A method for preparing electronic ink with high contrast and long stable time
Modification of electrophoretic particles through silane coupling agent grafting and polymer coating technology solves the problems of insufficient contrast and steady-state time of electronic ink, significantly improves the performance of electronic ink, and realizes electronic ink with high contrast and long steady-state time. Ink preparation improves the display effect and durability of electrophoretic display devices.
Patent Information
- Application Number
- CN202410111801.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-26
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-01-26
AI Technical Summary
The existing electronic ink has low contrast and short steady-state time, which limits the development of electronic paper technology. This is mainly due to the unstable dispersion caused by the density difference and poor compatibility between the electrophoretic particles and the electrophoretic medium.
The electrophoretic particles are grafted and modified with a silane coupling agent and coated with a polymer to increase the covering power and compatibility of the particles, reduce the density, form a cross-linked layer to protect the charge, and improve the steady-state time.
It significantly improves the contrast and steady-state time of electronic ink, reduces leakage current, and significantly improves the display effect and durability of electrophoretic display devices.
Smart Images

Figure CN117930556B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electrophoretic display, and in particular to a method for preparing electronic ink with high contrast and long stable time. Background Art
[0002] Electronic paper is a technology applied to electrophoretic display, which aims to simulate paper-like reflective and flexible display. Unlike traditional LCD screens, electronic paper technology does not require a backlight source and does not actively emit light. Instead, it displays based on reflected ambient light, which has the advantage of eye protection. In addition, based on the bi-stable characteristics of electronic paper, electronic paper only consumes power when the page is refreshed, and almost no power is consumed when the display state is maintained, which makes electronic paper display technology have the advantages of low power consumption and environmental protection.
[0003] Electronic ink is the core of electronic paper display devices. Electronic ink is composed of electrophoretic particles and electrophoretic medium. The electrophoretic particles largely determine the reflectivity, contrast, response speed and steady-state time of electronic paper display devices. At present, contrast and steady-state time are a major problem restricting the development of electronic paper technology. Commonly used electrophoretic particles such as titanium oxide, aluminum oxide, iron manganese black, copper chromium black, etc. are difficult to disperse stably due to the large difference in density with the electrophoretic medium and poor compatibility, resulting in low contrast and poor steady-state time of electrophoretic display devices made based on existing particles. In view of the above problems, the present invention provides a method for preparing electronic ink with high contrast and long steady-state time. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing electronic ink with high contrast and long stable time. The electronic ink is prepared by coating an organic polymer and can be used in an electrophoretic display device to improve its contrast and stable time.
[0005] To achieve the above object, the present invention provides a method for preparing electronic ink with high contrast and long stable time, comprising the following steps:
[0006] S1, Silane coupling agent grafted modified electrophoretic particle raw materials
[0007] Take a mixed solvent of ethanol and water, adjust the pH with ammonia water, add the raw material of electrophoretic particles, then add the silane coupling agent and zirconium beads, ball mill, transfer the ball milling solution to a four-necked flask, stir, heat to 85°C for reaction, centrifuge and wash after the reaction is completed, and vacuum dry to obtain the modified electrophoretic particles after the silane coupling agent grafting treatment;
[0008] S2. Polymer-coated modified electrophoretic particles
[0009] The modified electrophoretic particles, solvent, monomer 1, monomer 2, monomer 3, monomer 4 and zirconium beads are ball-milled, and the ball-milled solution is transferred to a four-necked flask and stirred, and then the initiator is added after heating to 50° C., and then the temperature is heated to 70-85° C. for reaction. After the reaction is completed, the temperature is cooled to room temperature, and monomer 3 is added. After stirring and heating to 50° C. again, the initiator is added, and then the temperature is heated to 70-85° C. for reaction. After the reaction is completed, the modified electrophoretic particles are washed by centrifugation and vacuum drying to obtain the modified electrophoretic particles after polymer coating treatment;
[0010] S3. Preparation of electronic ink
[0011] The modified electrophoretic particles coated with the polymer prepared above are mixed with a charge control agent and an electrophoretic medium to obtain electronic ink.
[0012] Preferably, in step S1, the mixture comprises, by weight, 10 to 20 parts of a mixed solvent, 1 part of an electrophoretic particle raw material, 0.1 to 0.5 parts of a silane coupling agent, and 5 to 20 parts of zirconium beads;
[0013] The pH value of the mixed solvent is adjusted to 7-10, ball milled for 5-12 hours, mechanically stirred for reaction at 200-400 rpm for 5-10 hours, and vacuum dried at 100°C.
[0014] Preferably, in step S2, the components include, by weight, 1 part of modified electrophoretic particles, 10 to 20 parts of solvent, 0.1 to 0.1 parts of monomer 1, 0.1 to 1 parts of monomer 2, 0.2 to 2 parts of monomer 3, 0.01 to 0.1 parts of monomer 4, and 5 to 20 parts of zirconium beads;
[0015] Ball milling for 5 to 12 hours, mechanical stirring at 200 to 500 rpm under inert gas protection, and vacuum drying at 100°C for 5 to 12 hours;
[0016] The mass of the initiator is 0.5-5% of the total mass of the monomers.
[0017] Preferably, the raw material of the electrophoretic particles in step S1 is electrophoretic black and white particles, wherein the electrophoretic black particles are one or more of iron manganese black, copper chromium black, and carbon black; and the electrophoretic white particles are one or more of titanium oxide, aluminum oxide, calcium carbonate, and barium sulfate.
[0018] Preferably, the silane coupling agent in step S1 is one of γ-(methacryloyloxy)propyltrimethoxysilane, trimethoxy(7-octen-1-yl)silane, 10-undecenyltrichlorosilane, and [3-(triethoxysilyl)propyl]carbamic acid 2-propynyl ester.
[0019] Preferably, the solvent in step S2 is one of ethanol, isopropanol, toluene, cyclohexane, Isopar L, and Isopar G.
[0020] Preferably, the monomer 1 and the monomer 2 in step S2 are both one of styrene, methyl acrylate, methyl methacrylate, butyl methacrylate, dodecyl methacrylate, octadecyl methacrylate, acrylic acid, acrylamide, oleic acid, and oleylamine;
[0021] Monomer 3 and monomer 4 are both one of isocyanate, divinylbenzene, 1,3-butadiene, N,N-methylenebisacrylamide and diallyldimethylammonium chloride.
[0022] Preferably, the initiator in step S2 is one of benzoyl peroxide, potassium persulfate, azobisisobutyronitrile, and dimethyl azobisisobutyrate.
[0023] Preferably, the charge control agent in step S3 is one of organic sulfate, organic sulfonate, polyester and polyolefin; and the electrophoretic medium is a non-polar solvent.
[0024] Preferably, the non-polar solvent is one of paraffin, isoparaffin, silicone oil, halogenated hydrocarbon and aromatic hydrocarbon.
[0025] Therefore, the method for preparing the electronic ink with high contrast and long stable time adopted by the present invention has the following beneficial effects compared with the prior art:
[0026] (1) Through the method of organic modification, polymers are coated on the surface of electrophoretic particles to increase the covering power of the particles, thereby improving the contrast of the device; the density of the particles is reduced, and the compatibility of the particles and the system is enhanced through the solvation of organic monomers in the system, thereby improving the steady-state time of the device;
[0027] (2) By coating the polymer cross-linking layer, the charge is protected, the leakage current of the system is reduced, and the steady-state time of the electrophoretic display device is increased.
[0028] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is the TGA curve diagram of particles A to D prepared in the present invention;
[0030] Figure 2 This is a TGA curve diagram of the E-H particles prepared in the present invention;
[0031] Figure 3 The time-current curve of the A-D particle dispersion prepared in the present invention;
[0032] Figure 4 The time-current curve of the E-H particle dispersion prepared in the present invention;
[0033] Figure 5 The electrophoretic display device of the present invention, which is prepared by using D and H particles, displays a photograph;
[0034] Figure 6 This is a photograph of the electrophoretic display device prepared by using D and H particles in the present invention, which was left to stand for 24 hours. DETAILED DESCRIPTION
[0035] The following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] Example 1
[0037] The present invention provides a method for preparing electronic ink with high contrast and long stable time, comprising the following steps:
[0038] S1, Silane coupling agent grafted modified electrophoretic white particles
[0039] Take 50g of titanium dioxide raw material A, take 1000mL of a mixed solvent of water and ethanol (volume ratio of 1:1) and adjust the pH of the mixed solvent to 9 with ammonia water, take 10g of γ-(methacryloyloxy)propyltrimethoxysilane, mix the three and add 500g of zirconium beads for ball milling for 12h. After the ball milling is completed, the zirconium beads are removed and the ball milling liquid is transferred to a four-necked flask, mechanically stirred at 85°C and 300rpm for 5h, centrifuged, and vacuum dried at 100°C to obtain modified electrophoretic white particles B after silane coupling agent grafting treatment.
[0040] S2, polymer coated modified electrophoretic white particles:
[0041] Take 10g of the modified electrophoretic white particles B after grafting with the silane coupling agent, 200mL of ethanol, 2.5g of lauryl methacrylate, 2.5g of acrylamide, 1.25g of divinylbenzene, 0.27g of diallyldimethylammonium chloride, and 100g of zirconium beads, and ball mill for 12h. After ball milling, remove the zirconium beads, transfer the ball milling solution to a 500mL four-necked flask, pass Ar gas for 30min, heat to 50°C with mechanical stirring at 300rpm, add 0.0326g of azobisisobutyronitrile, heat to 75°C for reaction for 12h, cool to room temperature, add 1.25g of divinylbenzene, heat to 50°C with mechanical stirring at 300rpm, add 0.00625g of azobisisobutyronitrile, heat to 70-85°C, react for 12h, centrifuge after the reaction, wash several times with water / ethanol as solvent, and dry at 100°C in vacuum for 12h to obtain modified electrophoretic white particles D after polymer coating.
[0042] S3, Silane coupling agent grafted modified electrophoretic black particles
[0043] Take 50g of iron manganese black raw material E, take 1000mL of a mixed solvent of water and ethanol (volume ratio of 1:1) and adjust the pH of the mixed solvent to 9 with ammonia water, take 10g of γ-(methacryloyloxy)propyltrimethoxysilane, mix the three and add 500g of zirconium beads for ball milling for 12h. After the ball milling is completed, the zirconium beads are removed and the ball milling liquid is transferred to a 500mL four-necked flask, mechanically stirred at 85°C and 300rpm for 5h, centrifuged, and vacuum dried at 100°C to obtain modified electrophoretic black particles F after silane coupling agent grafting treatment.
[0044] S4, polymer coated modified electrophoretic black particles
[0045] Take 10g of the modified electrophoretic black particles F after the above-mentioned silane coupling agent grafting treatment, 200mL of ethanol, 5g of lauryl methacrylate, 2.5g of divinylbenzene, 2.5g of acrylic acid, and 100g of zirconium beads, and ball mill for 12h. After the ball milling is completed, the zirconium beads are removed, and the ball milling liquid is transferred to a 500mL four-necked flask, Ar gas is passed for 30min, and the mixture is heated to 50°C with mechanical stirring at 300rpm. 0.5g of azobisisobutyronitrile is added, and the mixture is heated to 75°C for reaction for 12h. The mixture is cooled to room temperature, 2.5g of divinylbenzene is added, and the mixture is heated to 50°C with mechanical stirring at 300rpm. 0.0125g of azobisisobutyronitrile is added, and the mixture is heated to 75°C for reaction for 12h. After the reaction is completed, the mixture is centrifuged, washed several times with ethanol as a solvent, and dried at 100°C in vacuum for 12h to obtain the modified electrophoretic black particles H after polymer coating treatment.
[0046] S5. Preparation of electronic ink
[0047] The polymer-coated modified electrophoretic black particles and the polymer-coated modified electrophoretic white particles prepared above are mixed with the charge control agent Solsperse 17000 and the electrophoretic medium Isopar L to obtain electronic ink.
[0048] Comparative Example 1
[0049] S1, Silane coupling agent grafted modified electrophoretic white particles
[0050] The process is the same as step S1 in embodiment 1 and will not be repeated here.
[0051] S2, polymer coated modified electrophoretic white particles
[0052] Take 10g of the modified electrophoretic white particles B after grafting with the silane coupling agent, 200mL of ethanol, 2.5g of lauryl methacrylate, 2.5g of acrylamide, 1.25g of divinylbenzene, 0.27g of diallyldimethylammonium chloride, and 100g of zirconium beads, and ball mill for 12h. After the ball milling is completed, the zirconium beads are removed, and the ball milling liquid is transferred to a 500mL four-necked flask, and Ar gas is passed for 30min. The mixture is heated to 50°C with mechanical stirring at 300rpm, and 0.0326g of azobisisobutyronitrile is added. The mixture is heated to 75°C for reaction for 12h. After the reaction is completed, the mixture is centrifuged, washed several times with water / ethanol as solvent, and dried at 100°C in vacuum for 12h to obtain particles C after polymer coating.
[0053] S3, Silane coupling agent grafted modified electrophoretic black particles
[0054] The process is the same as step S3 in embodiment 1 and will not be repeated here.
[0055] S4, polymer coated modified electrophoretic black particles:
[0056] Take 10g of the modified electrophoretic black particles F after grafting treatment with the above-mentioned silane coupling agent, 200mL of ethanol, 5g of lauryl methacrylate, 2.5g of divinylbenzene, and 100g of zirconium beads, and ball mill for 12h. After ball milling, remove the zirconium beads, transfer the ball milling solution to a 500mL four-necked flask, pass Ar gas for 30min, heat to 50°C with mechanical stirring at 300rpm, add 0.0375g of azobisisobutyronitrile, heat to 75°C for reaction for 12h, centrifuge after the reaction is completed, wash several times with ethanol as solvent, and dry at 100°C in vacuum for 12h to obtain particles G after polymer coating.
[0057] S5. Preparation of electronic ink
[0058] The polymer-coated modified electrophoretic black particles and the polymer-coated modified electrophoretic white particles prepared above are mixed with the charge control agent Solsperse 17000 and the electrophoretic medium Isopar L to obtain electronic ink.
[0059] Experimental testing
[0060] 10 mg of white particles A to D and black particles E to H were placed in a platinum pan and thermogravimetrically tested in turn. The instrument model used was TA-Q500, the test gas atmosphere was nitrogen, the temperature range was 0 to 800 °C, and the heating rate was 10 °C / min. The results are as follows Figure 1 , Figure 2 As shown by Figure 1 and Figure 2 It can be seen that the white particles and the black particles are successfully grafted with the silane coupling agent, and the weight loss temperatures of the polymer-modified particles C, D, G, and H are concentrated in the range of 300 to 500 °C.
[0061] Take 0.75g of each of A-D particles (0.5g of each of E-H particles), 3.81g of isoparaffin Isopar L, 0.07g of charge control agent Solsperse 170000, and 10g of zirconium beads, add them into a ball mill bottle and ball mill for 2 hours to obtain a white dispersion. Separate two conductive glass sheets of size 100mm×100mm×0.7mm with an insulating film. The film size is 100mm×100mm, and a 22mm×22mm square opening is opened in the middle. Inject the dispersion between the two conductive glass sheets to make a prototype device, and perform a leakage current test. The instrument model used is Keyteley 2400. The results are as follows Figure 3 , Figure 4 As shown by Figure 3 and Figure 4 It can be seen that the leakage current of the dispersion prepared by polymer-modified particles is significantly lower than that of the raw material, among which the leakage current of polymer-modified white particles C and D can be reduced to 0.17μA and 0.015μA; the leakage current of polymer-modified black particles G and H can be reduced to 0.65μA and 0.43μA.
[0062] Take 0.5g of white electrophoretic liquid and 0.1g of black electrophoretic liquid, mix them by ultrasonic for 10 minutes, use the electrophoretic dispersion to support the electrophoretic display prototype device according to the above method (3), and use Xrite Pantone colorimeter to test the white / black state reflectivity of the device. Figure 5 Schematic diagram of the display effect of the electrophoretic display prototype device made of D and H particles. Figure 6 The device is left to stand for 24 hours to display the effect. Figure 5 It can be seen that the initial white state reflectivity of the electrophoretic display prototype device made of D and H particles is 42%, and the initial black state reflectivity is 0.56%. Figure 6 It can be seen that the white state reflectivity after power-off for 24 hours is 31%, and the black state reflectivity is 1.7%.
[0063] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for preparing electronic ink with high contrast and long stable time, characterized in that: The following steps are involved: S1, Silane coupling agent grafted modified electrophoretic particle raw materials Take a mixed solvent of ethanol and water, adjust the pH with ammonia water, add the raw material of electrophoretic particles, then add the silane coupling agent and zirconium beads, ball mill, transfer the ball milling solution to a four-necked flask, stir, heat to 85°C for reaction, centrifuge and wash after the reaction is completed, and vacuum dry to obtain modified electrophoretic particles after silane coupling agent grafting treatment; S2. Polymer-coated modified electrophoretic particles The modified electrophoretic particles, solvent, monomer 1, monomer 2, monomer 3, monomer 4 and zirconium beads are ball-milled, and the ball-milled solution is transferred to a four-necked flask and stirred, and then the initiator is added after heating to 50° C., and then the temperature is heated to 70-85° C. for reaction. After the reaction is completed, the temperature is cooled to room temperature, and monomer 3 is added. After stirring and heating to 50° C. again, the initiator is added, and then the temperature is heated to 70-85° C. for reaction. After the reaction is completed, the modified electrophoretic particles are washed by centrifugation and vacuum drying to obtain the modified electrophoretic particles after polymer coating treatment; S3. Preparation of electronic ink The modified electrophoretic particles coated with the polymer prepared above are mixed with a charge control agent and an electrophoretic medium to obtain electronic ink; The monomer 1 and the monomer 2 in step S2 are each one of styrene, methyl acrylate, methyl methacrylate, butyl methacrylate, dodecyl methacrylate, octadecyl methacrylate, acrylic acid, acrylamide, oleic acid, and oleylamine; Monomer 3 and monomer 4 are both one of isocyanate, divinylbenzene, 1,3-butadiene, N,N-methylenebisacrylamide and diallyldimethylammonium chloride.
2. The method for preparing electronic ink with high contrast and long stable time according to claim 1, characterized in that: In the step S1, the mixture comprises, by weight, 10 to 20 parts of a mixed solvent, 1 part of an electrophoretic particle raw material, 0.1 to 0.5 parts of a silane coupling agent, and 5 to 20 parts of zirconium beads; The pH value of the mixed solvent is adjusted to 7-10, ball milled for 5-12 hours, mechanically stirred for reaction at 200-400 rpm for 5-10 hours, and vacuum dried at 100°C.
3. The method for preparing electronic ink with high contrast and long stable time according to claim 1, characterized in that: In the step S2, the modified electrophoretic particles, 10 to 20 parts of solvent, 0.1 to 0.1 parts of monomer 1, 0.1 to 1 parts of monomer 2, 0.2 to 2 parts of monomer 3, 0.01 to 0.1 parts of monomer 4 and 5 to 20 parts of zirconium beads are included in the step S2. Ball milling for 5 to 12 hours, mechanical stirring at 200 to 500 rpm under inert gas protection, and vacuum drying at 100 ° C for 5 to 12 hours; The mass of the initiator is 0.5-5% of the total mass of the monomers.
4. The method for preparing electronic ink with high contrast and long stable time according to claim 1, characterized in that: The raw material of the electrophoretic particles in step S1 is electrophoretic black and white particles, wherein the electrophoretic black particles are one or more of iron manganese black, copper chromium black, and carbon black; and the electrophoretic white particles are one or more of titanium oxide, aluminum oxide, calcium carbonate, and barium sulfate.
5. The method for preparing electronic ink with high contrast and long stable time according to claim 1, characterized in that: The silane coupling agent in step S1 is one of γ-(methacryloyloxy)propyltrimethoxysilane, trimethoxy(7-octen-1-yl)silane, 10-undecenyltrichlorosilane, and [3-(triethoxysilyl)propyl]carbamic acid 2-propynyl ester.
6. The method for preparing electronic ink with high contrast and long stable time according to claim 1, characterized in that: The solvent in step S2 is one of ethanol, isopropanol, toluene, cyclohexane, Isopar L and Isopar G.
7. The method for preparing electronic ink with high contrast and long stable time according to claim 1, characterized in that: The initiator in step S2 is one of benzoyl peroxide, potassium persulfate, azobisisobutyronitrile and dimethyl azobisisobutyrate.
8. The method for preparing electronic ink with high contrast and long stable time according to claim 1, characterized in that: The charge control agent in step S3 is one of organic sulfate, organic sulfonate, polyester and polyolefin; and the electrophoretic medium is a non-polar solvent.
9. The method for preparing electronic ink with high contrast and long stable time according to claim 8, characterized in that: The non-polar solvent is one of paraffin, isoparaffin, silicone oil, halogenated hydrocarbon and aromatic hydrocarbon.
Citation Information
Patent Citations
Preparation method of electropositive electrophoresis particle
CN102161735A
Electrophoresis display liquid and preparation method for granules of electrophoresis display liquid
CN102591086A
Electrophoresis display particles as well as preparation method and application thereof
CN103173040A
Black particle, black electrophoretic particle, preparation method and application
CN116354404A
Quick-response electronic ink, preparation method and electrophoretic display device with high refresh rate
CN116496663A