031] Figure 6 This is a schematic structural diagram of a second connecting sheet according to an embodiment of the present invention;
[0032] Figure 7 It is a schematic structural diagram of the third connecting piece described in an embodiment of the present invention.
[0033] Description of reference numerals:
[0034] 1. Pole connection part; 2. Pole ear connection part;
[0035] 100, indentation area; 101, laser incident surface; 102, connecting rib; 103, indentation;
[0036] 201. Second welding surface. DETAILED DESCRIPTION
[0037] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.
[0038] In the description of the present invention, it should be noted that if there are terms indicating orientation or positional relationship such as "upper", "lower", "inner", "back", etc., they are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, if there are terms such as "first", "second", etc., they are also used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.
[0039] The present invention will be described in detail below with reference to the accompanying drawings and in conjunction with embodiments.
[0040] This embodiment relates to a connecting piece, which aims to reduce the reflection problem of the laser beam by optimizing the structure of the connecting piece, thereby improving the energy absorption rate of the laser beam and the laser welding efficiency.
[0041] In terms of overall structure, the connecting piece includes a pole lug connecting portion 2 and a pole connecting portion 1 which are connected to each other. The pole connecting portion 1 has a first welding surface connected to the pole by welding, and a laser incident surface 101 which is arranged opposite to the first welding surface, and an indentation area 100 having a plurality of indentations 103 is arranged on the laser incident surface 101. The projection area S of each indentation 103 in the thickness direction of the pole connecting portion 1 satisfies: 0.04mm 2 ≤S≤6mm 2 , the depth H of each indentation 103 satisfies: 0.1mm≤H≤0.5mm.
[0042] The connecting piece of this embodiment is provided with a plurality of indentations 103 on the laser incident surface 101 on the pole connecting portion 1, and the projection area S of the indentations 103 in the thickness direction of the pole connecting portion 1 satisfies: 0.04 mm 2 ≤S≤6mm 2 The depth H of each indentation 103 satisfies: 0.1mm≤H≤0.5mm, which is conducive to reducing the reflection problem of the laser beam and effectively avoiding the shutdown of the welding equipment, thereby improving the absorption rate of the pole connecting part 1 to the laser beam energy, which is not only conducive to improving the laser welding efficiency, but also conducive to improving the laser welding quality, thereby improving the assembly safety and reliability of the connecting piece, as well as the production efficiency, and also conducive to reducing the production cost of the battery cell.
[0043] At the same time, by setting the range of the projection area S and the depth H of the indentation 103, it is also beneficial to reduce the wear of the molding die in the indentation area 100, thereby extending the service life of the die and further reducing the production cost.
[0044] Based on the overall introduction above, an exemplary structure of the connecting sheet in this embodiment is as follows: Figure 1 and Figure 2 As shown in . The indentations 103 in this embodiment are arranged in multiple rows along the length direction and the width direction of the pole connection part 1, and the above-mentioned indentation area 100 is formed on the laser incident surface 101. The indentation area 100 here extends from the free end of the laser incident surface 101 to the other end, and a gap is formed between the indentation area 100 and the pole lug connection part 2. It can be understood that in specific implementation, the range of the indentation area 100 can also be adaptively adjusted according to the use requirements.
[0045] In addition, if Figure 5 As shown in FIG. 1 , the depth H of the indentation 103 refers to the distance between the bottom surface of the indentation 103 and the laser incident surface 101. In a specific implementation, the projection area S of the indentation 103 in the thickness direction of the pole connecting part 1 can be 0.04 mm. 2 , 0.1mm 2 , 1mm 2 , 2mm 2 , 3mm 2 , 4mm 2 , 5mm 2 , 5.5mm 2 or 6mm 2 The depth H of the indentation 103 may be 0.1 mm, 0.2 mm, 0.3 mm, 0.4 mm or 0.5 mm. In this embodiment, the projection area range and depth range of the indentation 103 are both conducive to improving the problem of high reflectivity of the laser beam, thereby avoiding the problem of shutdown of the welding equipment due to high reflectivity, and further facilitating the welding efficiency of the connecting piece.
[0046] It should be noted that the projection area S of the indentation 103 in the thickness direction of the pole connecting part 1 in this embodiment specifically refers to the area of the outer contour of the indentation 103 projected from top to bottom along the thickness direction of the pole connecting part 1 .
[0047] In this embodiment, the two numerical ranges of the projected area S of the indentation 103 in the thickness direction of the pole connecting part 1 and the depth H of the indentation 103 cooperate with each other from the two aspects of area and depth to reduce the problem of laser beam reflection, so that more energy of the laser beam is absorbed by the pole connecting part 1, so that the energy is sufficient to cause the contact area between the welded bottom plate and the pole connecting part 1 to melt, thereby welding the first welding surface and the bottom plate of the pole together.
[0048] Specifically, when the projection area S of the indentation 103 is less than 0.04 mm 2 When the depth H of the indentation 103 is less than 0.1 mm, the welding equipment is still prone to shutdown, indicating that the setting of the indentation area and depth at this time cannot improve the high-reflection problem. At the same time, the specifications of the indentation 103 are small, so the specifications of the pressure head corresponding to each indentation 103 on the mold required for the stamping of the indentation 103 are also small, which will cause the mold to be prone to wear during use, thereby shortening the life of the mold. The production cost of the stamping mold is high. When the mold cannot be used due to wear, a new mold needs to be used, which will increase the production cost.
[0049] At the same time, when the projection area S of the indentation 103 is greater than 6 mm 2 When the depth H of the indentation 103 is greater than 0.5 mm, the welding equipment is still prone to shutdown, indicating that the setting of the indentation area and depth cannot improve the high-reflection problem. At the same time, the thickness of the indentation area 100 is significantly reduced, making the structural strength here low, and it is also prone to heat generation, which is not conducive to the safety of the connection piece.
[0050] like Figure 4 As shown in , the lateral spacing X between two adjacent indentations 103 in the width direction of the laser incident surface 101 satisfies: 0.2mm≤X≤2mm; the longitudinal spacing Y between two adjacent indentations 103 in the length direction of the laser incident surface 101 satisfies: 0.2mm≤Y≤2mm. In specific implementation, the lateral spacing X and the longitudinal spacing Y can be 0.2mm, 0.5mm, 0.8mm, 1mm, 1.5mm or 2mm. By setting the range of the lateral spacing X and the longitudinal spacing Y to between 0.2mm and 2mm, it is beneficial to improve the anti-high-reflection effect of the indentations 103 cooperating with each other.
[0051] In this embodiment, when the values of the transverse spacing X and the longitudinal spacing Y are both less than 0.2 mm, the density of the indentation 103 will be relatively high, which will have a greater impact on the structural strength of the pole connection part, thereby affecting the connection strength after the connection piece and the pole are welded, which is not conducive to the safety of the battery cell. When the values of the transverse spacing X and the longitudinal spacing Y are both greater than 2 mm, the density of the indentation 103 will be relatively low, and the indentation area 100 will not have a good improvement effect on the reflection of the laser beam.
[0052] As a preferred embodiment, the area Q of the indentation region 100, the area M of the laser incident surface, and the ratio N of the area Q of the indentation region 100 to the area M of the laser incident surface 101 satisfy: 35%≤N≤95%. For example, N may be 35%, 45%, 55%, 75%, 76%, 78%, 79%, 80%, 85%, 88%, 89%, 90%, 92% or 95%. Here, by setting the range of the ratio N of the area Q of the indentation region 100 to the area M of the laser incident surface 101, the anti-high-reflection effect of the indentation region 100 is better, and the absorption efficiency of the laser beam energy is high.
[0053] When the ratio N is less than 35%, it means that the area of the indentation region 100 is relatively low, and the improvement effect of the indentation region 100 on the reflection problem is not obvious, which is not conducive to the welding of the connecting piece and the pole. When the ratio N is greater than 95%, it means that the area of the indentation region 100 is relatively high, which will cause the indentation region 100 to have redundant functions and low utilization rate, which is not conducive to reducing production costs.
[0054] Reference Figure 5 As shown in , in this embodiment, the angle Z between the side wall of the indentation 103 and the laser incident surface 101 satisfies: 45°≤Z≤85°. For example, the angle Z may be 45°, 55°, 65°, 75°, 80° or 85°. By setting the angle range between the side wall of the indentation 103 and the laser incident surface 101, the side walls of the indentation 103 are all inclined, which is conducive to strengthening the anti-reflection effect of the indentation 103, and the structure of the indentation 103 is simple and easy to process. When the angle A is less than 45°, or greater than 85°, the anti-reflection effect of the side wall on the laser beam is not ideal, and the welding equipment is still prone to shutdown, and the problem of poor welding effect caused by the high reflection of the laser beam.
[0055] In addition, in this embodiment, the indentation 103 is formed by the indenter pressing down the laser incident surface 101, so the shape of the indentation 103 depends on the shape of the indenter on the stamping die. As a preferred structural example, the cross section of the indentation 103 is at least one of square, circular, trapezoidal or triangular. It should be noted that the cross section of the indentation 103 is arranged parallel to the laser incident surface 101. Figure 3As shown in , the cross section of the indentation 103 in this embodiment is square, which is formed by punching a plurality of square indenters. Here, the side length a of each indentation 103 satisfies: 0.2mm≤a≤2mm, for example, the side length a can be 0.2mm, 0.4mm, 0.6mm, 1mm, 1.5mm, 2mm or 2.5mm, etc. Here, the cross section of the indentation 103 is square, which has the advantages of simple structure, good uniformity, and good anti-reflection effect.
[0056] It is understandable that, in addition to being square, the cross section of the indentation 103 in this embodiment may also be circular or triangular. When the cross section of the indentation 103 is circular, the indenter is cylindrical or conical. When the cross section of the indentation 103 is triangular, the indenter may be prismatic. Of course, in specific implementation, the cross section of the indentation 103 may also be other geometric shapes, or a combination of multiple shapes, as long as the use requirements are met.
[0057] In order to more intuitively reflect the welding effect of the connecting piece in this embodiment, laser welding tests are performed on connecting pieces with different characteristics, and the experimental results are shown in Tables 1 and 2. As can be seen from Tables 1 and 2, in Samples 2, 5, 6, and 8, the projection area S of the indentation 103 meets 0.04 mm 2 ≤S≤6mm 2 , the depth H of the indentation 103 satisfies: 0.1mm≤H≤0.5mm, the lateral spacing X satisfies: 0.2mm≤X≤2mm; the longitudinal spacing Y satisfies: 0.2mm≤Y≤2mm. The ratio N of the area Q of the indentation region 100 to the area M of the laser incident surface 101 satisfies: 35%≤N<90%. The angle Z between the side wall of the indentation 103 and the laser incident surface 101 satisfies: 45°≤Z≤85°. Therefore, when laser welding was performed on samples 2, 5, 6 and 8, the welding equipment did not have any shutdown problems, and continuous welding of the connecting pieces was achieved, with high welding efficiency and good welding effect, and the welding results were all qualified.
[0058] In this embodiment, the projected area S of the indentation 103 in the sample 1 is less than 0.04 mm 2 , the projected area S of the indentation 103 in sample 9 is greater than 6 mm 2 , the ranges of other parameters meet the requirements, but the welding equipment has a shutdown problem, so the projection area S is less than 0.04mm 2 Or larger than 6mm 2None of them can solve the problem of laser beam reflection, resulting in poor welding effects of samples 1 and 9. Among the parameters of samples 3 and 4, only one of the horizontal spacing X and the vertical spacing Y is less than 0.2mm, and among the parameters of samples 12 and 13, only one of the horizontal spacing X and the vertical spacing Y is greater than 2mm, and the ranges of other parameters meet the requirements. At this time, the problem of laser beam reflection is still serious, the welding equipment has a shutdown problem, and the welding effect is still not ideal.
[0059] Among the parameters of sample 7, only the angle Z is greater than 80°, and the angle Z of sample 10 is less than 45°. The ranges of other parameters meet the requirements. However, at this time, the welding equipment has a shutdown problem. Obviously, when the value of angle Z is not within the set reasonable range, the welding effects of samples 7 and 10 are still unqualified. Among the parameters of sample 11, only the depth H of indentation 103 is less than 0.1mm, and in sample 14, only the depth H of indentation 103 is greater than 0.5mm. The ranges of other parameters meet the requirements. At this time, the laser welding effect of the laser beam is still not ideal, the welding equipment is still shut down, and when the depth H of indentation 103 is less than 0.1mm, the structural strength of the indentation area 100 on the connecting piece is low, resulting in the welding of samples 11 and 14 still unqualified.
[0060] In addition, the area ratio N of sample 15 is less than 35%, and the area ratio N of sample 16 is greater than 95%. Other parameters meet the requirements. At this time, the welding results of the two samples are still unqualified, and the problem of welding equipment shutdown also occurs. At the same time, the area ratio N of sample 16 is greater than 95%, which also makes the utilization rate of the indentation area 100 low.
[0061] In addition, the qualified samples solved the reflection problem during welding, improved the absorption efficiency of laser energy, and helped solve the problem of welding equipment shutdown, which was conducive to the continuous operation of welding equipment, thereby improving welding efficiency and effect. However, the unqualified samples did not solve the reflection problem during welding, which caused the laser welding equipment to shut down during operation, seriously affecting the production rhythm and was not conducive to the production of battery cells.
[0062] like Figure 1 As shown in the figure, in the first structural form of the connecting piece, the pole lug connecting portion 2 is in a "U" shape, and relative to the "U"-shaped opening, the pole connecting portion 1 is connected to the other end of the pole lug connecting portion 2. In this embodiment, the pole connecting portion 1 is specifically welded to the bottom plate of the pole, and the width of the pole connecting portion 1 is smaller than the width of the pole lug connecting portion 2. In specific implementation, the specifications and shapes of the pole lug connecting portion 2 and the pole connecting portion 1 can be determined according to the use requirements.
[0063] Still refer to Figure 1As shown in the figure, the pole connection part 1 and the tab connection part 2 in this embodiment are staggered and arranged at intervals, and the pole connection part 1 is connected to the tab connection part 2 through an inclined connection rib 102, that is, the tab connection part 2 and the pole connection part 1 are not arranged on the same plane. The structure of the connecting piece here is simple, easy to process and shape, and has a good use effect.
[0064] As a preferred embodiment, the spacing distance L between the pole connection part and the lug connection part satisfies: L ≥ 4 mm. For example, the spacing distance can be 4 mm, 4.5 mm or 5 mm, etc., which can be determined according to the use requirements. The inclination angle α of the connecting rib satisfies: 0°<α<90°, for example, the inclination angle α can be 30°, 60° or 80°, etc., which can also be determined according to the use requirements during specific implementation.
[0065] It is understandable that the solution of arranging the pole connection part 1 and the pole lug connection part 2 in the same plane is also feasible, in which case there is no need to arrange the inclined connection rib 102. In addition, the pole connection part 1 and the pole lug connection part 2 in this embodiment are preferably integrally formed, and both can be made of copper and stamped by a stamping die. This is conducive to improving the processing efficiency of the connecting piece, and the connecting piece has good structural strength and electrical performance. In addition, the second structure of the connecting piece in this embodiment is as follows Figure 6 As shown in the figure, at this time, the connecting piece of the whole vehicle is L-shaped, which can also meet the connection requirements between the pole ear and the pole.
[0066] The tab connection part 2 in this embodiment is connected to the tab by welding through the second welding surface 201. As a preferred method, the second welding surface 201 of the tab connection part 2 is connected to the tab by ultrasonic welding or laser welding. In order to improve the quality of the connecting piece, the scratch roughness on the first welding surface and the second welding surface 201 preferably meets the following conditions: Ra≤1.0μm, Rz≤16μm. Among them, Ra is from the roughness level of the scratch, and Rz is from the scratch depth to define the conditions that the first welding surface and the second welding surface 201 need to meet.
[0067] In addition, in this embodiment, the length of the scratches on both the first welding surface and the second welding surface 201 does not exceed 1 / 3 of their own length. In this embodiment, the welding areas of the first welding surface and the second welding surface 201 are not allowed to bend. In specific implementation, the flatness of the first welding surface and the second welding surface 201 both meet: ⊥≤0.1mm. For example, the flatness of the first welding surface and the second welding surface 201 is 0.02mm, 0.05mm, 0.08mm or 0.1mm, etc.
[0068] In addition, the hardness requirement of the connecting piece in this embodiment is HV55-65, which is conducive to improving the welding strength. In specific implementation, the oxidation area on the connecting piece should be less than one-third of its own area. After the connecting piece is welded and assembled, the burr direction of its edges should be away from the pole group setting.
[0069] It should be noted that the connecting piece in this embodiment can be Figure 1 and Figure 6 In addition to the structural form shown in Figure 7 Specifically, the connecting piece is rectangular, and the pole connecting part 1 and the tab connecting part 2 are respectively arranged at both ends of the connecting piece. The tab connecting part 2 has a second welding surface connected to the tab by welding, and relative to the second welding surface, an indentation area 100 is also provided on the other side of the tab connecting part 2, and the tab connecting part 2 is connected to the tab by laser welding.
[0070] Among them, there are two indentation areas 100 arranged at intervals on the pole connection part 1, and there is one indentation area 100 on the pole ear connection part 2. The area, specification and quantity of each indentation area 100 can be adjusted according to the use requirements. In specific implementation, the connecting piece can be applied to a long blade battery, and folded after being welded to the pole and the pole ear respectively, so as to achieve installation on the battery cell. The connecting piece in this embodiment can be adjusted according to the use requirements of different types of battery cells to have a better range of applications.
[0071] This embodiment helps to ensure the product quality of the connecting piece by optimizing the production technology requirements, material requirements and appearance quality requirements of the connecting piece, and effectively prevents the occurrence of problems such as burn points, cold welds, laser welding reflections, and production assembly interference in the production welding process of the connecting piece, thereby helping to improve the safety and reliability of the connecting piece assembly, and helping to improve production efficiency and reduce the production cost of the battery cell.
[0072] In this embodiment, the specifications of the indentation 103 are specially set to alleviate the problem of obvious reflection after the laser beam is shot toward the laser entrance surface 101 during laser welding, thereby helping to increase the penetration depth of the laser beam, and improve the efficiency of the pole bottom plate and the first welding surface during the welding process, and also help to improve the welding quality between the pole and the connecting piece.
[0073] Table 1: Experimental results of samples 1 to 8 (area in mm 2 , the unit of spacing is mm, NG represents failure, OK represents passing).
[0074]
[0075] Table 2: Experimental results of samples 9 to 15 (where the unit of area is mm 2, the unit of spacing is mm, NG represents failure, OK represents passing).
[0076]
[0077] In addition, this embodiment relates to a battery cell, which includes the above-mentioned connecting piece. The battery cell of this embodiment is provided with the above-mentioned connecting piece, which is beneficial to improving the production efficiency and qualified rate of the battery cell.
[0078] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A connecting piece, Features: It comprises a pole lug connection part (2) and a pole connection part (1) which are connected to each other; The pole connection part (1) has a first welding surface connected to the pole by welding, and a laser incident surface (101) arranged opposite to the first welding surface, and an indentation area (100) having a plurality of indentations (103) is stamped on the laser incident surface (101), and a projection area S of each indentation (103) in the thickness direction of the pole connection part (1) satisfies: 0.04 mm 2 ≤S≤6mm 2 , the depth H of each of the indentations (103) satisfies: 0.1 mm ≤ H ≤ 0.5 mm; The area Q of the indentation region (100), the area M of the laser incident surface (101), and the ratio N of the area Q of the indentation region (100) to the area M of the laser incident surface (101) satisfy: 35%≤N<80%; A lateral spacing X between two adjacent indentations (103) in the width direction of the laser incident surface (101) satisfies: 0.2 mm ≤ X ≤ 2 mm; A longitudinal distance Y between two adjacent indentations (103) in the length direction of the laser incident surface (101) satisfies: 0.2 mm ≤ Y ≤ 2 mm; The bottom wall of the indentation (103) is arranged parallel to the laser incident surface (101), and the angle Z between the side wall of the indentation (103) and the bottom wall of the indentation (103) satisfies: 45°≤Z≤85°; The pole connecting portion (1) and the pole lug connecting portion (2) are both made of copper.
2. The connecting sheet according to claim 1, Features: The cross section of the indentation (103) is at least one of square, circular, trapezoidal or triangular; and / or the flatness of the first welding surface and the second welding surface (201) both satisfy: ⊥≤0.1 mm.
3. The connecting sheet according to claim 1, Features: The pole lug connection portion (2) is in a "U" shape, and the pole connection portion (1) is connected to the other end of the pole lug connection portion (2) relative to the opening of the "U" shape; and / or, The tab connection portion (2) has a second welding surface (201) connected to the tab by welding, and the indentation area (100) is also provided on the other side of the tab connection portion (2) relative to the second welding surface (201), and the tab connection portion (2) is connected to the tab by laser welding.
4. The connecting sheet according to claim 1, Features: The pole connecting portion (1) and the pole lug connecting portion (2) are integrally formed, and / or, The hardness requirement of the connecting piece is HV55-65.
5. The connecting sheet according to claim 1, Features: The pole connecting portion (1) and the pole lug connecting portion (2) are arranged in the same plane, or, The pole connecting portion (1) and the pole lug connecting portion (2) are staggered and arranged at intervals up and down, and the pole connecting portion (1) is connected to the pole lug connecting portion (2) via an inclined connecting rib (102).
6. The connecting sheet according to claim 5, Features: The spacing distance L between the pole connecting portion (1) and the tab connecting portion (2) satisfies: L ≥ 4 mm; and / or, The inclination angle α of the connecting rib (102) satisfies: 0°<α<90°.
7. The connecting sheet according to claim 2, Features: The scratch roughness on the first welding surface and the second welding surface (201) satisfies: Ra≤1.0μm, Rz≤16μm.
8. A battery cell, Features: The battery cell comprises the connecting sheet according to any one of claims 1 to 7.