Fluororubber composition
By adding compounds with specific number average molecular weights and introducing iodine and/or bromine groups into the fluororubber composition, the problem of scorch stability of fluororubber during high-speed vulcanization molding is solved, and high-speed vulcanization and good scorch stability are achieved. , improving the quality and durability of the product.
Patent Information
- Application Number
- CN202280060935.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-09-09
- Filing Date
- 2022-09-05
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-09-05
AI Technical Summary
Existing fluorine rubber is prone to scorch during high-speed vulcanization and molding in a short period of time, resulting in reduced product quality and insufficient scorch stability.
For every 100 parts by weight of peroxide-crosslinked fluororubber in the fluorine rubber composition, 0.1 to 1 part by weight of a compound with a number average molecular weight Mn of 200 to 300 is added, and an iodine group and/or a bromine group is introduced through a copolymerization reaction to form Cross-linking points to improve scorch stability and cure speed.
It achieves high-speed vulcanization and good scorch stability of fluorine rubber, shortens the vulcanization time, and improves the quality and durability of the product.
Smart Images

Figure CN117916308B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a fluororubber composition, and more particularly to a fluororubber composition capable of obtaining stable product quality and being vulcanized at a high speed. Background Art
[0002] Fluororubber compositions have excellent oil and fuel resistance and are used as sealing molding materials such as oil seals, O-rings, and gaskets in a wide range of fields such as automobiles and industrial machinery.
[0003] In recent years, from CO 2 From the perspective of reducing the demand for reduction or reducing costs, the demand for short-term vulcanization has increased, and fluororubber that can be vulcanized at a high speed has become the mainstream.
[0004] However, when vulcanization molding is completed in a short time, scorching is easily generated due to the thermal history in the processing step, and the scorching leads to a decrease in the quality of the product.
[0005] Under such background, products having excellent scorch stability while using fluororubber capable of high-speed vulcanization have been recently demanded.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Laid-Open No. 6-16892
[0009] Patent Document 2: Japanese Patent Application Laid-Open No. 5-279535 Summary of the invention
[0010] Technical problem to be solved by the invention
[0011] An object of the present invention is to provide a fluororubber composition which can be vulcanized at a high speed and has excellent scorch stability.
[0012] Solutions for solving technical problems
[0013] The above-mentioned object of the present invention can be achieved by the following fluororubber composition, in which, per 100 parts by weight of peroxide cross-linked fluororubber, 0.1 to 1 parts by weight of a compound represented by the general formula [I] having a number average molecular weight Mn of 200 to 300 is contained,
[0014]
[0015] In the formula, R 1 , R 2 and R 3Any two of them are lower alkyl groups having 1 to 5 carbon atoms, the remaining one is hydrogen, and X is methyl or hydroxy.
[0016] Effects of the Invention
[0017] The fluororubber composition of the present invention exhibits the following excellent effects: it can be vulcanized at a high speed and exhibits good scorch stability. DETAILED DESCRIPTION
[0018] The fluororubber composition of the present invention contains 0.1 to 1 parts by weight of a compound represented by the general formula [I] per 100 parts by weight of the peroxide cross-linked fluororubber.
[0019]
[0020] In the formula, R 1 , R 2 and R 3 Any two of them are lower alkyl groups having 1 to 5 carbon atoms, the remaining one is hydrogen, and X is methyl or hydroxy.
[0021] As the fluororubber, a peroxide-crosslinkable fluororubber can be used, and a homopolymer or copolymer of a fluorine-containing olefin can be used.
[0022] Examples of the fluorine-containing olefin include vinylidene fluoride, hexafluoropropylene, pentafluoropropylene, trifluoroethylene, chlorotrifluoroethylene, tetrafluoroethylene, vinyl fluoride, perfluoroacrylate, perfluoroalkyl acrylate, perfluoromethyl vinyl ether, perfluoroethyl vinyl ether, and perfluoropropyl vinyl ether.
[0023] The introduction of iodine groups and / or bromine groups that can peroxide-crosslink the fluororubber can be carried out by copolymerization in the presence of a saturated or unsaturated compound containing an iodine group and / or bromine group.
[0024] When the fluorinated copolymer contains a bromine group and / or an iodine group in the side chain, examples thereof include copolymers of crosslinking point forming monomers such as perfluoro(2-bromoethylvinyl ether), 3,3,4,4-tetrafluoro-4-bromo-1-butene, 2-bromo-1,1-difluoroethylene, bromotrifluoroethylene, perfluoro(2-iodoethylvinyl ether) and iodotrifluoroethylene.
[0025] When the fluorinated copolymer contains an iodine group and / or a bromine group at the end, the fluorinated copolymer represented by the general formula X can be used. 1 C n F 2n X 2 (X 1 :F, Br, I, X 2:Br, I, n:1~12), from the viewpoint of the balance between reactivity and operability, it is preferred to use a copolymer containing iodine and / or bromine groups, such as 1-bromonoperfluoroethane, 1-bromonoperfluoropropane, 1-bromonoperfluorobutane, 1-bromonoperfluoropentane, 1-bromonoperfluorohexane, 1-iodoperfluoroethane, 1-iodoperfluoropropane, 1-iodoperfluorobutane, 1-iodoperfluoropentane, 1-iodoperfluorohexane, etc., where n:1~6.
[0026] In addition, by making X 1 and X 2 It is I and / or Br, so that crosslinking points can be introduced at the end of the fluorinated copolymer. As the compound, for example, 1-bromo-2-iodotetrafluoroethane, 1-bromo-3-iodoperfluoropropane, 1-bromo-4-iodoperfluorobutane, 2-bromo-3-iodoperfluorobutane, monobromo-monoiodoperfluoropentane, monobromo-monoiodoperfluoro-n-hexane, 1,2-dibromoperfluoroethane, 1,3-dibromoperfluoropropane, 1,4-dibromoperfluorobutane, 1,5-dibromoperfluoropentane, 1,6-dibromoperfluorohexane, 1,2-diiodoperfluoroethane, 1,3-diiodoperfluoropropane, 1,4-diiodoperfluorobutane, 1,5-diiodoperfluoropentane, 1,6-diiodoperfluorohexane, etc. can be used. These compounds can also be used as chain transfer agents.
[0027] These copolymers can be obtained by solution polymerization, suspension polymerization or emulsion polymerization, and can also be purchased as commercial products, for example, P959 manufactured by Solvay, GBL-600S and GLT-600S manufactured by DuPont, and DAIEL-G801 and DAIEL-G901 manufactured by Daikin Industries, Ltd.
[0028] In the peroxide-cured fluororubber, a compound having a number average molecular weight Mn of 200 to 300 represented by the general formula [I] is added in a ratio of 0.1 to 1 part by weight, preferably 0.1 to 0.8 part by weight, per 100 parts by weight of the peroxide-cured fluororubber.
[0029]
[0030] In the formula, R 1 , R 2 and R 3 Any two of them are lower alkyl groups having 1 to 5 carbon atoms, preferably butyl or pentyl, more preferably tert-butyl or tert-pentyl, the remaining one is hydrogen, and X is methyl or hydroxyl. Here, if the ratio is less than the above range, scorch stability cannot be achieved, while if the ratio is more than the above range, the vulcanization time becomes longer.
[0031] Examples of the compound include 2,6-di-tert-butyl-4-methylphenol having a number average molecular weight Mn of 220.35, 2,5-di-tert-butylhydroquinone having a number average molecular weight Mn of 222.33, and 2,5-di-tert-amylhydroquinone having a number average molecular weight Mn of 250.38. Preferably, a hydroquinone derivative having an excellent balance between the scorch T5 and the rheometer t90 values is used.
[0032] It should be noted that Patent Document 1 describes an example of using 10 parts by weight of Nocrac NS-7 (2,5-di-tert-butylhydroquinone: number average molecular weight Mn: 222.33) manufactured by Ouchi Shinko Chemical as an antioxidant relative to 100 parts by weight of the fluoropolymer. However, in this method, the vulcanization time becomes long and the purpose of the present invention cannot be achieved.
[0033] In addition, Patent Document 2 discloses a fluorine-containing elastomer vulcanization composition, which contains a peroxide-vulcanizable fluorine-containing elastomer, an organic peroxide, a multifunctional co-crosslinking agent, and 0.1 to 10 parts by weight, preferably 0.2 to 5.0 parts by weight of a phenolic antioxidant (the phenolic antioxidant contains 1 to 4 hydroxyphenyl groups having 1 or 2 tert-butyl groups in one molecule) relative to 100 parts by weight of fluororubber. Although a number of examples of antioxidants are listed, the antioxidant used in the present invention is not listed. Particularly preferred is tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanurate having a molecular weight of 784.08.
[0034] To the fluororubber composition composed of the above essential ingredients, the following compounding agents may be appropriately added: fillers or reinforcing agents such as carbon black and silica; processing aids such as wax, metal soap, and carnauba wax; acid acceptors such as calcium hydroxide, magnesium oxide, zinc oxide, and hydrotalcite; antioxidants; thermoplastic resins; and colorants.
[0035] The process of dispersing the ingredients in the fluororubber can be performed by an open roll method, a closed mixing method or a multi-screw extrusion mixing method. Alternatively, a kneader can be used, in which case the mixing is performed at about 100 to 200°C, preferably about 140 to 180°C.
[0036] A cross-linking agent can be added to the mixed material for cross-linking molding to produce a fluororubber cross-linked molded product. As the cross-linking agent, a peroxide cross-linking agent can be used.
[0037] As the peroxide-based crosslinking agent, for example, 2,5-dimethylhexane-2,5-dihydroperoxide, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, tert-butyl peroxide, diisopropylbenzene peroxide, tert-butylisopropylbenzene peroxide, 1,1-di(tert-butylperoxy)-3,3,5-trimethylcyclohexane, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3, 1,3-di(tert-butylperoxyisopropyl)benzene, tert-butyl peroxybenzoate, tert-butyl peroxyisopropyl carbonate, 4,4-di(tert-butylperoxy)butyl valerate, etc. These can be used as commercial products (for example, Perhexa 25B-40 manufactured by NOF Corporation, etc.). The peroxide-based crosslinking agent is used in a ratio of about 1 to 10 parts by weight per 100 parts by weight of the fluororubber.
[0038] In addition, as the peroxide crosslinking agent, a commercially available masterbatch containing a raw rubber and a crosslinking agent may be used. These crosslinking agents may be used alone or in combination of two or more.
[0039] As a crosslinking accelerator (crosslinking auxiliary agent) which can be used for a peroxide-based crosslinking system, triallyl isocyanurate, triallyl cyanurate, trimethylolpropane trimethacrylate, etc. can be used.
[0040] The mixed product, i.e., the fluororubber composition, can be molded into a cross-linked molded product by, for example, pressurizing and heating the vulcanization. Specifically, the obtained fluororubber composition is heated (primary vulcanization) at a temperature of about 150 to 200° C. for about 3 to 300 minutes using an injection molding machine, a compression molding machine, a vulcanization press, an oven, etc., thereby obtaining a fluororubber cross-linked molded product. In addition, as required, a heat treatment is performed in an oven for about 1 to 20 hours at a temperature range of about 200 to 300° C., for example, for secondary vulcanization.
[0041] The obtained cross-linked molded product can be effectively used as a sealing member or the like.
[0042] Example
[0043] Hereinafter, the present invention will be described based on examples.
[0044] Example 1
[0045]
[0046]
[0047] The above components were kneaded using a kneader and an open roll, and the kneaded product was vulcanized at 180° C. for 4 minutes using a cross-linking press to obtain a cross-linked product.
[0048] Using uncrosslinked rubber sheets as test specimens, scorch T5 and rheometer t90 were measured.
[0049] Scorch T5: The time (T5) for the torque to rise by 5 M units at a temperature of 125° C. was measured. If T5 was 15 minutes or more, there was no concern about scorch, and it was evaluated as 0, and if it was less than 15 minutes, it was evaluated as ×.
[0050] Rheometer t90: According to JIS K6300 corresponding to ISO 289-1, a crosslinking curve is measured at a temperature of 180°C for 10 minutes, and the time t90 until a torque equivalent to 90% of the maximum torque value MH is reached is calculated. If t90 is less than 4 minutes, the crosslinking time is sufficiently short and is effective for reducing CO2 and reducing costs, so it is evaluated as 0, and 4 minutes or more is evaluated as ×.
[0051] The results obtained were: T5 was 25 (evaluation 0), and t90 was 1.17 (evaluation 0).
[0052] Example 2
[0053] In Example 1, the amount of 2,6-di-tert-butyl-4-methylphenol was changed to 0.1 parts by weight. As a result, T5 was 18 (evaluation 0) and t90 was 1.01 (evaluation 0).
[0054] Example 3
[0055] In Example 1, the amount of 2,6-di-tert-butyl-4-methylphenol was changed to 0.5 parts by weight. As a result, T5 was 40 or more (evaluation 0), and t90 was 1.78 (evaluation 0).
[0056] Example 4
[0057] In Example 1, the amount of 2,6-di-tert-butyl-4-methylphenol was changed to 1 part by weight. As a result, T5 was 40 or more (evaluation 0), and t90 was 3.42 (evaluation 0).
[0058] Example 5
[0059] In Example 1, instead of 2,6-di-tert-butyl-4-methylphenol, an equal amount (0.2 parts by weight) of 2,5-di-tert-butylhydroquinone (Nocrac NS-7 manufactured by Ouchi Shinko Chemical Industry Co., Ltd.: number average molecular weight Mn is 222.33) was used, and the results showed that T5 was 20 (evaluation 0) and t90 was 1.50 (evaluation 0).
[0060] Example 6
[0061] In Example 1, instead of 2,6-di-tert-butyl-4-methylphenol, an equal amount (0.2 parts by weight) of 2,5-di-tert-amylhydroquinone (Nocrac DAH, manufactured by Ouchi Shinko Chemical Industry Co., Ltd.: number average molecular weight Mn is 250.38) was used, and the results showed that T5 was 26 (evaluation 0) and t90 was 1.58 (evaluation 0).
[0062] Comparative Example 1
[0063] In Example 1, 2,6-di-tert-butyl-4-methylphenol was not used, and as a result, T5 was 11 (evaluation ×) and t90 was 0.83 (evaluation ○).
[0064] Comparative Example 2
[0065] In Example 1, instead of 2,6-di-tert-butyl-4-methylphenol, an equal amount (0.2 parts by weight) of 2,2-methylenebis(4-methyl-6-tert-butylphenol (Nocrac NS-6 manufactured by Ouchi Shinko Chemical Industry Co., Ltd.: number average molecular weight Mn is 340.51) was used, and the results showed that T5 was 10 (evaluation ×) and t90 was 1.40 (evaluation 0).
[0066] Comparative Example 3
[0067] In Example 1, instead of 2,6-di-tert-butyl-4-methylphenol, an equal amount (0.2 parts by weight) of tetrakis[methylene-3-(3',5'-di-tert-butyl-4-hydroxyphenyl)propionate]methane (ADK STAB AO-60 manufactured by ADEKA: number average molecular weight Mn is 1178) was used, and the results showed that T5 was 10 (evaluation ×) and t90 was 1.03 (evaluation 0).
[0068] Comparative Example 4
[0069] In Example 1, the amount of 2,6-di-tert-butyl-4-methylphenol used was changed to 1.3 parts by weight. As a result, T5 was 40 or more (evaluation 0), and t90 was 4.33 (evaluation ×).
Claims
1. A fluororubber composition, characterized in that: The peroxide cross-linked fluororubber contains 0.1 to 1 parts by weight of a compound represented by the general formula [I] having a number average molecular weight Mn of 200 to 300, per 100 parts by weight of the peroxide cross-linked fluororubber. In the formula, any two of R1, R2 and R3 are lower alkyl groups having 1 to 5 carbon atoms, the remaining one is hydrogen, and X is methyl or hydroxyl.
2. The fluororubber composition according to claim 1, characterized in that: The lower alkyl group having 1 to 5 carbon atoms is tert-butyl or tert-pentyl.
3. The fluororubber composition according to claim 2, characterized in that: The compound represented by the general formula [I] is 2,6-di-tert-butyl-4-methylphenol.
4. The fluororubber composition according to claim 1, characterized in that: The compound represented by the general formula [I] is a hydroquinone derivative.
5. The fluororubber composition according to claim 4, characterized in that: The hydroquinone derivative is 2,5-di-tert-butylhydroquinone or 2,5-di-tert-amylhydroquinone.
6. The fluororubber composition according to claim 1, characterized in that: A peroxide crosslinking agent is further compounded.
7. A cross-linked molded article, characterized in that: It is a cross-linked product of the fluororubber composition according to claim 6.
8. The cross-linked molded article according to claim 7, characterized in that Used as sealing material.
Citation Information
Patent Citations
Fluorine-containing elastomer vulcanized composition
JP1993279535A
Manufacturing method of rubber sealing gasket
CN107337818A
Anti-corrosion water-blocking buffer layer material for cable
CN108164887A
Crosslinking agent for ethylene propylene diene monomers and sealing strip prepared by crosslinking agent
CN110105624A
Irradiation crosslinking modified ECTFE (ethylene chlorotrifluoroethylene) heat shrinkable sleeve and preparation method thereof
CN110256762A