A hydrogel dressing for promoting wound healing and preparation method thereof
By using hydrogel dressings with ingredients such as modified gluten and retinol-binding protein, the problem of difficulty in absorbing wound exudate in existing dressings has been solved, improving wound healing and fluid absorption performance, and reducing the frequency of replacement. , reduces patient pain, has low cytotoxicity and is suitable for industrial production.
Patent Information
- Application Number
- CN202410354394.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-03-27
AI Technical Summary
Existing medical dressings are difficult to effectively absorb exudate when treating burn or scald wounds, resulting in frequent replacement, increasing patient pain, and possibly causing secondary damage to the wound surface.
A hydrogel dressing composed of hydroxypropyl cellulose, carboxymethyl chitosan, sodium hyaluronate, recombinant human bone morphogenetic protein, retinol-binding protein and modified gluten powder is used through enzymatic hydrolysis, fermentation and Prepared by sterilization process, it has good liquid absorption properties and low cytotoxicity.
The hydrogel dressing significantly improves liquid absorption performance, reduces the frequency of replacement, relieves patient pain, and promotes wound healing through the synergistic effect of retinol-binding protein and recombinant human bone morphogenetic protein, and the preparation method is simple and suitable for industrial production .
Smart Images

Figure CN117942425B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of medical dressings, and particularly relates to a hydrogel dressing for promoting wound healing and a preparation method thereof. Background Art
[0002] The human body's natural protective barrier is the skin tissue covering its surface. Skin tissue plays an important role in preventing the body from dehydration and protecting internal organs from external damage. If the skin is severely damaged, such as burns and scalds, the skin will lose its protective function, thus forming wounds. The formation of wounds may cause damage to the body, such as: drop in body temperature, rapid loss of water, immune system disorders, etc. The treatment method for wounds is usually to cover the wound with medical dressings to promote wound healing. The medical dressings used in the early days included gauze, cotton pads, etc., which have the characteristics of good hemostatic effect, low price, and simple preparation process. However, this type of medical dressing is easy to adhere to the wound, and the new tissue often falls off when replaced, which will cause secondary damage to the wound.
[0003] With the development of science and technology, the choice of medical dressings is becoming increasingly rich, and more medical dressings are being developed and researched. Hydrogel is a swollen body with a three-dimensional network structure, which is obtained by cross-linking hydrophilic polymer compounds. It has the advantages of high water content, high compressive strength, and good biocompatibility. It also meets the requirements of an ideal dressing and has attracted much attention in technical fields such as trauma dressings and tissue engineering scaffolds. However, wounds caused by burns and scalds have a lot of exudate in the wound. If the exudate cannot be absorbed in time, it will seriously affect the healing of the wound and require frequent dressing changes, which also increases the pain of the patient. Therefore, it is urgent to develop a new type of hydrogel dressing. Summary of the invention
[0004] The first object of the present invention is to provide a hydrogel dressing for promoting wound healing, which promotes wound healing and has good liquid absorption performance.
[0005] The second purpose of the present invention is to provide a method for preparing a hydrogel dressing for promoting wound healing, which has a simple process and is conducive to industrial production.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] A hydrogel dressing for promoting wound healing, comprising the following raw materials in parts by weight: 1-5 parts of hydroxypropyl cellulose, 5-10 parts of carboxymethyl chitosan, 3-8 parts of sodium hyaluronate, 0.1-0.5 parts of recombinant human bone morphogenetic protein 4, 0.1-0.5 parts of retinol binding protein, 3-5 parts of modified gluten powder, and 90-100 parts of water;
[0008] The preparation steps of the modified gluten are as follows:
[0009] A: Take gluten powder and add it into water, then add glutamine transaminase for enzymatic hydrolysis;
[0010] B: performing enzyme inactivation and sterilization treatment on the solution after enzymatic hydrolysis in step A to obtain an enzymatic hydrolyzate;
[0011] C: adding bacterial agent to the enzymatic hydrolysate of step B for fermentation, collecting the fermentation liquid, filtering it and freeze-drying it to obtain modified gluten powder.
[0012] Preferably, the enzymatic hydrolysis conditions in step A are: temperature 50-55°C, pH 5-7, and time 100-120 min.
[0013] Preferably, the enzyme inactivation and sterilization process in step B is: enzyme inactivation and sterilization at 85-90° C. for 15-20 min.
[0014] Preferably, in step A, the mass content of gluten in water is 20-30%, and the mass ratio of gluten to transglutaminase is 1:0.1-0.3.
[0015] Preferably, the bacterial agent in step C is Lactobacillus plantarum, and the inoculation amount is 10 6 -10 7 CFU / g.
[0016] Preferably, the fermentation temperature in step C is 37-39° C. and the fermentation time is 60-70 h.
[0017] The preparation method of the hydrogel dressing for promoting wound healing comprises the following steps:
[0018] (1) Weighing raw materials by weight, adding carboxymethyl chitosan, modified gluten powder and hydroxypropyl cellulose into water, stirring and mixing under heat preservation conditions to obtain a mixture;
[0019] (2) Add sodium hyaluronate, recombinant human bone morphogenetic protein 4, and retinol binding protein to the mixture of step (1), stir and mix under heat preservation conditions, and then place at 4-6°C for 1-2 hours. After sterilization, a hydrogel dressing that promotes wound healing is obtained.
[0020] Preferably, the insulation temperature in step (1) is 60-70°C for 3-5 hours, and the insulation temperature in step (2) is 40-50°C for 1-3 hours.
[0021] Compared with the prior art, the beneficial effects of the present invention are mainly:
[0022] The present invention adds retinol binding protein, recombinant human bone morphogenetic protein 4 and modified gluten to the raw materials for preparation. The wound healing and liquid absorption performance of the hydrogel dressing obtained by using the above raw materials are tested and it is found that the synergistic effect of retinol binding protein and recombinant human bone morphogenetic protein 4 can promote wound healing; modified gluten can effectively improve the liquid absorption performance of the hydrogel dressing, thereby reducing the frequency of replacement and alleviating the pain of patients. In addition, the hydrogel dressing of the present invention has low cytotoxicity. The preparation method of the present invention has a simple process and is conducive to industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a graph showing the liquid absorption results of the hydrogel dressings of Examples 1-3 and Comparative Examples 1-6. DETAILED DESCRIPTION
[0024] The technical scheme of the present invention is further described below in conjunction with specific embodiments. However, it should be understood by those skilled in the art that the following examples are only used to illustrate the present invention and should not be regarded as limiting the present invention. The specific conditions not specified in the examples are carried out according to conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, unless otherwise specified, are conventional products obtained through commercial channels.
[0025] Example
[0026] Example 1
[0027] The present embodiment provides a hydrogel dressing for promoting wound healing, which is composed of the following raw materials in parts by weight: 2 parts of hydroxypropyl cellulose, 6 parts of carboxymethyl chitosan, 5 parts of sodium hyaluronate, 0.3 parts of recombinant human bone morphogenetic protein 4, 0.4 parts of retinol binding protein, 4 parts of modified gluten powder, and 97 parts of water.
[0028] The preparation steps of the modified gluten are as follows:
[0029] A: Take gluten powder and add it into water. The mass content of gluten powder in water is 22%. Add gluten aminotransferase at a mass ratio of gluten powder to glutamine aminotransferase of 1:0.2. Perform enzymatic hydrolysis at 52°C and pH 6 for 106 minutes.
[0030] B: The solution after enzymatic hydrolysis in step A is subjected to enzyme inactivation and sterilization treatment at 88°C for 17 minutes to obtain an enzymatic hydrolyzate;
[0031] C: Add Lactobacillus plantarum to the enzymatic hydrolysate of step B. The inoculum amount of Lactobacillus plantarum is 10 6 CFU / g, fermented at 38℃ for 62h, collected the fermentation liquid, filtered it and freeze-dried it to obtain modified gluten powder.
[0032] This embodiment also provides a method for preparing the hydrogel dressing for promoting wound healing, and the preparation steps are as follows:
[0033] (1) Weigh the above raw materials according to weight, add carboxymethyl chitosan, modified gluten powder and hydroxypropyl cellulose into water, and stir and mix at 65° C. for 4 h to obtain a mixture;
[0034] (2) Sodium hyaluronate, recombinant human bone morphogenetic protein 4, and retinol binding protein are added to the mixture of step (1), the mixture is stirred and mixed at 42° C. for 2.1 hours, and the mixture is placed at 4° C. for 2 hours. After sterilization, a hydrogel dressing that promotes wound healing is obtained.
[0035] Example 2
[0036] The present embodiment provides a hydrogel dressing for promoting wound healing, which is composed of the following raw materials in parts by weight: 1 part of hydroxypropyl cellulose, 5 parts of carboxymethyl chitosan, 3 parts of sodium hyaluronate, 0.1 parts of recombinant human bone morphogenetic protein 4, 0.5 parts of retinol binding protein, 3 parts of modified gluten powder, and 100 parts of water.
[0037] The preparation steps of the modified gluten are as follows:
[0038] A: Take gluten and add it into water, the mass content of gluten in water is 20%, add gluten transaminase at a mass ratio of gluten to glutamine transaminase of 1:0.1, and perform enzymolysis at 50°C and pH 5 for 120 minutes;
[0039] B: The solution after enzymatic hydrolysis in step A is subjected to enzyme inactivation and sterilization treatment at 85°C for 20 minutes to obtain an enzymatic hydrolyzate;
[0040] C: Add Lactobacillus plantarum to the enzymatic hydrolysate of step B. The inoculum amount of Lactobacillus plantarum is 10 7 CFU / g, fermented at 37℃ for 70h, collected the fermentation liquid, filtered it and freeze-dried it to obtain modified gluten powder.
[0041] This embodiment also provides a method for preparing the hydrogel dressing for promoting wound healing, and the preparation steps are as follows:
[0042] (1) Weigh the above raw materials according to weight, add carboxymethyl chitosan, modified gluten powder and hydroxypropyl cellulose into water, and stir and mix at 60° C. for 5 h to obtain a mixture;
[0043] (2) Sodium hyaluronate, recombinant human bone morphogenetic protein 4, and retinol binding protein are added to the mixture of step (1), the mixture is stirred and mixed at 40° C. for 3 h, and placed at 5° C. for 1.5 h. After sterilization, a hydrogel dressing that promotes wound healing is obtained.
[0044] Example 3
[0045] The present embodiment provides a hydrogel dressing for promoting wound healing, which is composed of the following raw materials in parts by weight: 5 parts of hydroxypropyl cellulose, 10 parts of carboxymethyl chitosan, 8 parts of sodium hyaluronate, 0.5 parts of recombinant human bone morphogenetic protein 4, 0.1 parts of retinol binding protein, 5 parts of modified gluten powder, and 90 parts of water.
[0046] The preparation steps of the modified gluten are as follows:
[0047] A: Take gluten and add it into water, the mass content of gluten in water is 30%, add gluten transaminase at a mass ratio of gluten to glutamine transaminase of 1:0.3, and enzymolyze for 100 minutes at 55°C and pH 7;
[0048] B: The solution after enzymatic hydrolysis in step A is subjected to enzyme inactivation and sterilization treatment at 90° C. for 15 min to obtain an enzymatic hydrolyzate;
[0049] C: Add Lactobacillus plantarum to the enzymatic hydrolysate of step B. The inoculum amount of Lactobacillus plantarum is 10 6 CFU / g, fermented at 39℃ for 60h, collected the fermentation liquid, filtered it and freeze-dried it to obtain modified gluten powder.
[0050] This embodiment also provides a method for preparing the hydrogel dressing for promoting wound healing, and the preparation steps are as follows:
[0051] (1) Weigh the above raw materials according to weight, add carboxymethyl chitosan, modified gluten powder and hydroxypropyl cellulose into water, and stir and mix at 70° C. for 3 h to obtain a mixture;
[0052] (2) Sodium hyaluronate, recombinant human bone morphogenetic protein 4, and retinol binding protein are added to the mixture of step (1), the mixture is stirred and mixed at 50° C. for 1 hour, and the mixture is placed at 6° C. for 1 hour. After sterilization, a hydrogel dressing that promotes wound healing is obtained.
[0053] Comparative Example
[0054] Comparative Example 1
[0055] The difference between this comparative example and Example 1 is that the hydrogel dressing is composed of the following raw materials in parts by weight: 2 parts of hydroxypropyl cellulose, 6 parts of carboxymethyl chitosan, 5 parts of sodium hyaluronate, 0.4 parts of retinol binding protein, 4 parts of modified gluten powder, and 97 parts of water, and the rest is the same as Example 1.
[0056] Comparative Example 2
[0057] The difference between this comparative example and Example 1 is that the hydrogel dressing is composed of the following raw materials in parts by weight: 2 parts of hydroxypropyl cellulose, 6 parts of carboxymethyl chitosan, 5 parts of sodium hyaluronate, 0.3 parts of recombinant human bone morphogenetic protein 4, 4 parts of modified gluten, and 97 parts of water, and the rest is the same as Example 1.
[0058] Comparative Example 3
[0059] The difference between this comparative example and Example 1 is that the hydrogel dressing is composed of the following raw materials in parts by weight: 2 parts of hydroxypropyl cellulose, 6 parts of carboxymethyl chitosan, 5 parts of sodium hyaluronate, 0.7 parts of recombinant human bone morphogenetic protein 4, 4 parts of modified gluten, and 97 parts of water, and the rest is the same as Example 1.
[0060] Comparative Example 4
[0061] The difference between this comparative example and Example 1 is that the hydrogel dressing is composed of the following raw materials in parts by weight: 2 parts of hydroxypropyl cellulose, 6 parts of carboxymethyl chitosan, 5 parts of sodium hyaluronate, 0.7 parts of retinol binding protein, 4 parts of modified gluten powder, and 97 parts of water, and the rest is the same as Example 1.
[0062] Comparative Example 5
[0063] The difference between this comparative example and Example 1 is that the hydrogel dressing is composed of the following raw materials in parts by weight: 2 parts of hydroxypropyl cellulose, 6 parts of carboxymethyl chitosan, 5 parts of sodium hyaluronate, 0.3 parts of recombinant human bone morphogenetic protein 4, 0.4 parts of retinol binding protein, 4 parts of gluten, and 97 parts of water, and the rest is the same as Example 1.
[0064] Comparative Example 6
[0065] The difference between this comparative example and Example 1 is that the hydrogel dressing is composed of the following raw materials in parts by weight: 2 parts of hydroxypropyl cellulose, 6 parts of carboxymethyl chitosan, 5 parts of sodium hyaluronate, 0.3 parts of recombinant human bone morphogenetic protein 4, 0.4 parts of retinol binding protein, and 97 parts of water, and the rest is the same as Example 1.
[0066] The performance of the hydrogel dressings of Examples 1-3 and Comparative Examples 1-6 was tested:
[0067] (1) Wound healing properties
[0068] I. A total of 90 SD rats with similar growth status were selected, with a male-female ratio of 1:1, and randomly divided into 9 groups. The hair on the back was removed using a depilatory agent, and the depilatory area was about 16cm 2 After anesthesia, paraffin is dripped onto the hair removal area to form a burn wound;
[0069] II. The hydrogel dressings of Examples 1-3 and Comparative Examples 1-6 were uniformly applied to the wound sites of each group with a coating thickness of 2 mm, and then bandaged with sterile gauze. The hydrogel dressings were changed every 2 days for 12 consecutive days. The scab areas of the wounds on the 6th and 12th days were counted. The results are shown in Table 1.
[0070] Table 1 Wound healing performance results of hydrogel dressings of Examples 1-3 and Comparative Examples 1-6
[0071]
[0072] It can be seen from Table 1 that the hydrogel dressing of the present invention can promote wound healing. The wound healing performance of the hydrogel dressings of Examples 1-3 and Comparative Examples 1-4 is significantly reduced, and the wound healing performance of the hydrogel dressings of Comparative Examples 5-6 is slightly reduced. The above results show that the synergistic effect of retinol binding protein, recombinant human bone morphogenetic protein 4, and modified gluten can promote wound healing.
[0073] (2) Liquid absorption performance
[0074] I. Weigh 0.3 g of the hydrogel dressing of Examples 1-3 and Comparative Examples 1-6, denoted as m0;
[0075] II. Weigh the mass of each set of bags and strings, record it as m1;
[0076] III. Place the above hydrogel dressings in cloth bags, tie the bag mouth with a string, and place the bag in a beaker filled with sufficient water. After the bag swells to saturation, hang the bag for 30 seconds and weigh the mass of each group, recorded as m2. Liquid absorption rate = (m2-m1-m0) / m0×100%, the result is as follows Figure 1 shown.
[0077] Figure 1 The results of the liquid absorption rate of the hydrogel dressings of Examples 1-3 and Comparative Examples 1-6 are shown in FIG. Figure 1 It can be seen that the hydrogel dressing of the present invention has excellent liquid absorption performance. Compared with Examples 1-3, the liquid absorption rate of the hydrogel dressings of Comparative Examples 1-4 is not significantly different, and the liquid absorption rate of the hydrogel dressings of Comparative Examples 5-6 is significantly reduced. The above results show that modified gluten can effectively improve the liquid absorption performance of the hydrogel dressing, thereby reducing the frequency of changing the hydrogel dressing and alleviating the pain of the patient.
[0078] (3) Cytotoxicity
[0079] The cytotoxicity test experiment was carried out on the hydrogel dressings of Examples 1-3 with reference to GB / T 16886.5-2017. The results are shown in Table 2.
[0080] Table 2 Cytotoxicity test results of hydrogel dressings of Examples 1-3
[0081]
[0082] It can be seen from Table 2 that the hydrogel dressing of the present invention has low cytotoxicity.
[0083] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them. The basic principles and main features of the present invention have been described above with specific implementation schemes. On the basis of the present invention, some modifications or replacements may be made thereto, but these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of protection claimed by the present invention.
Claims
1. A hydrogel dressing for promoting wound healing, characterized in that: The invention is composed of the following raw materials in parts by weight: 1-5 parts of hydroxypropyl cellulose, 5-10 parts of carboxymethyl chitosan, 3-8 parts of sodium hyaluronate, 0.1-0.5 parts of recombinant human bone morphogenetic protein 4, 0.1-0.5 parts of retinol binding protein, 3-5 parts of modified gluten powder, and 90-100 parts of water; The preparation steps of the modified gluten are as follows: A: Take gluten powder and add it into water, then add glutamine transaminase for enzymatic hydrolysis; B: performing enzyme inactivation and sterilization treatment on the solution after enzymatic hydrolysis in step A to obtain an enzymatic hydrolyzate; C: adding bacterial agent to the enzymatic hydrolysate of step B for fermentation, collecting the fermentation liquid, filtering it and freeze-drying it to obtain modified gluten powder.
2. A hydrogel dressing for promoting wound healing according to claim 1, characterized in that: The enzymatic hydrolysis conditions in step A are: temperature 50-55° C., pH 5-7, and time 100-120 min.
3. A hydrogel dressing for promoting wound healing according to claim 1, characterized in that: The enzyme inactivation and sterilization process in step B is: enzyme inactivation and sterilization at 85-90° C. for 15-20 minutes.
4. A hydrogel dressing for promoting wound healing according to claim 1, characterized in that: In step A, the mass content of gluten in water is 20-30%, and the mass ratio of gluten to transglutaminase is 1:0.1-0.
3.
5. The hydrogel dressing for promoting wound healing according to claim 1, characterized in that: The bacterial agent in step C is Lactobacillus plantarum, and the inoculation amount is 10 6 -10 7 CFU / g.
6. The hydrogel dressing for promoting wound healing according to claim 1, characterized in that: In step C, the fermentation temperature is 37-39° C. and the fermentation time is 60-70 hours.
7. A method for preparing a hydrogel dressing for promoting wound healing according to any one of claims 1 to 6, characterized in that: The following steps are involved: (1) Weighing raw materials by weight, adding carboxymethyl chitosan, modified gluten powder and hydroxypropyl cellulose into water, stirring and mixing under heat preservation conditions to obtain a mixture; (2) Add sodium hyaluronate, recombinant human bone morphogenetic protein 4, and retinol binding protein to the mixture of step (1), stir and mix under heat preservation conditions, and then place at 4-6°C for 1-2 hours. After sterilization, a hydrogel dressing that promotes wound healing is obtained.
8. The method for preparing a hydrogel dressing for promoting wound healing according to claim 7, characterized in that: The insulation temperature in step (1) is 60-70°C for 3-5 hours, and the insulation temperature in step (2) is 40-50°C for 1-3 hours.