A single crystal or quasi-single crystal lithium-rich manganese-based positive electrode material precursor and its preparation method and application

By using a composite precipitant in an oxidative environment, the problem of low compaction density of lithium-rich manganese-based positive electrode material is solved, and the comprehensive performance improvement of high compaction density and high discharge ratio energy is achieved. It is suitable for lithium-ion batteries commercial application.

CN117923561BActive Publication Date: 2024-11-01TIANJIN GUOAN MGL NEW MATERIALS TECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202311012045.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-11
Publication Date
2024-11-01
Estimated Expiration
2043-08-11

AI Technical Summary

Technical Problem

The compaction density of lithium-rich manganese-based cathode materials is hindered from its commercial application in high-energy density lithium-ion batteries, and the traditional single crystallization process is difficult to apply, resulting in a decrease in discharge specific capacity.

Method used

The co-precipitation reaction is carried out under an oxidation environment by using a composite precipitation agent. Through the synergistic action of alkaline substances and soluble carbonates, the hydroxide precursor containing carbonate is synthesized, the primary grain size is reduced, and the internal porosity of the particles is improved. Specific surface area, thereby increasing the compaction density and discharge specific energy of the material.

Benefits of technology

The high compaction density and high discharge ratio energy of lithium-rich manganese-based cathode materials are achieved, which improves the comprehensive performance of the material and simplifies the process, which is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117923561B_ABST
    Figure CN117923561B_ABST
Patent Text Reader

Abstract

The present invention provides a single crystal or quasi-single crystal lithium-rich manganese-based positive electrode material precursor and its preparation method and application, the preparation method comprising: introducing a metal salt solution, a composite precipitant, a complexing agent and an oxidant into a reaction vessel in parallel, performing a coprecipitation reaction, and then performing crystallization to obtain the lithium-rich manganese-based positive electrode material precursor; wherein the metal salt in the metal salt solution comprises a manganese salt and an M salt, and the M salt comprises a nickel salt and / or a cobalt salt; the composite precipitant comprises a solution containing an alkaline substance and a soluble carbonate. The present invention can increase the specific surface area and activity of the precursor through the combined action of alkaline substances and soluble carbonates and the coprecipitation reaction in an oxidizing environment, thereby being able to increase the compaction density of the single crystal or quasi-single crystal lithium-rich manganese-based positive electrode material while ensuring its high discharge specific energy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of batteries and relates to a single crystal or quasi-single crystal lithium-rich manganese-based positive electrode material precursor and a preparation method and application thereof. Background Art

[0002] Compared with traditional layered oxide positive electrode materials and polyanion positive electrode materials, lithium-manganese-rich layered positive electrode materials have low raw material costs, relatively simple processing, and ultra-high discharge specific capacity, which can reach more than 300mAh / g at 2.0-4.8V. The highest capacity of lithium-manganese-rich materials reported so far reaches 400mAh / g, which is the only known positive electrode material that can meet the requirements of high energy density batteries of more than 350Wh / kg. Therefore, it has received high attention from all walks of life since its introduction. However, the inherent disadvantages of lithium-manganese-rich positive electrode materials such as low conductivity, poor high-rate performance, fast cycle voltage decay and low compaction density have hindered the commercial application of the material and delayed the development of high-energy-density lithium-ion batteries. Among them, low compaction density is a major factor hindering the commercial application of lithium-manganese-rich positive electrode materials.

[0003] There are two main reasons for the low compaction density of lithium-rich manganese-based materials. One is the high content of Mn elements. Since the true density of the lithium-oxygen compound of Mn is low, the high Mn content leads to a decrease in the density of the material. The other is that due to the low ionic conductivity of lithium-rich manganese-based materials, the excessive density inside the particles will cause difficulties in the removal / embedding of lithium ions, resulting in a significant decrease in capacity. In order to ensure high capacity, lithium-rich manganese-based materials usually use carbonates as precursors, and the sintered products are aggregated from submicron-sized fine particles (referred to as primary particles) into spherical or quasi-spherical secondary agglomerate particles (referred to as secondary particles). The carbonate precursor produces a certain amount of internal pores by releasing carbon dioxide gas during the sintering process. Although the generation of internal pores will reduce the size of the primary grains, thereby reducing the resistance to lithium ion diffusion and ensuring the high capacity characteristics of lithium-rich manganese-based materials, the large number of gaps between these particles and the porous structure inside the particles bring about the problems of low particle density and low pole piece compaction density, resulting in low overall mass energy density of the material.

[0004] In order to improve the compaction density of lithium-rich manganese-based materials, some researchers have done some work on the development of single-crystal lithium-rich manganese-based materials. For example, patent CN102832387B discloses a method for improving the compaction density of lithium-rich manganese-based materials by ball milling mixing and calcination in an oxygen environment. However, the ball milling mixing method makes the morphology of the raw materials after ball milling uncontrollable, resulting in uncontrollable particle size and wide distribution of the sintered products. The particle size distribution is wide and the material capacity and discharge capacity are low.

[0005] In order to improve the compaction density of lithium-rich manganese-based materials and improve the safety performance of materials, single-crystal or single-crystal lithium-rich manganese-based materials have been proposed by developers in academia and the business community. This idea is mostly derived from single-crystal ternary materials and single-crystal high-nickel materials. By sintering into a single crystal morphology, the inherent grain boundaries inside the polycrystalline material particles are eliminated, and the compaction density and compressive resistance of the particles are improved. However, the traditional synthesis method and process route ideas of single-crystal ternary materials are difficult to apply to lithium-rich manganese-based positive electrode materials. The main reason is that the ion diffusion rate of lithium-rich manganese-based positive electrode materials is lower than that of ternary and high-nickel materials. Excessive density and single crystallization will lead to a serious decrease in the discharge specific capacity of lithium-rich manganese-based materials. For example, the discharge capacity of 2.0~4.8V0.1C is reduced to 160~220mAh / g, and the unit energy density depends on the compaction density and discharge specific energy.

[0006] Therefore, in order to improve the overall performance, while increasing the compaction density of the material, it is necessary to ensure the discharge specific energy of the material to ensure the unit energy density. This is a major challenge faced in the commercial application of lithium-rich manganese-based materials. Summary of the invention

[0007] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a single crystal or quasi-single crystal lithium-rich manganese-based positive electrode material precursor and its preparation method and application. The present invention can synthesize a hydroxide composite precursor containing carbonate through the synergistic effect of alkaline substances and soluble carbonates in the composite precipitant, and unlike traditional hydroxide precursors, the precursor of the present invention undergoes a coprecipitation reaction in an oxidizing environment, and the precursor has a smaller primary grain size and a large number of gaps, thereby increasing the specific surface area and activity of the precursor, significantly increasing the compaction density of the material, and at the same time ensuring a high discharge specific capacity, thereby improving the overall performance of the material.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a method for preparing a single crystal or quasi-single crystal lithium-rich manganese-based positive electrode material precursor, the preparation method comprising:

[0010] The metal salt solution, the composite precipitant, the complexing agent and the oxidant are introduced into the reaction container in parallel to perform a coprecipitation reaction, and then crystallize to obtain the lithium-rich manganese-based positive electrode material precursor;

[0011] Wherein, the metal salt in the metal salt solution includes manganese salt and M salt, and the M salt includes nickel salt and / or cobalt salt;

[0012] The composite precipitant comprises a solution containing an alkaline substance and a soluble carbonate.

[0013] The present invention provides a method for preparing a single crystal or quasi-single crystal lithium-rich manganese-based positive electrode material precursor, which adopts a composite precipitant to carry out a coprecipitation reaction in an oxidizing environment, and can synthesize a hydroxide precursor containing carbonate through the synergistic effect of alkaline substances and soluble carbonates in the composite precipitant, and under the action of an oxidant, Mn ions can be partially or completely oxidized to carry out a coprecipitation reaction, which can greatly reduce the primary grain size and increase the porosity inside the particles, thereby improving the specific surface area and activity of the precursor, and further ensuring its high discharge specific energy while improving the compaction density of the single crystal or quasi-single crystal lithium-rich manganese-based positive electrode material.

[0014] Preferably, the alkaline substance includes at least one of sodium hydroxide, potassium hydroxide and lithium hydroxide.

[0015] Preferably, the soluble carbonate includes at least one of sodium carbonate, ammonium carbonate, ammonium bicarbonate and sodium bicarbonate.

[0016] Preferably, in the solution containing alkaline substances and soluble carbonates, the concentration of the alkaline substances is 2 to 10 mol / L, for example, it can be 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L, 9 mol / L or 10 mol / L.

[0017] Preferably, in the solution containing the alkaline substance and the soluble carbonate, the concentration of carbonate ion is 1 to 5 mol / L, for example, 1 mol / L, 2 mol / L, 3 mol / L, 4 mol / L or 5 mol / L.

[0018] Preferably, in the solution containing the alkaline substance and the soluble carbonate, the molar ratio of hydroxide to carbonate is (2-10):1, for example, it can be 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1 or 10:1.

[0019] Preferably, the manganese salt includes at least one of manganese sulfate, manganese nitrate, manganese chloride and manganese acetate.

[0020] Preferably, the nickel salt includes at least one of nickel sulfate, nickel nitrate, nickel chloride and nickel acetate.

[0021] Preferably, the cobalt salt includes at least one of cobalt sulfate, cobalt nitrate, cobalt chloride and cobalt acetate.

[0022] In the present invention, when the metal salt solution contains cobalt salt, under the action of the oxidant, the Co ions will also be partially oxidized or completely oxidized.

[0023] Preferably, in the metal salt solution, the concentration of the metal salt is 0.5-3 mol / L, for example, it can be 0.5 mol / L, 0.7 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L, 2.7 mol / L or 3 mol / L, etc., preferably 0.5-2.5 mol / L.

[0024] Preferably, the complexing agent includes at least one of ammonia water, ammonium carbonate, ammonium bicarbonate, glutamic acid, ammonium citrate, disodium ethylenediaminetetraacetate and citric acid.

[0025] Preferably, before mixing the metal salt solution, the composite precipitant and the complexing agent, a base liquid (e.g., deionized water) is added to the reaction container, and then the complexing agent and the composite precipitant are added to the base liquid, so that the pH value of the base liquid is 9 to 12.5, for example, 9, 9.5, 10, 10.5, 11, 11.5, 12 or 12.5, etc.

[0026] Preferably, the pH value of the coprecipitation reaction is 9 to 12.5, for example, 9, 9.5, 10, 10.5, 11, 11.5, 12 or 12.5, etc. Further, the pH value fluctuates within a range of no more than ±1.

[0027] In the present invention, the pH value of the coprecipitation reaction may be the same as or different from the pH value of the base solution.

[0028] Preferably, within 2 to 4 hours after the start of the coprecipitation reaction, the pH value is 11.5 to 12.5, and the pH value fluctuates within ±0.2; after 2 to 4 hours of reaction, the pH value is adjusted to 9 to 11.5, and the pH value fluctuates within ±1, preferably within ±0.2.

[0029] Preferably, the coprecipitation reaction temperature is 15-65°C, for example, it can be 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 50°C, 55°C, 60°C or 65°C.

[0030] In the present invention, the temperature range of the coprecipitation reaction is relatively wide, and the coprecipitation reaction can be carried out at a relatively low temperature. If the temperature of the coprecipitation reaction is too low, a large number of amorphous precursor particles will appear without spherical morphology; if the temperature of the coprecipitation reaction is too high, the precursor crystallinity will be too high, the particle density will be high, and the discharge capacity of the sintered product will be low.

[0031] Preferably, the coprecipitation reaction is accompanied by stirring, and the stirring speed is 200-1100 rpm, for example, 200 rpm, 400 rpm, 600 rpm, 800 rpm or 1000 rpm.

[0032] Preferably, the oxidant includes at least one of oxygen-containing gas, hydrogen peroxide, sodium hypochlorite, ammonium persulfate, potassium persulfate, sodium persulfate and potassium permanganate.

[0033] The present invention does not specifically limit the oxygen-containing gas, including but not limited to air or oxygen.

[0034] In the reaction system of the coprecipitation reaction, the concentration of ammonium ions is 0.5 to 3 g / L, for example, 0.5 g / L, 1 g / L, 1.5 g / L, 2 g / L, 2.5 g / L or 3 g / L.

[0035] Preferably, the crystallization temperature is 50-90°C, for example, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C or 90°C.

[0036] Preferably, the crystallization time is 1 to 24 hours, for example, 1 hour, 2 hours, 5 hours, 7 hours, 10 hours, 15 hours, 20 hours, 22 hours or 24 hours.

[0037] In the present invention, under the action of the complexing agent, the metal salt solution and the composite precipitant undergo a coprecipitation reaction to form spherical or quasi-spherical particles. After the particles gradually grow to a target particle size, the pumping of the metal salt solution, the composite precipitant, the complexing agent and the oxidant is stopped, and crystallization is carried out at 50 to 90° C. for 1 to 24 hours. The crystallization process is accompanied by stirring, and the stirring speed is 200 to 1100 rpm, for example, 200 rpm, 400 rpm, 600 rpm, 800 rpm or 1000 rpm, etc., preferably consistent with the stirring speed during the coprecipitation reaction.

[0038] Preferably, after the crystallization, the crystallization product is soaked in alkaline solution, and then the steps of filtering, washing and drying are performed in sequence to obtain the single crystal or quasi-single crystal lithium-rich manganese-based positive electrode material precursor. Preferably, the drying temperature is 100-150°C, for example, it can be 100°C, 110°C, 120°C, 130°C or 140°C, and the drying time is 4-10h, for example, it can be 4h, 6h, 8h or 10h, etc.

[0039] Preferably, the alkali solution includes at least one of sodium hydroxide, potassium hydroxide, sodium carbonate, sodium bicarbonate and ammonium bicarbonate; the concentration of the alkali solution is 1-10%, for example, it can be 1%, 2%, 5%, 7% or 10%.

[0040] Preferably, the alkali solution soaking time is 5 to 120 min, for example, it can be 5 min, 10 min, 15 min, 20 min, 50 min, 70 min, 100 min or 120 min.

[0041] In a second aspect, the present invention provides a single-crystal or quasi-single-crystal lithium-rich manganese-based cathode material precursor, which is prepared by the preparation method described in the first aspect.

[0042] Preferably, the D50 of the lithium-rich manganese-based cathode material precursor is 3 to 9 μm, preferably 3 to 7 μm.

[0043] Preferably, the primary grain length of the lithium-rich manganese-based cathode material precursor is 0.35 - 1.0 μm.

[0044] Preferably, the specific surface area of the lithium-rich manganese-based cathode material precursor is 20 - 100 m 2 / g.

[0045] Preferably, the tap density of the lithium-rich manganese-based cathode material precursor is 0.5 - 1.2 g / cm 3 .

[0046] In a third aspect, the present invention provides a single-crystal or quasi-single-crystal lithium-rich manganese-based cathode material, which is obtained by mixing and sintering the single-crystal or quasi-single-crystal lithium-rich manganese-based cathode material precursor described in the second aspect and a lithium source.

[0047] Preferably, the lithium source includes at least one of lithium hydroxide, lithium carbonate, lithium nitrate, lithium chloride, and lithium acetate.

[0048] Preferably, the ratio of the molar amount of lithium element in the lithium source to the sum of the molar amounts of metal elements in the precursor is 1.0 - 1.25, and can be, for example, 1.0, 1.1, 1.2, or 1.25, etc.

[0049] Preferably, the chemical formula of the lithium-rich manganese-based cathode material is Li[Li a (Mn x Ni y Co z ) 1-a O2, where 0 < a < 0.5, x + y + z = 1, 0 ≤ y < x, 0 ≤ z < x, x < 1, 0 ≤ y ≤ 0.5, 0 ≤ z ≤ 0.5, where a can be, for example, 0.1, 0.2, 0.3, 0.4, or 0.45, etc., x can be, for example, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, or 0.9, etc., y can be, for example, 0, 0.05, 0.1, 0.2, 0.3, 0.4, or 0.5, etc., and z can be, for example, 0, 0.05, 0.1, 0.2, 0.3, 0.4, or 0.5, etc.

[0050] Preferably, the primary grain length of the lithium-rich manganese-based cathode material is 0.35 - 1.0 μm.

[0051] Preferably, the sintering is step-by-step sintering, and the step-by-step sintering includes a primary sintering and a secondary sintering performed sequentially.

[0052] Preferably, the primary sintering temperature is 300-600°C, for example, 300°C, 350°C, 400°C, 450°C, 500°C, 550°C or 600°C, and the primary sintering time is 2-6h, for example, 2h, 3h, 4h, 5h or 6h.

[0053] Preferably, the secondary sintering temperature is 850-1100°C, for example, it can be 850°C, 900°C, 950°C, 1000°C, 1050°C or 1100°C, and the secondary sintering time is 6-18h, for example, it can be 6h, 8h, 10h, 12h, 14h, 16h or 18h.

[0054] Preferably, the heating rates of the primary sintering and the secondary sintering are independently 1 to 5°C / min, for example, 1°C / min, 2°C / min, 3°C / min or 5°C / min.

[0055] In the present invention, the higher the sintering temperature, the closer the morphology of the sintered material particles is to single crystal. Therefore, according to actual needs, the sintering temperature and sintering time can be controlled to adjust the primary grain size and morphology to prepare a single-crystal-like or completely single-crystal lithium-manganese-based positive electrode material.

[0056] Preferably, after the sintering, the sintered product is post-treated to obtain the lithium-rich manganese-based positive electrode material.

[0057] Preferably, a pulverization step is performed between the sintering and the post-treatment. The particle size D50 of the pulverized product is 2 to 7 μm, for example, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm or 7 μm.

[0058] Optionally, the pulverizing equipment includes a mechanical pulverizer or a jet pulverizer.

[0059] Preferably, the post-treatment comprises pickling treatment and calcination performed sequentially.

[0060] In the present invention, after pickling treatment, the discharge capacity of the lithium-rich manganese-based positive electrode material of the present invention can be increased by 15 to 25 mAh / g compared to the untreated material, and the first discharge efficiency can be increased by 5 to 8%. The treatment process can use a dilute acid with a lower concentration, which has little damage to the main structure of the lithium-rich manganese-based material, and the solvent is removed by filtering, eliminating the high energy consumption of the evaporation process. If the pickling step is omitted, the first efficiency and discharge capacity will be low.

[0061] Preferably, the pickling treatment comprises: immersing the product to be treated in acid for 0.5 to 4 hours, for example, 0.5 hours, 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, 3.5 hours or 4 hours.

[0062] Preferably, the acid comprises a soluble acid, and the soluble acid includes but is not limited to acetic acid, sulfuric acid, nitric acid, oxalic acid, boric acid or phosphoric acid.

[0063] Preferably, the concentration of the acid is 0.1 to 3 mol / L, for example, 0.1 mol / L, 0.2 mol / L, 0.5 mol / L, 1 mol / L, 2 mol / L or 3 mol / L.

[0064] Preferably, the ratio of the mass of the product to be treated to the volume of the acid is 1g:(0.5-10)mL, for example, it can be 1g:0.5mL, 1g:1mL, 1g:2mL, 1g:4mL, 1g:6mL, 1g:8mL or 1g:10mL, etc.

[0065] Preferably, the pickling process is accompanied by stirring, and the stirring speed is 50-500 rpm, for example, 50 rpm, 100 rpm, 200 rpm, 300 rpm or 400 rpm.

[0066] Preferably, between the acid washing treatment and the calcination, a step of filtering and washing to neutrality is performed, and then drying at 100-200° C. for 5-10 hours. The 100-200° C. may be, for example, 100° C., 120° C., 140° C., 160° C. or 180° C., and the 5-10 hours may be, for example, 5 hours, 6 hours, 7 hours, 8 hours or 9 hours.

[0067] Preferably, the calcination temperature is 350-600°C, for example, 350°C, 400°C, 450°C, 500°C, 550°C or 600°C, and the calcination time is 2-6h, for example, 2h, 3h, 4h, 5h or 6h.

[0068] In a fourth aspect, the present invention provides a lithium secondary battery, wherein the positive electrode of the lithium secondary battery comprises the single crystal or quasi-single crystal lithium-rich manganese-based positive electrode material described in the third aspect.

[0069] The lithium secondary battery includes but is not limited to a liquid lithium battery, a semi-solid lithium battery or an all-solid lithium battery; in addition to the single crystal lithium-rich manganese-based positive electrode material described in the third aspect, the positive electrode of the lithium secondary battery may also include other positive electrode materials, such as 5 series, 6 series or 7 series medium and low nickel ternary materials or 8 series, 9 series and above high nickel positive electrode materials, which can improve the discharge capacity and overcharge resistance of these positive electrode materials.

[0070] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0071] Compared with the prior art, the present invention has the following beneficial effects:

[0072] (1) The present invention provides a method for preparing a single crystal or quasi-single crystal lithium-rich manganese-based positive electrode material precursor, which uses a composite precipitant to carry out a coprecipitation reaction in an oxidizing environment. Through the combined action of alkaline substances, soluble carbonates and oxidants in the composite precipitant, a hydroxide composite precursor containing carbonate can be synthesized, which can greatly reduce the primary grain size of the precursor and the internal porosity of the precursor particles, thereby increasing the specific surface area and activity of the precursor. The specific surface area of ​​the precursor can reach 20m 2 / g and above, the highest can reach 100m 2 / g; Furthermore, the present invention can improve the compaction density of single crystal or quasi-single crystal lithium-rich manganese-based positive electrode materials while ensuring their high discharge specific energy;

[0073] (2) The present invention can control the thickness and length of the primary grain layer in the precursor particles by controlling the precursor process conditions;

[0074] (3) The lithium-rich manganese-based positive electrode material of the present invention has a single crystal-like or single crystal morphology and a high compaction density. The compaction density of the positive electrode sheet can reach 2.85-3.0 g / cm 3 , the discharge capacity can reach more than 250mAh / g at 2.0-4.8V, and the discharge capacity can reach more than 210mAh / g when tested in the voltage range of 2.0-4.6V, and the first discharge efficiency can reach more than 82%;

[0075] (4) The process of the present invention is simple and easy to implement, suitable for large-scale production, and has strong controllability over product performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0076] Figure 1 This is a SEM image of the single-crystal-like lithium-manganese-rich positive electrode material provided in Example 1 of the present invention. DETAILED DESCRIPTION

[0077] The technical solution of the present invention is further illustrated below through specific implementation methods.

[0078] Example 1

[0079] This embodiment provides a method for preparing a single-crystal-like lithium-rich manganese-based positive electrode material precursor, comprising the following steps:

[0080] Nickel sulfate and manganese sulfate are dissolved in a molar ratio of Ni:Mn=1:3 to form a mixed salt solution with a concentration of 2 mol / L, a mixed alkali solution of 10 mol / L sodium hydroxide and 5 mol / L sodium carbonate (i.e., a composite precipitant) is prepared, and ammonia water (i.e., a complexing agent) with a concentration of 10 mol / L is prepared; 10 L of pure water and 5 L of ammonia water are added to a 100 L reactor, and then several liters of the mixed alkali solution are added to adjust the pH value to 12.4-12.5, the reactor temperature is controlled at 65°C, the stirring speed is 500 rpm, the mixed salt solution, the mixed alkali solution and the complexing agent are pumped into the reactor at the same time, and the mixed alkali solution is introduced into the reactor through an air inlet pipe. Air (i.e., oxidant) was introduced into the solution at a rate of 20 mL / min, the flow rates of the mixed salt solution, the complexing agent, and the oxidant were fixed, the flow rate of the mixed alkali solution was adjusted to control the pH value to be between 12.3 and 12.5, after reacting for 4 hours, the pH value was reduced to 11.3 to 11.5, the flow rates of the three solutions were stabilized, the pH fluctuation range was controlled within ±0.1, and the coprecipitation reaction was carried out by an intermittent method, the ammonium concentration in the system was 3 g / L, and the solution was stopped from being pumped until the particles grew to 6.5 μm, the reaction temperature was increased to 75°C, and stirring and temperature crystallization were maintained for 12 hours; the reaction product was filtered, washed, and dried to obtain Ni 0.25 Mn 0.75 The (OH)2 precursor, denoted as P1, has an average particle size D50 of 6.0 μm and a tap density of 1.1 g / cm 3 , specific surface area 25m 2 / g, and the length of the lamellar primary grains is about 0.8μm.

[0081] This embodiment also provides a method for preparing a single-crystal-like lithium-rich manganese-based positive electrode material, comprising the following steps:

[0082] (1) 1000 g of P1 precursor and the corresponding weight of lithium carbonate were weighed at a molar ratio of Li:(Ni+Mn)=1.5:1, mixed evenly in a high-speed mixer, and then put into a sagger and placed in a box furnace. The temperature was raised to 500°C at a rate of 5°C / min, and the temperature was kept at this temperature for 3 hours. The temperature was then raised to 1100°C at a rate of 5°C / min, and the mixture was calcined for 10 hours. After the mixture was cooled to room temperature in the furnace, the sintered material was crushed to 3.0 μm using a jet mill. The particle morphology was in a single crystal-like state and was recorded as RL1.

[0083] (2) Add 5 L of 1 mol / L boric acid solution to a stirring container, add 500 g of RL1 while stirring, continue stirring for 4 h after adding, then filter quickly, dry at 100 ° C for 24 h, calcine at 600 ° C for 6 h, cool to room temperature with the furnace, and use a mechanical crusher to crush to an average particle size D50 of 4.1 μm to obtain a single-crystal-like lithium-rich manganese-based positive electrode material, recorded as RL-T1, as shown in Figure 1 shown.

[0084] Example 2

[0085] This embodiment provides a method for preparing a single-crystal lithium-rich manganese-based positive electrode material precursor, comprising the following steps:

[0086] Nickel chloride and manganese chloride were dissolved in a molar ratio of Ni:Mn=1:3 to form a mixed salt solution with a concentration of 3 mol / L, and a mixed alkali solution of 5 mol / L sodium hydroxide and 1 mol / L ammonium bicarbonate (i.e., a composite precipitant), 1 mol / L EDTA solution (i.e., a complexing agent), and 10% hydrogen peroxide solution (i.e., an oxidant) were prepared; 10 L of pure water and 5 L of EDTA solution, and then add several liters of mixed alkali solution to adjust the pH value to 11.9-12.1, control the reactor temperature to 50°C, stir at 500rpm, pump the mixed salt solution, mixed alkali solution, complexing agent and oxidant into the reactor at the same time, fix the flow rate of the mixed salt solution, complexing agent and oxidant, adjust the flow rate of the mixed alkali solution to control the pH value at 11.9-12.1, react for 4 hours, reduce the pH value to 11.8-12.0, stabilize the flow rate of the four solutions, control the pH fluctuation range within ±0.1, and use a continuous method to carry out coprecipitation reaction. The ammonium concentration in the system is 1g / L. Stop pumping the solution until the particles grow to 3.0μm, increase the reaction temperature to 70°C, and keep stirring and temperature crystallization for 10 hours. The reaction product is filtered, washed and dried to obtain Ni 0.25 Mn 0.75 The (OH)2 precursor, denoted as P2, has an average particle size D50 of 3.0 μm and a tap density of 0.62 g / cm 3 , specific surface area 38m 2 / g, and the length of the lamellar primary grains is about 0.7μm.

[0087] This embodiment also provides a method for preparing a single-crystal lithium-rich manganese-based positive electrode material, comprising the following steps:

[0088] (1) 1000 g of P2 precursor and corresponding weight of lithium carbonate were weighed at a molar ratio of Li:(Ni+Mn)=1.5:1, mixed evenly in a high-speed mixer, and then placed in a sagger and placed in a box furnace. The temperature was raised to 500°C at a rate of 5°C / min, and the temperature was kept at this temperature for 3 hours. The temperature was then raised to 1100°C at a rate of 5°C / min, and the mixture was calcined for 10 hours. After the mixture was cooled to room temperature in the furnace, the sintered material was crushed to 3.0 μm using a jet mill. The particle morphology was single crystal, and was recorded as RL2.

[0089] (2) Add 5 L of 1 mol / L boric acid solution to a stirring container, add 500 g of RL2 while stirring, continue stirring for 4 hours after addition, then quickly filter, dry at 100 ° C for 24 hours, calcine at 600 ° C for 6 hours, cool to room temperature with the furnace, and use a mechanical crusher to crush to an average particle size D50 of 3.0 μm to obtain a single crystal lithium-rich manganese-based positive electrode material, recorded as RL-T2.

[0090] Example 3

[0091] This embodiment provides a method for preparing a single-crystal-like lithium-rich manganese-based positive electrode material precursor, comprising the following steps:

[0092] Nickel nitrate, manganese nitrate and cobalt nitrate were dissolved into a mixed salt solution with a molar ratio of Ni:Mn:Co=5:14:1, and a mixed alkali solution (i.e., a composite precipitant) of 8 mol / L potassium hydroxide and 1 mol / L ammonium carbonate, a citric acid solution (i.e., a complexing agent) of 0.5 mol / L, and a sodium hypochlorite solution (i.e., an oxidant) of 1 mol / L were prepared; 10 L of pure water and 5 L of citric acid solution were added to a 100 L reactor, and then several liters of the mixed alkali solution were added to adjust the pH value to 11.4-11.6, and the temperature of the reactor was controlled to 45°C. The stirring speed is 500rpm, and the mixed salt solution, mixed alkali solution, complexing agent and oxidant are pumped into the reactor at the same time. The flow rates of the mixed salt solution, complexing agent and oxidant are fixed, and the flow rate of the mixed alkali solution is adjusted to control the pH value at 11.4-11.6. After 4 hours of reaction, the pH value is reduced to 10.8-11.0, and the flow rates of the four solutions are stabilized. The pH fluctuation range is controlled within ±0.1. The coprecipitation reaction is carried out by the intermittent method. The ammonium concentration in the system is 2g / L. The solution is stopped from being pumped until the particles grow to 5.0μm. The reaction temperature is increased to 50°C, and stirring and temperature crystallization are maintained for 18 hours. The reaction product is filtered, washed and dried to obtain Ni 0.25 Mn 0.7 0Co 0.05 (OH)2 precursor, denoted as P3, tap density 0.55 g / cm 3 , specific surface area 76m 2 / g, and the length of the lamellar primary grains is about 0.65μm.

[0093] This embodiment also provides a method for preparing a single-crystal lithium-rich manganese-based positive electrode material, comprising the following steps:

[0094] (1) Molar ratio Li:(Ni+Mn+Co)=1.5:1 1000g P3 precursor and corresponding weight of lithium carbonate were weighed, mixed evenly in a high-speed mixer, put into a sagger and put into a box furnace, heated at a rate of 5°C / min, first heated to 500°C, kept at this temperature for 3 hours, then heated to 1000°C at a rate of 5°C / min, calcined for 10 hours, cooled to room temperature with the furnace, and then crushed into 4.1μm by a jet mill. The average primary grain size was 0.65-0.8μm, and the particle morphology was single crystal-like, recorded as RL3;

[0095] (2) Add 5 L of 1 mol / L boric acid solution to a stirring container, add 500 g of RL3 while stirring, continue stirring for 4 hours after addition, then quickly filter, dry at 100 ° C for 24 hours, calcine at 600 ° C for 6 hours, cool to room temperature with the furnace, and use a mechanical crusher to crush to an average particle size D50 of 4.0 μm to obtain a single-crystal lithium-rich manganese-based positive electrode material, recorded as RL-T3.

[0096] Example 4

[0097] This embodiment provides a method for preparing a single-crystal-like lithium-rich manganese-based positive electrode material precursor, comprising the following steps:

[0098] Nickel sulfate, manganese sulfate and cobalt sulfate were dissolved into a mixed salt solution with a molar ratio of Ni:Mn:Co=5:14:1 to form a 1 mol / L mixed salt solution, a mixed alkali solution (i.e., a composite precipitant) of 2 mol / L sodium hydroxide and 0.1 mol / L sodium carbonate, a 10 mol / L ammonia water (i.e., a complexing agent), and a 3 mol / L sodium persulfate solution (oxidant) were prepared; 10 L of pure water and 5 L of ammonia solution were added to a 100 L reactor, and then several liters of the mixed alkali solution were added to adjust the pH value to 11.4-11.6, the reactor temperature was controlled at 30°C, and the mixture was stirred and rotated for 2 hours. The mixed salt solution, mixed alkali solution, complexing agent and oxidant were pumped into the reactor at the same time at a speed of 500rpm. The flow rates of the mixed salt solution, complexing agent and oxidant were fixed. The flow rate of the mixed alkali solution was adjusted to control the pH value at 11.4-11.6. After 4 hours of reaction, the pH value was reduced to 10.8-11.0, the flow rates of the four solutions were stabilized, and the pH fluctuation range was controlled within ±0.1. The coprecipitation reaction was carried out by a continuous method. The ammonium concentration in the system was 0.5g / L. The solution was stopped after the particles grew to 4.0μm. The reaction temperature was increased to 90°C, and stirring and temperature crystallization were maintained for 1 hour. The reaction product was filtered, washed and dried to obtain Ni 0.25 Mn 0.7 0Co 0.05 The (OH)2 precursor, denoted as P4, has an average particle size D50 of 4.5 μm and a tap density of 0.51 g / cm 3, specific surface area 88m 2 / g, and the length of the lamellar primary grains is about 0.5 to 0.65 μm.

[0099] This embodiment also provides a method for preparing a single-crystal-like lithium-rich manganese-based positive electrode material, comprising the following steps:

[0100] (1) Molar ratio Li:(Ni+Mn+Co)=1.45:1 1000g P4 precursor and corresponding weight of lithium carbonate were weighed, mixed evenly in a high-speed mixer, put into a sagger and put into a box furnace, heated at a rate of 5°C / min, first heated to 500°C, kept at this temperature for 3 hours, then heated to 1000°C at a rate of 5°C / min, calcined for 10 hours, cooled to room temperature with the furnace, and then crushed into 4.0μm by a jet mill. The average primary grain size was 0.5-0.6μm, and the particle morphology was in a single crystal-like state, denoted as RL4;

[0101] (2) Add 5 L of 1 mol / L boric acid solution to a stirring container, add 500 g of RL4 while stirring, continue stirring for 4 hours after addition, then quickly filter, dry at 100 ° C for 24 hours, calcine at 600 ° C for 6 hours, cool to room temperature with the furnace, and use a mechanical crusher to crush to an average particle size D50 of 4.0 μm to obtain a single-crystal lithium-rich manganese-based positive electrode material, recorded as RL-T4.

[0102] Example 5

[0103] This embodiment provides a method for preparing a single-crystal-like lithium-rich manganese-based positive electrode material precursor, comprising the following steps:

[0104] Nickel nitrate, manganese nitrate and cobalt nitrate were dissolved into a mixed salt solution with a molar ratio of Ni:Mn:Co=5:13:2, and a mixed alkali solution with a concentration of 8mol / L sodium hydroxide and 2mol / L sodium carbonate (i.e., a composite precipitant), 10mol / L 80% ammonia water and 20% glutamic acid solution (i.e., a complexing agent), and 3mol / L ammonium persulfate solution (oxidant) were prepared; 10L pure water was added into a 100L reactor, and 5L 80% ammonia water and 20% glutamic acid solution, and then add several liters of mixed alkali solution to adjust the pH value to 11.4-11.6, control the temperature of the reactor to 15°C, stir at 500rpm, pump the mixed salt solution, mixed alkali solution, complexing agent and oxidant into the reactor at the same time, fix the flow rate of the mixed salt solution, complexing agent and oxidant, adjust the flow rate of the mixed alkali solution to control the pH value at 11.4-11.6, react for 4 hours, reduce the pH value to 9.5-10.0, stabilize the flow rate of the four solutions, control the pH fluctuation range within ±0.1, use the intermittent method to carry out the coprecipitation reaction, the ammonium concentration in the system is 1g / L, stop pumping the solution until the particles grow to 5.0μm, increase the reaction temperature to 80°C, and keep stirring and temperature crystallization for 24 hours. The reaction product is filtered, washed and dried to obtain Ni 0.25 Mn 0.65 Co 0.10 The (OH)2 precursor, denoted as P5, has an average particle size D50 of 5.0 μm and a tap density of 0.50 g / cm 3 , specific surface area 102m 2 / g, and the length of the lamellar primary grains is about 0.35μm.

[0105] This embodiment also provides a method for preparing a single-crystal-like lithium-rich manganese-based positive electrode material, comprising the following steps:

[0106] (1) 1000 g of P5 precursor and corresponding weight of lithium carbonate were weighed at a molar ratio of Li:(Ni+Mn+Co)=1.4:1, mixed evenly in a high-speed mixer, and then placed in a sagger and placed in a box furnace. The temperature was raised to 500°C at a rate of 5°C / min, and the temperature was kept at this temperature for 3 hours. The temperature was then raised to 950°C at a rate of 5°C / min, and the mixture was calcined for 10 hours. After the mixture was cooled to room temperature in the furnace, the sintered material was crushed to 4.0 μm using a jet mill. The average primary grain size was 0.35-0.5 μm, and the particle morphology was in a single crystal-like state, which was recorded as RL5.

[0107] (2) Add 5 L of 1 mol / L boric acid solution to a stirring container, add 500 g of RL5 while stirring, continue stirring for 4 hours after addition, then quickly filter, dry at 100 ° C for 24 hours, calcine at 600 ° C for 6 hours, cool to room temperature with the furnace, and use a mechanical crusher to crush to an average particle size D50 of 4.0 μm to obtain a single-crystal lithium-rich manganese-based positive electrode material, recorded as RL-T5.

[0108] Example 6

[0109] This embodiment provides a method for preparing a single-crystal-like lithium-rich manganese-based positive electrode material precursor, comprising the following steps:

[0110] Nickel sulfate, manganese sulfate and cobalt sulfate were dissolved into a mixed salt solution with a molar ratio of Ni:Mn:Co=2:7:1, and a mixed alkali solution (i.e., a composite precipitant) of 10 mol / L sodium hydroxide and 1 mol / L sodium carbonate, a 10 mol / L ammonia water (i.e., a complexing agent), and a 2 mol / L ammonium persulfate solution (oxidant) were prepared; 10 L of pure water and 5 L of ammonia water were added to a 100 L reactor, and then several liters of the mixed alkali solution were added to adjust the pH value to 10.9-11.1, the reactor temperature was controlled at 25°C, and the stirring speed was 250°C. 500rpm, the mixed salt solution, mixed alkali solution, complexing agent and oxidant are pumped into the reactor at the same time, the flow rate of the mixed salt solution, complexing agent and oxidant is fixed, the flow rate of the mixed alkali solution is adjusted to control the pH value at 10.9-11.1, after 4 hours of reaction, the pH value is reduced to 10.0-10.5, the flow rate of the four solutions is stabilized, and the pH fluctuation range is controlled within ±0.1. The coprecipitation reaction is carried out by intermittent method, and the ammonium concentration in the system is 3g / L. Stop pumping the solution until the particles grow to 5.0μm, increase the reaction temperature to 85℃, and keep stirring and temperature crystallization for 12 hours. The reaction product is filtered, washed and dried to obtain Ni 0.20 Mn 0.70 Co 0.10 The (OH)2 precursor, denoted as P6, has an average particle size D50 of 4.0 μm and a tap density of 1.1 g / cm 3 , specific surface area 98m 2 / g, and the length of the lamellar primary grains is about 1.0μm.

[0111] This embodiment also provides a method for preparing a single-crystal-like lithium-rich manganese-based positive electrode material, comprising the following steps:

[0112] (1) 1000 g of P6 precursor and corresponding weight of lithium carbonate were weighed at a molar ratio of Li:(Ni+Mn+Co)=1.45:1, mixed evenly in a high-speed mixer, and then placed in a sagger and placed in a box furnace. The temperature was raised to 500°C at a rate of 5°C / min, and the temperature was kept at this temperature for 3 hours. The temperature was then raised to 850°C at a rate of 5°C / min, and the calcination was performed for 10 hours. After the sintering material was cooled to room temperature in the furnace, it was crushed to 4.5 μm using a jet mill. The average primary grain size was 0.8-1.0 μm, and the particle morphology was in a single crystal-like state, which was recorded as RL6.

[0113] (2) Add 5 L of 1 mol / L boric acid solution to a stirring container, add 500 g of RL6 while stirring, continue stirring for 4 hours after addition, then quickly filter, dry at 100 ° C for 24 hours, calcine at 600 ° C for 6 hours, cool to room temperature with the furnace, and use a mechanical crusher to crush to an average particle size D50 of 4.0 μm to obtain a single-crystal lithium-rich manganese-based material, recorded as RL-T6.

[0114] Example 7

[0115] The only difference between this embodiment and embodiment 1 is that the molar ratio of hydroxide to carbonate in the mixed alkaline solution is adjusted to 1.5:1.

[0116] Example 8

[0117] The only difference between this embodiment and embodiment 1 is that the molar ratio of hydroxide to carbonate in the mixed alkaline solution is adjusted to 10.5:1, and the sintering temperature is adjusted to 900°C.

[0118] Comparative Example 1

[0119] This comparative example provides a method for preparing a single-crystal lithium-rich manganese-based positive electrode material precursor, comprising the following steps:

[0120] Dissolve nickel sulfate and manganese sulfate in a molar ratio of Ni:Mn=1:3 into a mixed salt solution with a concentration of 2 mol / L, prepare a sodium hydroxide solution with a concentration of 10 mol / L (i.e., a precipitant) and an ammonia solution with a concentration of 10 mol / L (i.e., a complexing agent); add 10 L of pure water and 5 L of ammonia solution into a 100 L reactor, and then add several liters of sodium hydroxide solution to adjust the pH value to 11.5-12.0, control the reactor temperature to 60°C, stir at 500 rpm, and pump the mixed salt solution, sodium hydroxide solution and complexing agent into the reactor at the same time, The flow rates of the mixed salt solution and the complexing agent were fixed, and the flow rate of the sodium hydroxide solution was adjusted to control the pH value to be between 11.5 and 12.0. After reacting for 4 hours, the pH value was reduced to 10.8 to 11.0, and the flow rates of the three solutions were stabilized, and the pH fluctuation range was controlled within ±0.1. In a nitrogen atmosphere, a coprecipitation reaction was carried out by an intermittent method, and the ammonium concentration in the system was 5 g / L. The solution was stopped from being pumped until the particles grew to 4.0 μm, and the reaction temperature was increased to 60°C, and stirring and temperature crystallization were maintained for 4 hours; the reaction product was filtered, washed and dried to obtain Ni 0.25 Mn 0.75 The (OH)2 precursor, denoted as P7, has an average particle size D50 of 4.0 μm and a tap density of 1.5 g / cm 3 , specific surface area 15m 2 / g, and the length of the lamellar primary grains is about 1.5μm.

[0121] This comparative example also provides a method for preparing a single-crystalline lithium-rich manganese-based positive electrode material. The only difference from Example 1 is that the P1 precursor is replaced by the P7 precursor, and the mechanical crusher is adjusted so that the average particle size D50 of the single-crystalline lithium-rich manganese-based positive electrode material (denoted as RL-T7) is 4.0 μm.

[0122] Comparative Example 2

[0123] This comparative example provides a method for preparing a single-crystal lithium-rich manganese-based positive electrode material precursor, comprising the following steps:

[0124] Nickel sulfate and manganese sulfate were dissolved in a molar ratio of Ni:Mn=1:3 to form a mixed salt solution with a concentration of 2 mol / L, and a sodium hydroxide solution with a concentration of 10 mol / L (i.e., a precipitant) and ammonia water with a concentration of 15 mol / L (i.e., a complexing agent) were prepared; 10 L of pure water and 5 L of ammonia water were added to a 100 L reactor, and then several liters of sodium hydroxide solution were added to adjust the pH value to 11.3-11.5, the reactor temperature was controlled at 55°C, the stirring speed was 500 rpm, and the mixed salt solution, sodium hydroxide solution and complexing agent were mixed. The agent was pumped into the reactor at the same time, the flow rate of the mixed salt solution and the complexing agent was fixed, the flow rate of the sodium hydroxide solution was adjusted to control the pH value at 11.3-11.5, and after 4 hours of reaction, the pH value was reduced to 10.8-11.0, the flow rate of the three solutions was stabilized, and the pH fluctuation range was controlled within ±0.1. In a nitrogen atmosphere, the coprecipitation reaction was carried out by an intermittent method, and the ammonium concentration in the system was 8g / L. The solution was stopped after the particles grew to 4.0μm, and the reaction temperature was increased to 55°C. Stirring and temperature crystallization were maintained for 4 hours. The reaction product was filtered, washed and dried to obtain Ni 0.25 Mn 0.75 The (OH)2 precursor, denoted as P8, has an average particle size D50 of 4.0 μm and a tap density of 1.7 g / cm 3 , specific surface area 10m 2 / g, and the length of the lamellar primary grains is about 2μm.

[0125] This comparative example also provides a method for preparing a single-crystalline lithium-rich manganese-based positive electrode material. The only difference from Example 1 is that the P1 precursor is replaced by the P8 precursor, and the mechanical crusher is adjusted so that the average particle size D50 of the single-crystalline lithium-rich manganese-based positive electrode material (denoted as RL-T8) is 7.5 μm.

[0126] Comparative Example 3

[0127] This comparative example provides a method for preparing a single crystal or quasi-single crystal lithium-rich manganese-based positive electrode material precursor, comprising the following steps:

[0128] Nickel sulfate and manganese sulfate are dissolved into a mixed salt solution with a molar ratio of Ni:Mn=1:3 to form a 2 mol / L concentration, and a sodium hydroxide solution (i.e., a precipitant) with a concentration of 10 mol / L and ammonia water (i.e., a complexing agent) with a concentration of 15 mol / L are prepared; 10 L of pure water and 5 L of ammonia water are added to a 100 L reactor, and then several liters of sodium hydroxide solution are added to adjust the pH value to 11.3-11.5, the reactor temperature is controlled at 50° C., the stirring speed is 500 rpm, the mixed salt solution, the sodium hydroxide solution and the complexing agent are pumped into the reactor at the same time, the flow rates of the mixed salt solution and the complexing agent are fixed, the flow rate of the sodium hydroxide solution is adjusted to control the pH value to 11.3-11.5, the flow rates of the three solutions are stabilized, and the pH fluctuation range is controlled to be within ±0.1, and a coprecipitation reaction is carried out by an intermittent method under an air atmosphere, the ammonium concentration in the system is 6 g / L, and the solution is stopped from being pumped in after the particles grow to 4.0 μm, the reaction temperature is maintained at 50° C., and stirring is maintained for 4 hours. The reaction product is filtered, washed and dried to obtain Ni 0.25 Mn 0.75 The (OH)2 precursor, denoted as P8, has an average particle size D50 of 5.0 μm and a tap density of 1.4 g / cm 3 , specific surface area 16m 2 / g, and the length of the lamellar primary grains is about 1.2μm.

[0129] This comparative example also provides a method for preparing a single-crystalline lithium-rich manganese-based positive electrode material. The only difference from Example 1 is that the P1 precursor is replaced by the P8 precursor, and the mechanical crusher is adjusted so that the average particle size D50 of the single-crystalline lithium-rich manganese-based positive electrode material (denoted as RL-T8) is 4.5 μm.

[0130] Performance Testing

[0131] (1) Specific surface area test

[0132] The specific surface area of ​​the cathode material precursors provided in Examples 1-8 and Comparative Examples 1-3 was tested using a Tristar 3020 instrument.

[0133] The test results are shown in Table 1.

[0134] (2) Compaction density test

[0135] The positive electrode materials provided by Examples 1-8 and Comparative Examples 1-3 were dissolved in N-methylpyrrolidone with a conductive glue and a mass ratio of 9:10:2.4 to obtain a slurry. A scraper with a thickness of 200 μm was used to apply the slurry on the surface of an aluminum foil with a thickness of 20 μm. After drying, the slurry was rolled at a rolling pressure of 130 tons to obtain a positive electrode plate. The surface density and thickness of the plate were measured, and the compacted density = plate surface density / plate thickness.

[0136] The test results are shown in Table 1.

[0137] (3) Charge and discharge test

[0138] The positive electrode sheets, Ube Industries separators and lithium metal negative electrodes corresponding to Examples 1-8 and Comparative Examples 1-3 were assembled into lithium-ion half-cells, wherein the electrolyte was HR8825.

[0139] In the voltage range of 2.0~4.8V, 0.1C charging and 0.1C discharging.

[0140] The test results are shown in Table 1.

[0141] Table 1

[0142]

[0143] analyze:

[0144] It can be seen from the data results of Examples 1-6 that the present invention uses a composite precipitant to carry out a co-precipitation reaction. Through the synergistic effect of the alkaline substance and the soluble carbonate in the composite precipitant, the specific surface area and activity of the precursor can be increased, thereby enabling the single-crystal lithium-rich manganese-based positive electrode material to have excellent comprehensive performance, that is, it has both a high compaction density and a high discharge specific energy.

[0145] From the data results of Example 1 and Example 7-8, it can be seen that if the molar ratio of the alkaline substance to the soluble carbonate in the composite precipitant is too small, the precursor will be mainly carbonate, the product structure will be loose after sintering, and the rolling density will be low; if the molar ratio of the alkaline substance to the soluble carbonate in the composite precipitant is too large, the precursor particles will be too dense and the discharge capacity of the sintered product will be low. In addition, lowering the sintering temperature to increase the capacity and the particle morphology will become polycrystalline, which will also cause a decrease in rolling density.

[0146] It can be seen from the data results of Examples 1-6 and Comparative Examples 1-2 that if the atmosphere of the coprecipitation reaction is an inert atmosphere, the precursor crystal structure will be too dense, and the discharge capacity will be low due to the low conductivity of the lithium-rich manganese-based material.

[0147] It can be seen from the data results of Examples 1-6 and Comparative Examples 1-3 that if a conventional alkaline solution precipitant is used for the co-precipitation reaction, the precursor will all exist in the form of hydroxide, the crystal density is high, and the capacity of the product after sintering is greatly reduced.

[0148] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a single crystal or quasi-single crystal lithium-rich manganese-based cathode material precursor, It is characterized in that The preparation method comprises: The metal salt solution, the composite precipitant, the complexing agent and the oxidant are introduced into the reaction container in parallel to perform a coprecipitation reaction, and then crystallize to obtain the lithium-rich manganese-based positive electrode material precursor; Wherein, the metal salt in the metal salt solution includes manganese salt and M salt, and the M salt includes nickel salt and / or cobalt salt; The composite precipitant comprises a solution containing an alkaline substance and a soluble carbonate, wherein the concentration of the alkaline substance is 2-10 mol / L, the concentration of the carbonate ion is 1-5 mol / L, and the molar ratio of the hydroxide ion to the carbonate ion is (2-10):1; The oxidant is at least one of hydrogen peroxide, sodium hypochlorite, ammonium persulfate, potassium persulfate, sodium persulfate and potassium permanganate; The temperature of the coprecipitation reaction is 15-65°C; The crystallization process is accompanied by stirring; the crystallization temperature is 50-90° C., and the crystallization time is 1-24 hours.

2. The preparation method according to claim 1, It is characterized in that The alkaline substance includes at least one of sodium hydroxide, potassium hydroxide and lithium hydroxide.

3. The preparation method according to claim 1, It is characterized in that The soluble carbonate includes at least one of sodium carbonate, ammonium carbonate, ammonium bicarbonate and sodium bicarbonate.

4. The preparation method according to claim 1, It is characterized in that In the metal salt solution, the concentration of the metal salt is 0.5-3 mol / L.

5. The preparation method according to claim 1, It is characterized in that The complexing agent includes at least one of ammonia water, ammonium carbonate, ammonium bicarbonate, glutamic acid, ammonium citrate, disodium ethylenediaminetetraacetate and citric acid.

6. The preparation method according to claim 1, It is characterized in that The pH value of the coprecipitation reaction is 9-12.

5.

7. The preparation method according to claim 1, It is characterized in that In the reaction system of the coprecipitation reaction, the concentration of ammonium ions is 0.5-3 g / L.

8. A single crystal or quasi-single crystal lithium-rich manganese-based cathode material precursor, It is characterized in that The lithium-rich manganese-based positive electrode material precursor is prepared by the preparation method described in any one of claims 1-7.

9. The single crystal or quasi-single crystal lithium-rich manganese-based cathode material precursor according to claim 8, It is characterized in that The particle size D50 of the lithium-rich manganese-based positive electrode material precursor is 3-9 mm.

10. The single crystal or quasi-single crystal lithium-rich manganese-based cathode material precursor according to claim 8, It is characterized in that The primary grain length of the lithium-rich manganese-based positive electrode material precursor is 0.35-1.0 mm.

11. The single crystal or quasi-single crystal lithium-rich manganese-based cathode material precursor according to claim 8, It is characterized in that The specific surface area of ​​the lithium-rich manganese-based positive electrode material precursor is 20-100 m 2 / g.

12. The single crystal or quasi-single crystal lithium-rich manganese-based cathode material precursor according to claim 8, It is characterized in that The tap density of the lithium-rich manganese-based positive electrode material precursor is 0.5-1.2 g / cm 3 .

13. A single crystal or quasi-single crystal lithium-rich manganese-based positive electrode material, It is characterized in that The lithium-rich manganese-based positive electrode material is obtained by mixing and sintering a single crystal or quasi-single crystal lithium-rich manganese-based positive electrode material precursor as described in any one of claims 8 to 12 and a lithium source.

14. The single crystal or quasi-single crystal lithium-rich manganese-based positive electrode material according to claim 13, It is characterized in that The chemical formula of the lithium-rich manganese-based positive electrode material is Li[Li a (Mn x Ni y Co z ) 1−a ]O 2 , where 0 <a<0.5,x+y+z=1,0≤y<x,0≤z<x,x<1,0≤y≤0.5,0≤z≤0.5。 15. The single crystal or quasi-single crystal lithium-rich manganese-based positive electrode material according to claim 13, It is characterized in that The primary grain length of the lithium-rich manganese-based positive electrode material is 0.35-1.0 mm.

16. The single crystal or quasi-single crystal lithium-rich manganese-based positive electrode material according to claim 13, It is characterized in that The sintering is a step-by-step sintering, which includes a primary sintering and a secondary sintering performed sequentially.

17. The single crystal or quasi-single crystal lithium-rich manganese-based positive electrode material according to claim 16, It is characterized in that The primary sintering temperature is 300-600° C., and the primary sintering time is 2-6 hours.

18. The single crystal or quasi-single crystal lithium-rich manganese-based positive electrode material according to claim 16, It is characterized in that The temperature of the secondary sintering is 850-1100° C., and the time of the secondary sintering is 6-18 hours.

19. The single crystal or quasi-single crystal lithium-rich manganese-based positive electrode material according to claim 13, It is characterized in that After the sintering, the sintered product is post-treated to obtain the lithium-rich manganese-based positive electrode material.

20. The single crystal or quasi-single crystal lithium-rich manganese-based positive electrode material according to claim 19, It is characterized in that The post-treatment includes acid washing and calcination performed in sequence.

21. The single crystal or quasi-single crystal lithium-rich manganese-based positive electrode material according to claim 20, It is characterized in that The calcination temperature is 350-600° C., and the calcination time is 2-6 hours.

22. A lithium secondary battery, It is characterized in that The positive electrode of the lithium secondary battery comprises the single crystal or quasi-single crystal lithium-rich manganese-based positive electrode material according to any one of claims 13 to 21.

Citation Information

Patent Citations

  • Layer-structured ternary material with rich lithium and high manganese as well as preparation method and application thereof

    CN102832387B

  • Preparation method of lithium-rich manganese-base anode material

    CN103972491A

  • Preparation method for lithium-rich manganese based anode material hydroxide precursor

    CN104752709A

  • Preparation method of lithium-rich manganese-based positive electrode material

    CN111170377A

  • Preparation method of lithium-rich manganese-based positive electrode material

    CN111640931A