Travertine permeable concrete doped with powdered waste and preparation method thereof
By using powder waste to replace cement in travertine permeable concrete, the impact of traditional concrete materials on the environment and water resource management problems are solved, efficient resource utilization and low-carbon goals are achieved, and the design requirements of permeable concrete are met.
Patent Information
- Application Number
- CN202410106734.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-25
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-01-25
AI Technical Summary
Traditional non-permeable concrete causes rainfall to fail to penetrate underground quickly, resulting in waterlogging and waste of water resources. The preparation of traditional building materials consumes a lot of resources and has an impact on the environment. A sustainable permeable concrete material is needed to solve these problems.
Travertine permeable concrete doped with powder waste is used to replace concrete raw material cement through powder waste, reducing cement usage, improving resource utilization efficiency, and ensuring the compressive strength and permeability of concrete through specific mixing sequence and raw material ratio.
It realizes the recycling of powder waste, reduces cement consumption and carbon dioxide emissions, meets the design requirements of permeable concrete pavement, has good compressive strength and permeable properties, and supports environmental sustainable development.
Smart Images

Figure CN117886573B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of concrete materials, in particular to a travertine permeable concrete doped with powdered waste and a preparation method thereof. Background Art
[0002] As the global urban population grows and urbanization accelerates, cities face more water resource management challenges. Traditional non-permeable concrete prevents rainwater from quickly penetrating into the ground, leading to waterlogging and water waste. Climate change has triggered more frequent and intense rainfall events. Cities lack effective drainage systems to cope with these extreme weather conditions, making the problem of waterlogging more serious. In addition, strengthening environmental protection has become a global consensus, and buildings and infrastructure also need to develop in a more sustainable and eco-friendly direction.
[0003] Permeable concrete, also known as porous concrete, is a type of concrete with high water permeability. It contains tiny gaps and pore structures inside, allowing rainwater to quickly penetrate the concrete surface into the ground, achieving the purpose of natural recharge of groundwater by rainwater. Permeable concrete can effectively reduce urban surface runoff, alleviate urban waterlogging problems, and improve the city's ecological environment.
[0004] In traditional construction projects, ordinary concrete with natural aggregates is often used as the main building material, but the preparation of this material consumes a lot of resources and has a certain impact on the environment. In order to achieve sustainable development and protect the environment, recycled aggregate permeable concrete came into being. Recycled aggregates can effectively replace traditional natural aggregates, reduce the cost of building materials and the degree of dependence on natural resources. At the same time, permeable concrete can improve the way urban rainwater is discharged and reduce the occurrence of urban waterlogging. This new building material has broad application prospects in urban planning and green buildings.
[0005] CN109665772A discloses a permeable concrete mixed with recycled concrete block aggregate and a preparation method thereof, wherein the recycled concrete block aggregate is used to replace the limestone aggregate in the permeable concrete, the recycled concrete block is crushed and screened to a suitable size, and mixed with silicate cement, superplasticizer and natural limestone aggregate to prepare permeable concrete that meets the engineering requirements. The permeable concrete integrates the functional advantages of recycled concrete and permeable concrete, and can not only solve the various problems brought to the environment and resources by the rapid growth of construction waste in the existing practice, but also can reuse the concrete block material, turn waste into treasure, and prepare a permeable pavement that meets the actual requirements. The permeable concrete prepared by this method has high compressive strength and permeability, and can fully meet the compressive strength requirements of the permeable pavement in the existing city and even the permeable pavement on the highway and the permeability requirements of most permeable pavements.
[0006] CN107151111A discloses a recycled aggregate permeable concrete, which is made from the following raw materials in parts by weight: 40-55 parts of waste concrete particles, 15-30 parts of modified waste tire particles, 17-35 parts of epoxy resin, 0.5-1.5 parts of modifier, 1-2.6 parts of cycloalkyl crude oil, 0.4-1 parts of triethylenetetramine, 0.2-0.8 parts of diglycidyl ether, and 1-2 parts of tributyl phosphate. The recycled aggregate permeable concrete uses recycled aggregate and waste tires prepared from waste concrete as raw materials. Under the premise of meeting the compressive strength and water permeability coefficient, it has a low elastic modulus, good flexibility, good antifreeze performance, low density, light weight, and is easy to transport and lay. The recycled aggregate permeable concrete realizes the recycling of waste concrete and waste tires, solves the problem of their accumulation and storage and occupying a large amount of land, and has practical significance such as turning waste into treasure, promoting resource reuse, and environmentally friendly management.
[0007] CN114804763A discloses a fiber-reinforced recycled aggregate permeable concrete, which is made of the following formula: cement 270-350kg / m 3 and 355-450kg / m 3 , water 100-155kg / m 3 , coarse aggregate 1360-1950kg / m 3 , recycled aggregate accounts for 35%-100%, polymer emulsion 0-30kg / m 3 , water reducing agent 0-9.6kg / m 3 , high performance admixture 0-5kg / m 3 , water-cement ratio 0.24-0.42, slurry-aggregate ratio 1:3.8-1:4.7, maximum nominal particle size of coarse aggregate 5-20mm, and the preparation of permeable concrete by recycled aggregate further reduce the carbon emissions of ground and road paving materials throughout their life cycle. At the same time, it effectively utilizes construction waste and solid waste. Through fiber reinforcement technology, the flexural strength and toughness of the permeable pavement layer are greatly improved. The breakthrough use of premixed production has greatly improved production efficiency and ensured the quality stability of permeable concrete products to a greater extent. Summary of the invention
[0008] In view of the problems existing in the prior art, the present invention provides a travertine permeable concrete doped with powdered waste and a preparation method thereof. By using powdered waste to partially replace cement, a raw material of concrete, not only the problem of waste travertine powder and limestone powder can be solved, but also the resource utilization efficiency can be improved, which is beneficial to environmental sustainable development; the travertine permeable concrete doped with powdered waste still has good compressive strength and permeability, and meets the design requirements of permeable concrete pavement.
[0009] To achieve this object, the present invention adopts the following technical solutions:
[0010] In a first aspect, the present invention provides a travertine permeable concrete doped with powdered waste, wherein the travertine permeable concrete doped with powdered waste comprises the following raw materials in weight ratio:
[0011] Water: cement: water reducing agent: silica fume: limestone: travertine: powdered waste = (79.7-125.6): (242.8-418.8): (2.4-3.7): (30-46.5): (1214-1216): (369-370): (14.6-78.9); the powdered waste includes travertine powder or limestone powder.
[0012] The travertine permeable concrete doped with powder waste of the present invention replaces the concrete raw material cement by doping with powder waste travertine powder or limestone powder, thereby greatly reducing the amount of cement and saving the concrete preparation cost, while still obtaining travertine permeable concrete that meets the use requirements. The travertine permeable concrete of the present invention realizes the recycling of powder waste and has good environmental benefits.
[0013] The travertine permeable concrete doped with powdered waste of the present invention comprises raw materials in the following weight ratio: water: cement: water reducing agent: silica fume: limestone: travertine: powdered waste = (79.7-125.6): (242.8-418.8): (2.4-3.7): (30-46.5): (1214-1216): (369-370): (14.6-78.9), for example, it can be 79.7: 242.8: 2.4: 30: 1214: 369: 14.6, 82: 256: 2.5:33:1214.3:369.5:18, 90:270:2.8:35:1214.5:369.8:22.6, 105:320:3:38:1215:369.9:50, 110:380:3.2:42:1215.5:369.9:60 or 125.6:418.8:3.7:46.5:1216:370:78.9, etc., but are not limited to the listed values, other values not listed within the numerical range are also applicable.
[0014] Preferably, the designed porosity of the travertine permeable concrete doped with powdered waste is 15-25%, for example, it can be 15%, 16%, 17%, 18%, 20%, 22% or 25%, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0015] Preferably, the cement comprises Portland cement.
[0016] Preferably, the strength grade of the cement is 42.5 and the density is 3110 kg / m3 .
[0017] Preferably, the water reducing agent comprises Sika high-efficiency water reducing agent.
[0018] Preferably, the water reducing agent has a water reducing rate of 20-25%, for example, 20%, 21%, 22%, 23%, 23.5%, 24% or 25%, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0019] Preferably, the particle size of the limestone is 5 to 10 mm, for example, 5 mm, 6 mm, 7 mm, 8 mm, 8.5 mm, 9 mm, 9.5 mm or 10 mm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0020] Preferably, the particle size of the travertine is 5 to 10 mm, for example, 5 mm, 6 mm, 7 mm, 8 mm, 8.5 mm, 9 mm, 9.5 mm or 10 mm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0021] Preferably, the particle size of the travertine powder is less than 250 μm, for example, it can be 249 μm, 240 μm, 230 μm, 220 μm, 210 μm, 200 μm, 190 μm or 150 μm, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0022] Preferably, the particle size of the limestone powder is less than 250 μm, for example, it can be 249 μm, 240 μm, 230 μm, 220 μm, 210 μm, 200 μm, 190 μm or 150 μm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0023] Preferably, the density of the travertine powder is 2640 kg / m 3 .
[0024] Preferably, the density of the limestone powder is 2930 kg / m 3 .
[0025] In a second aspect, the present invention further provides a method for preparing the travertine permeable concrete doped with powdered waste as described in the first aspect, the preparation method comprising the following steps:
[0026] (1) Pour limestone and travertine into a mixer and stir for 60 seconds;
[0027] (2) After adding half of the water reducer and half of the water, stir for 90 seconds;
[0028] (3) After adding cement, silica fume and powdered waste, stir for 90 seconds;
[0029] (4) Add the remaining water and water, stir for 90 seconds, and then discharge the material into a mold.
[0030] The preparation method of the present invention is simple to operate, and various raw materials are added in a specific order and mixed by a forced mixer to achieve uniform mixing of the raw materials. In step (2), only half of the water reducer and half of the water are added, and then in step (3), cement, silica fume and powder waste are added, and in step (4), the remaining water reducer and the remaining water are added. Such mixing steps have the advantage of allowing cement and other cementitious materials to be better wrapped on the aggregate.
[0031] Compared with the prior art, the present invention has at least the following beneficial effects:
[0032] The travertine permeable concrete doped with powdered waste provided by the present invention adopts powdered waste travertine powder or limestone powder to partially replace cement as a cementitious material to prepare permeable concrete, thereby reducing the amount of cement used and reducing the overall carbon dioxide emissions, while realizing the recycling and reuse of powdered waste and achieving the goal of environmental sustainable development; the travertine permeable concrete doped with powdered waste still has excellent compressive strength and permeability, and can meet the design requirements of permeable concrete. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a diagram of the final shape of the travertine permeable concrete mixed with powdered waste after compressive crushing in Example 1 of the present invention.
[0034] Figure 2 This is a diagram of the final shape of the travertine permeable concrete mixed with powdered waste after compressive crushing in Example 2 of the present invention.
[0035] Figure 3 This is a diagram of the final morphology of the travertine permeable concrete after compressive crushing in Comparative Example 1 of the present invention.
[0036] Figure 4 It is a graph showing the compressive strength and water permeability coefficient of the travertine permeable concrete mixed with powdered waste in Examples 1 and 2 of the present invention and the travertine permeable concrete in Comparative Example 1.
[0037] Figure 5 It is a graph showing the compressive strength and water permeability coefficient of the travertine permeable concrete mixed with powdered waste in Examples 3 to 6 of the present invention and the travertine permeable concrete in Comparative Example 1.
[0038] Figure 6It is a graph showing the compressive strength and water permeability coefficient of the travertine permeable concrete mixed with powdered waste in Examples 7 to 10 of the present invention and the travertine permeable concrete in Comparative Example 1. DETAILED DESCRIPTION
[0039] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.
[0040] The present invention is further described in detail below. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.
[0041] Example 1
[0042] This embodiment provides a travertine permeable concrete doped with powdered waste, wherein the travertine permeable concrete doped with powdered waste comprises the following raw materials in weight ratio:
[0043] Water: cement: water reducing agent: silica fume: limestone: travertine: powdered waste = 102.5: 327.1: 3.0: 38.3: 1215: 369.7: 14.6; the powdered waste includes travertine powder.
[0044] The designed porosity of the travertine permeable concrete doped with powder waste is 20%.
[0045] The cement includes silicate cement; the strength grade of the cement is 42.5 and the density is 3110kg / m 3 .
[0046] The water reducing agent includes Sika high-efficiency water reducing agent; the water reducing rate of the water reducing agent is 20%.
[0047] The particle size of the limestone is 5 to 10 mm; the particle size of the travertine is 5 to 10 mm.
[0048] The particle size of the travertine powder is less than 250 μm. The density of the travertine powder is 2640 kg / m 3 .
[0049] This embodiment also provides a method for preparing the above-mentioned travertine permeable concrete doped with powdered waste, the preparation method comprising the following steps:
[0050] (1) Pour limestone and travertine into a mixer and stir for 60 seconds;
[0051] (2) After adding half of the water reducer and half of the water, stir for 90 seconds;
[0052] (3) After adding cement, silica fume and powdered waste, stir for 90 seconds;
[0053] (4) Add the remaining water and water, stir for 90 seconds, and then discharge the material into a mold.
[0054] Example 2
[0055] This embodiment provides a travertine permeable concrete doped with powdered waste, wherein the travertine permeable concrete doped with powdered waste comprises the following raw materials in weight ratio:
[0056] Water: cement: water reducing agent: silica fume: limestone: travertine: powdered waste = 79.7: 242.8: 2.4: 30.0: 1215: 369.7: 22.9; the powdered waste includes travertine powder.
[0057] The designed porosity of the travertine permeable concrete doped with powder waste is 25%.
[0058] The cement includes silicate cement; the strength grade of the cement is 42.5 and the density is 3110kg / m 3 .
[0059] The water reducing agent includes Sika high-efficiency water reducing agent; the water reducing rate of the water reducing agent is 22%.
[0060] The particle size of the limestone is 5 to 10 mm; the particle size of the travertine is 5 to 10 mm.
[0061] The particle size of the travertine powder is less than 250 μm. The density of the travertine powder is 2640 kg / m 3 .
[0062] This embodiment also provides a method for preparing the above-mentioned travertine permeable concrete doped with powdered waste, and the preparation method is the same as that in Example 1.
[0063] The final shape of the travertine permeable concrete mixed with powder waste in Example 1 after compressive crushing is shown in the figure below. Figure 1 The final shape of the travertine permeable concrete mixed with powder waste in Example 2 after compressive crushing is shown in FIG. Figure 2 As shown in the figure, it can be seen that as the designed porosity gradually increases, the amount of cement used decreases, and there is not enough cementitious material to fill the travertine permeable concrete, resulting in an increase in the pores inside the permeable concrete.
[0064] Example 3
[0065] This embodiment provides a travertine permeable concrete doped with powdered waste, wherein the travertine permeable concrete doped with powdered waste comprises the following raw materials in weight ratio:
[0066] Water: cement: water reducing agent: silica fume: limestone: travertine: powdered waste = 125.6: 397.9: 3.7: 46.5: 1215: 369.7: 17.8; the powdered waste includes travertine powder.
[0067] The designed porosity of the travertine permeable concrete doped with powdered waste is 15%, and the rest is the same as that of Example 1.
[0068] This embodiment also provides a method for preparing the above-mentioned travertine permeable concrete doped with powdered waste, and the preparation method is the same as that in Example 1.
[0069] Example 4
[0070] This embodiment provides a travertine permeable concrete doped with powdered waste, wherein the travertine permeable concrete doped with powdered waste comprises the following raw materials in weight ratio:
[0071] Water: cement: water reducing agent: silica fume: limestone: travertine: powdered waste = 125.6: 376.9: 3.7: 46.5: 1215: 369.7: 35.6; the powdered waste includes travertine powder.
[0072] The designed porosity of the travertine permeable concrete doped with powdered waste is 15%, and the rest is the same as that of Example 1.
[0073] This embodiment also provides a method for preparing the above-mentioned travertine permeable concrete doped with powdered waste, and the preparation method is the same as that in Example 1.
[0074] Example 5
[0075] This embodiment provides a travertine permeable concrete doped with powdered waste, wherein the travertine permeable concrete doped with powdered waste comprises the following raw materials in weight ratio:
[0076] Water: cement: water reducing agent: silica fume: limestone: travertine: powdered waste = 125.6: 356.0: 3.7: 46.5: 1215: 369.7: 53.3; the powdered waste includes travertine powder.
[0077] The designed porosity of the travertine permeable concrete doped with powdered waste is 15%, and the rest is the same as that of Example 1.
[0078] This embodiment also provides a method for preparing the above-mentioned travertine permeable concrete doped with powdered waste, and the preparation method is the same as that in Example 1.
[0079] Example 6
[0080] This embodiment provides a travertine permeable concrete doped with powdered waste, wherein the travertine permeable concrete doped with powdered waste comprises the following raw materials in weight ratio:
[0081] Water: cement: water reducing agent: silica fume: limestone: travertine: powdered waste = 125.6: 335.1: 3.7: 46.5: 1215: 369.7: 71.1; the powdered waste includes travertine powder.
[0082] The designed porosity of the travertine permeable concrete doped with powdered waste is 15%, and the rest is the same as that of Example 1.
[0083] This embodiment also provides a method for preparing the above-mentioned travertine permeable concrete doped with powdered waste, and the preparation method is the same as that in Example 1.
[0084] Example 7
[0085] This embodiment provides a travertine permeable concrete doped with powdered waste, wherein the travertine permeable concrete doped with powdered waste comprises the following raw materials in weight ratio:
[0086] Water: cement: water reducing agent: silica fume: limestone: travertine: powdered waste = 125.6: 397.9: 3.7: 46.5: 1215: 369.7: 19.7; the powdered waste includes limestone powder.
[0087] The designed porosity of the travertine permeable concrete doped with powdered waste is 15%, and the rest is the same as that of Example 1.
[0088] This embodiment also provides a method for preparing the above-mentioned travertine permeable concrete doped with powdered waste, and the preparation method is the same as that in Example 1.
[0089] Example 8
[0090] This embodiment provides a travertine permeable concrete doped with powdered waste, wherein the travertine permeable concrete doped with powdered waste comprises the following raw materials in weight ratio:
[0091] Water: cement: water reducing agent: silica fume: limestone: travertine: powdered waste = 125.6: 376.9: 3.7: 46.5: 1215: 369.7: 39.5; the powdered waste includes limestone powder.
[0092] The designed porosity of the travertine permeable concrete doped with powdered waste is 15%, and the rest is the same as that of Example 1.
[0093] This embodiment also provides a method for preparing the above-mentioned travertine permeable concrete doped with powdered waste, and the preparation method is the same as that in Example 1.
[0094] Example 9
[0095] This embodiment provides a travertine permeable concrete doped with powdered waste, wherein the travertine permeable concrete doped with powdered waste comprises the following raw materials in weight ratio:
[0096] Water: cement: water reducing agent: silica fume: limestone: travertine: powdered waste = 125.6: 356.0: 3.7: 46.5: 1215: 369.7: 59.2; the powdered waste includes limestone powder.
[0097] The designed porosity of the travertine permeable concrete doped with powdered waste is 15%, and the rest is the same as that of Example 1.
[0098] This embodiment also provides a method for preparing the above-mentioned travertine permeable concrete doped with powdered waste, and the preparation method is the same as that in Example 1.
[0099] Example 10
[0100] This embodiment provides a travertine permeable concrete doped with powdered waste, wherein the travertine permeable concrete doped with powdered waste comprises the following raw materials in weight ratio:
[0101] Water: cement: water reducing agent: silica fume: limestone: travertine: powdered waste = 125.6: 335.1: 3.7: 46.5: 1215: 369.7: 78.9; the powdered waste includes limestone powder.
[0102] The designed porosity of the travertine permeable concrete doped with powdered waste is 15%, and the rest is the same as that of Example 1.
[0103] This embodiment also provides a method for preparing the above-mentioned travertine permeable concrete doped with powdered waste, and the preparation method is the same as that in Example 1.
[0104] Comparative Example 1
[0105] This comparative example provides a travertine permeable concrete, which comprises the following raw materials in weight ratio:
[0106] Water: cement: water reducing agent: silica fume: limestone: travertine = 125.6: 418.8: 3.7: 46.5: 1215: 369.7. The designed porosity of the travertine permeable concrete doped with powdered waste is 15%. The rest is the same as in Example 1.
[0107] This comparative example also provides a method for preparing the above-mentioned travertine permeable concrete doped with powdered waste. The preparation method is the same as Example 1 except that powdered waste is not added in step (3).
[0108] The final shape of the travertine permeable concrete mixed with powder waste in this comparative example after compressive crushing is shown in the figure below. Figure 3 shown.
[0109] The concrete in the above-mentioned embodiment and comparative example was demoulded and marked after being left to stand for one day, and then placed in a water tank for curing for 27 days. After the curing, the compressive strength, continuous porosity, water permeability coefficient and density were tested, and 3 parallel samples were tested in each group, and the average value was taken as the reference value.
[0110] The test method is carried out in accordance with the methods specified in the "Standard for Test Methods of Mechanical Properties of Ordinary Concrete" (GB / T50081-2019) and the "Technical Code for Permeable Cement Concrete Pavement" (CJJT135-2009).
[0111] The 28-day compressive strength, water permeability coefficient, continuous porosity and density of the travertine permeable concrete obtained in the above examples and comparative examples are shown in Table 1.
[0112] Table 1
[0113]
[0114] It can be seen from Table 1 that the travertine permeable concrete doped with powder waste provided by the present invention has a 28-day compressive strength of 16.31-34.26 MPa, a water permeability coefficient of 2.94-9.78 mm / s, a continuous porosity of 16.2-26.6%, and a density of 2540.5-2668.1 kg / m 3 .
[0115] According to the Technical Specification for Permeable Cement Concrete Pavement CJJT135-2009, Figures 4 to 6 The two dotted lines from top to bottom represent: the compressive strength of permeable concrete is 30MPa and the compressive strength of permeable concrete is 20MPa.
[0116] The compressive strength and water permeability coefficient of the travertine permeable concrete mixed with powdered waste in Examples 1 to 2 and the travertine permeable concrete in Comparative Example 1 are shown in the figure. Figure 4 shown.
[0117] from Figure 4 It can be seen that Example 1 ( Figure 4 When the porosity of group 2 is 20% and the replacement rate of travertine powder for cement is 5%, the 28-day compressive strength of travertine permeable concrete is 25.92MPa. Although the compressive strength is reduced, it still meets the strength design requirements for the fully permeable sidewalk in the specification. The cement content of the permeable concrete produced under this mix design is 20.8% compared with that of the comparative example 1 ( Figure 4The water permeability coefficient of the comparative example 1 is increased by nearly 45% compared with the comparative example 1, which allows more water to penetrate.
[0118] Example 2 Figure 4 When the designed porosity of group 3 is 25% and the replacement rate of travertine powder for cement is 10%, the strength of travertine permeable concrete is 16.31MPa, which is higher than that of comparative example 1 ( Figure 4 The concrete used in this mix design can be applied to pavements with lower compressive strength requirements. The cement consumption of the permeable concrete produced under this mix design can be reduced by 42% compared with that in Comparative Example 1. In this case, the water permeability coefficient increased by nearly 132% compared with Comparative Example 1, reaching 9.78 mm / s. In certain cases, concrete designed with this mix design can also be applied to actual pavements, which can not only reuse waste, but also greatly reduce carbon emissions and achieve low-carbon goals.
[0119] The compressive strength and water permeability coefficient of the travertine permeable concrete mixed with powdered waste in Examples 3 to 6 of the present invention and the travertine permeable concrete in Comparative Example 1 are shown in the figure. Figure 5 The compressive strength and water permeability coefficient of the travertine permeable concrete mixed with powdered waste in Examples 7 to 10 of the present invention and the travertine permeable concrete in Comparative Example 1 are shown in the figure. Figure 6 shown.
[0120] from Figure 5 and Figure 6 It can be seen that replacing cement with powdered waste will reduce the strength of permeable concrete, and after the addition of powdered waste travertine powder or limestone powder, the overall performance change trend of the two on permeable concrete is consistent.
[0121] The replacement rates of travertine powder for cement in Examples 3 to 6 are 5%, 10%, 15% and 20%, respectively, and the replacement rates of limestone powder for cement in Examples 7 to 10 are 5%, 10%, 15% and 20%, respectively. Comparative Example 1 does not contain travertine powder or limestone powder, i.e., the replacement rate is 0.
[0122] from Figure 5 and Figure 6 It can be seen that when the replacement rate of travertine powder or limestone powder for cement is 5%, the compressive strength of the permeable concrete decreases most significantly compared with Comparative Example 1. At this time, the porosity increases and the water permeability coefficient increases accordingly. As the powder replacement rate increases, the compressive strength of the concrete gradually increases until the ratio of travertine powder to limestone powder to cement reaches 15%, after which the compressive strength gradually decreases. The changes in the compressive strength of these samples can be attributed to the adhesion of the cement paste and the role of the powder as a hydrating agent and filler.
[0123] When the replacement rate of travertine powder or limestone powder for cement is 5%, the compressive strength of permeable concrete is lower than the strength requirement of 30MPa, but the water permeability coefficient is increased compared with Comparative Example 1. This concrete can still meet the application requirements of various pavement scenarios. As the amount of powder replacement increases, the compressive strength increases first and then decreases, but the overall strength is still above the strength requirement of 30MPa. At this time, the water permeability coefficient gradually decreases, but it is still within an acceptable range, and the amount of cement used is also greatly reduced, which is conducive to reducing carbon dioxide emissions and achieving low-carbon goals.
[0124] In summary, the travertine permeable concrete doped with powder waste provided by the present invention can use travertine powder or limestone powder to partially replace cement as a cementitious material to prepare permeable concrete while meeting the requirements of concrete compressive strength and water permeability, and can also ensure its working performance. In this way, not only can the powder waste be effectively processed, but also the goal of environmental sustainable development can be achieved.
[0125] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A travertine permeable concrete mixed with powder waste, It is characterized in that The travertine permeable concrete doped with powdered waste materials comprises the following raw materials in weight ratio: Water: cement: water reducing agent: silica fume: limestone: travertine: powdered waste = (79.7-125.6): (242.8-327.1): (2.4-3.7): (30-46.5): (1214-1216): (369-370): (14.6-22.9); the powdered waste includes travertine powder or limestone powder; The designed porosity of the travertine permeable concrete doped with powdered waste is 20-25%; The particle size of the travertine powder is less than 250 μm, and the particle size of the limestone powder is less than 250 μm.
2. The travertine permeable concrete according to claim 1, It is characterized in that The cement includes Portland cement.
3. The travertine permeable concrete according to claim 1, It is characterized in that The strength grade of the cement is 42.5 and the density is 3110kg / m 3 .
4. The travertine permeable concrete according to claim 1, It is characterized in that The water reducing agent includes Sika high-efficiency water reducing agent.
5. The travertine permeable concrete according to claim 1, It is characterized in that The water reducing agent has a water reducing rate of 20-25%.
6. The travertine permeable concrete according to claim 1, It is characterized in that The particle size of the limestone is 5-10 mm.
7. The travertine permeable concrete according to claim 1, It is characterized in that The particle size of the travertine is 5-10 mm.
8. The travertine permeable concrete according to claim 1, It is characterized in that The density of the travertine powder is 2640 kg / m 3 .
9. The travertine permeable concrete according to claim 1, It is characterized in that The density of the limestone powder is 2930kg / m 3 .
10. A method for preparing travertine permeable concrete doped with powdered waste as claimed in any one of claims 1 to 9, It is characterized in that The preparation method comprises the following steps: (1) Pour limestone and travertine into a mixer and mix for 60 seconds; (2) Add half of the water reducer and half of the water and stir for 90 seconds; (3) After adding cement, silica fume and powdered waste, stir for 90 seconds; (4) Add the remaining water and water, stir for 90 seconds, and then discharge the material into the mold.
Citation Information
Cited By
Full travertine aggregate pervious concrete and preparation method thereof
CN122520408A