A forging method for TC11 titanium alloy bar

Through multiple modifications of forging and forming forging, combined with the use of different types of anvils, the problems of surface and core unevenness and multiple fire times in the forging of TC11 titanium alloy bars have been solved, and the production efficiency and structural qualification rate have been improved.

CN117960968BActive Publication Date: 2024-10-18TIPRO INT CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202410236839.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-01
Publication Date
2024-10-18
Estimated Expiration
2044-03-01

AI Technical Summary

Technical Problem

The TC11 titanium alloy bar forging method has problems such as uneven final surface and core, high number of reforging production fires, long production cycle, and low energy utilization, resulting in uneven deformation of the forged billet at high temperatures and unqualified structure. .

Method used

The method of multiple modified forging and forming forging is adopted, and the uniformity of the forging billet is gradually improved by setting the heating temperature and holding time. Different types of anvils are used for drawing and upsetting forging, which reduces the number of fires and improves high-temperature residues. Undeformed original grain structure.

Benefits of technology

It effectively solves the problems of uneven deformation and unqualified structure of forging blanks, improves the pass rate of modified forging and internal structure pass rate of forging production, simplifies the forging process, and improves forging efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117960968B_ABST
    Figure CN117960968B_ABST
Patent Text Reader

Abstract

The invention discloses a forging method of a TC11 titanium alloy bar. The forging method comprises: heating a bar raw material to 850°C, and continuously heating it to 1160-1175°C, forging the bar raw material to obtain a first bar blank; heating the first bar blank to 850°C, and continuously heating it to 1075-1085°C, forging the first bar blank to obtain a second bar blank; heating the second bar blank to 850°C, and continuously heating it to 1035-1045°C, forging the second bar blank to obtain to a third bar blank; heating the third bar blank to 850°C, and continuing to heat to 935-945°C, forging the third bar blank to obtain a fourth bar blank; heating the fourth bar blank to 950-955°C, forging the fourth bar blank to obtain a fifth bar blank; heating the fifth bar blank to 945-950°C, forging the fifth bar blank to obtain a sixth bar blank; heating the sixth bar blank to 940-945°C, forging the sixth bar blank to obtain a bar product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of titanium alloy bar forging, and in particular to a forging method of TC11 titanium alloy bar. Background Art

[0002] TC11 titanium alloy is a high-temperature resistant α+β duplex titanium alloy with a high Al equivalent, and its nominal composition is Ti-6.5Al-3.5Mo-1.5r-0.3Si. TC11 titanium alloy can work for a long time at 500℃ and is widely used in the manufacture of large and complex parts such as compressor discs and drum shafts of aircraft engines.

[0003] Usually in marine and atmospheric environments, a stable passivation film can be formed on the surface of titanium alloys, which has good corrosion resistance. However, key titanium alloy parts for aircraft engines are subjected to multiple extreme and harsh conditions such as high temperature, high pressure, high humidity, high salt and high continuous dynamic wear for a long time, and the corrosion resistance of titanium alloys may be greatly reduced due to the harsh corrosive service environment. In addition, the microstructure, chemical element composition, phase morphology and orientation of titanium alloys in different harsh corrosive environments have an important influence on corrosion resistance and corrosion behavior.

[0004] Compared with the transmission forging forming technology, the rod forging manufacturing technology for preparing titanium alloy rods has the characteristics of no need for molds and tooling, short manufacturing cycle, low cost, and high material utilization rate, especially in the optimization of large-size rod forming on 8000T and 4500T large hammer forgings.

[0005] However, the forging method of TC11 titanium alloy bar provided by the related art has the problem of unevenness of the final surface and core of the bar, and has the problems of many reforging production fires, long production cycle and low energy utilization rate. Summary of the invention

[0006] In view of this, an embodiment of the present application provides a forging method for TC11 titanium alloy bars, which can solve the problems of uneven final macrostructure and unqualified flaw detection caused by uneven deformation of the forging blank at high temperature, and improve the qualified rate of forging production and the qualified rate of internal structure.

[0007] The forging method of the TC11 titanium alloy bar provided in the embodiment of the present application includes:

[0008] The first reforging forging: the bar raw material is heated to 850°C and kept warm, and then heated to 1160-1175°C and kept warm, and then the bar raw material is forged to obtain the first bar blank; the second reforging forging: the first bar blank is heated to 850°C and kept warm, and then heated to 1075-1085°C and kept warm, and then the first bar blank is forged to obtain the second bar blank; the third reforging forging: the second bar blank is heated to 850°C and kept warm, and then heated to 1035-1045°C and kept warm, and then the second bar blank is forged to obtain the third bar blank; the fourth reforging forging: the first The three bar blanks are heated to 850°C and kept warm, and then heated to 935-945°C and kept warm, and then the third bar blank is forged to obtain a fourth bar blank; the first forming forging: the fourth bar blank is heated to 950-955°C and kept warm, and then the fourth bar blank is forged to obtain a fifth bar blank; the second forming forging: the fifth bar blank is heated to 945-950°C and kept warm, and then the fifth bar blank is forged to obtain a sixth bar blank; the third forming forging: the sixth bar blank is heated to 940-945°C and kept warm, and then the sixth bar blank is forged to obtain a bar product.

[0009] In a possible implementation of the present application, the holding time in the first forging is: heating the bar raw material to 850° C. and holding it for a first time period t 1 ; Continue heating to 1160-1175℃ and keep warm for the second time period t 2 The holding time of the second forging is: heating the first bar blank to 850°C and holding it for a third time period t 3 ; Continue heating to 1075-1085℃ and keep warm for the fourth time period t 4 The holding time of the third forging is: heating the second bar blank to 850°C and holding it for the fifth time period t 5 ; Continue heating to 1035-1045°C and keep warm for the sixth time period t 6 The holding time of the fourth forging is: heating the third bar blank to 850°C and holding it for the seventh time period t 7 ; Continue heating to 935-945°C and keep warm for the eighth time period t 8 ; where t 1 =0.45min / mm×d 1 , t 2 =0.5min / mm×d 1 , the cross-section shape of the rod raw material is circular, d1 is the diameter of the circular cross-section of the rod raw material; t 3 =0.4min / mm×d 2 , t 4 =0.45min / mm×d2 , the cross-sectional shape of the first bar blank is a square, d 2 is the side length of the square cross section of the first bar blank; t 5 =0.4min / mm×d 3 , t 6 =0.35min / mm×d 3 , the cross-sectional shape of the second bar blank is a square, and d3 is the side length of the square cross-sectional shape of the second bar blank; t 7 =0.35min / mm×d 4 , t 8 =0.25min / mm×d 4 The cross-sectional shape of the third bar blank is a square, and d4 is the side length of the square cross-sectional shape of the third bar blank.

[0010] In a possible implementation of the present application, the holding time of the first forming forging is: heating the fourth bar blank to 950-955° C. and holding it for a ninth time period t 9 The holding time of the second forming forging is: heating the fifth bar blank to 945-950°C and holding it for the tenth time period t 10 The holding time of the third forming forging is: heating the sixth bar blank to 940-945°C and keeping it warm for the eleventh time period t 11 ; where t 9 =(0.45-0.5min / mm)×d 5 , the cross-sectional shape of the fourth bar blank is a square, d 5 is the side length of the square cross section of the fourth bar blank; t 10 =(0.4-0.45min / mm)×d 6 , the cross-sectional shape of the fifth bar blank is circular, d 6 is the diameter of the circular cross section of the fifth bar blank; t 11 =(0.35-0.4min / mm)×d 7 , the cross-sectional shape of the sixth bar blank is circular, d 7 is the diameter of the circular cross section of the sixth bar blank.

[0011] In a possible implementation of the present application, the first reforging, the second reforging, the third reforging and the fourth reforging all include a first upsetting forging, a first stretching forging, a second upsetting forging and a second stretching forging performed sequentially.

[0012] In a possible implementation of the present application, the dimensions of the first stretching forging of the first reforging and each stretching forging of the subsequent reforging are the same; the dimensions of the second upsetting forging of the first reforging and each upsetting forging of the subsequent reforging are the same.

[0013] In a possible implementation of the present application, forging the bar raw material in the first modification forging includes: using a first type anvil to stretch the bar raw material; forging the first bar blank in the second modification forging includes: using a second type anvil to stretch the first bar blank; forging the second bar blank in the third modification forging includes: using a third type anvil to stretch the second bar blank; forging the third bar blank in the fourth modification forging includes: using a fourth type anvil to stretch the third bar blank; wherein the first type anvil, the second type anvil, the third type anvil and the fourth type anvil are all V-shaped anvils.

[0014] In a possible implementation of the present application, the V-shaped anvil includes a first bevel, a second bevel and a first top surface, a V-shaped opening is formed between the first bevel and the second bevel, the first bevel and the second bevel are symmetrically arranged about the center line of the V-shaped opening, a first chamfer is arranged at the position where the first bevel and the second bevel are connected, and a second chamfer is arranged at the position where the first bevel, the second bevel and the first top surface are connected; the angle between the first bevel and the second bevel of the first type anvil, the second type anvil, the third type anvil and the fourth type anvil increases successively; the radius of the first chamfer of the first type anvil, the second type anvil, the third type anvil and the fourth type anvil increases successively; the radius of the second chamfer of the first type anvil, the second type anvil, the third type anvil and the fourth type anvil decreases successively.

[0015] In a possible implementation of the present application, the angles between the first bevel and the second bevel of the first type anvil, the second type anvil, the third type anvil and the fourth type anvil are 60°, 70°, 80° and 90° respectively; the radii of the second rounded corners of the first type anvil, the second type anvil, the third type anvil and the fourth type anvil are d 1 / 4,d 1 / 5,d 1 / 6 and d 1 / 7; the opening heights of the first type anvil, the second type anvil, the third type anvil and the fourth type anvil are d 1 / 2,d 1 / 2.5,d 1 / 3 and d 1 / 4.5; where d 1 is the diameter of the bar raw material.

[0016] In a possible implementation of the present application, forging the fourth bar blank in the first forming forging includes: using a fifth anvil to perform stretch forging on the fourth bar blank; forging the fifth bar blank in the second forming forging includes: using a sixth anvil to perform stretch forging on the fifth bar blank; forging the sixth bar blank in the third forming forging includes: using a seventh anvil to perform stretch forging on the sixth bar blank; wherein the fifth anvil, the sixth anvil and the seventh anvil are all arc-shaped anvils, and the arc-shaped anvil includes an arc surface and a second top surface, a third chamfer is arranged between the arc surface and the second top surface, and the radius of the third chamfer of the fifth anvil, the sixth anvil and the seventh anvil decreases successively.

[0017] In a possible implementation of the present application, the radii of the third rounded corners of the fifth type anvil, the sixth type anvil and the seventh type anvil are d 1 / 5,d 1 / 6 and d 1 / 7; the radii corresponding to the arcuate surfaces of the fifth type anvil, the sixth type anvil and the seventh type anvil are d 1 / 3,d 1 / 4 and d 1 / 5; where d 1 is the diameter of the bar raw material.

[0018] In the forging method of TC11 titanium alloy bar provided in the embodiment of the present application, by setting the heating temperature, the first reforging to the fourth reforging are completed by four fires, and the first forming forging to the third forming forging are completed by three fires. Therefore, in the embodiment of the present application, the forging of TC11 titanium alloy can be completed with fewer fires, and the problems of uneven final low-magnification structure and unqualified flaw detection caused by uneven deformation of the forging blank at high temperature can be solved, and the qualified rate of reforging and the qualified rate of internal structure of forging production can be improved. In addition, in the forging method provided in the embodiment of the present application, the method of reforging and forming forging can effectively improve the original grain structure that remains undeformed at the high temperature of the blank, and can further improve the qualified rate of reforging and the qualified rate of internal structure of forging production. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the technical solution of the present application, the drawings required for use in the embodiments are briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.

[0020] Figure 1 A flow chart of a forging method of a TC11 titanium alloy bar provided in an embodiment of the present application;

[0021] Figure 2 A schematic diagram of the structure of a first type anvil, a second type anvil, a third type anvil or a fourth type anvil in the forging method of a TC11 titanium alloy bar provided in an embodiment of the present application;

[0022] Figure 3 A schematic cross-sectional view of a first type anvil, a second type anvil, a third type anvil or a fourth type anvil in the forging method of a TC11 titanium alloy bar provided in an embodiment of the present application;

[0023] Figure 4 A schematic diagram of the structure of a fifth type anvil, a sixth type anvil or a seventh type anvil in the forging method of a TC11 titanium alloy bar provided in an embodiment of the present application;

[0024] Figure 5 A schematic cross-sectional view of a fifth type anvil, a sixth type anvil or a seventh type anvil in the forging method of a TC11 titanium alloy bar provided in an embodiment of the present application.

[0025] Reference numerals:

[0026] 1. V-shaped anvil; 11. first inclined surface; 12. second inclined surface; 13. first top surface; 2. arc-shaped anvil; 21 arc-shaped surface; 22 second top surface. DETAILED DESCRIPTION

[0027] In order to enable those skilled in the art to better understand the technical solutions in this application, the technical solutions in the application embodiments will be clearly and completely described below in conjunction with the drawings in the embodiments of this application; it is obvious that the described embodiments are only part of the embodiments of this application, not all of them. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of this application.

[0028] TC11 titanium alloy is an α+β type heat-resistant titanium alloy with good comprehensive performance, which is widely used in the manufacture of large and complex parts such as compressor discs and drum shafts of aircraft engines. However, the TC11 titanium alloy forging method provided by the relevant technology has the problem of unevenness of the final surface and core of the bar, and there are problems such as more reforging production fires, long production cycle and low energy utilization.

[0029] In view of this, an embodiment of the present application provides a forging method for TC11 titanium alloy bars, which can solve the problems of uneven final macrostructure and unqualified flaw detection caused by uneven deformation of the forging blank at high temperature, and improve the qualified rate of forging production and the qualified rate of internal structure.

[0030] Specifically, refer to Figure 1The forging method of the TC11 titanium alloy bar provided in the embodiment of the present application includes steps S11 to S17, wherein:

[0031] Step S11, first reforging: heating the bar material to 850°C and keeping the temperature, further heating to 1160-1175°C and keeping the temperature, forging the bar material to obtain a first bar blank.

[0032] Step S12, second reforging: heating the first bar blank to 850° C. and keeping the temperature, further heating to 1075-1085° C. and keeping the temperature, forging the first bar blank to obtain a second bar blank.

[0033] Step S13, third reforging: heating the second bar blank to 850° C. and keeping the temperature, further heating to 1035-1045° C. and keeping the temperature, forging the second bar blank to obtain a third bar blank.

[0034] Step S14, fourth reforging: heating the third bar blank to 850° C. and keeping the temperature, further heating to 935-945° C. and keeping the temperature, forging the third bar blank to obtain a fourth bar blank.

[0035] Step S15, first forming forging: after heating the fourth bar blank to 950-955° C. and keeping the temperature, forging the fourth bar blank to obtain a fifth bar blank.

[0036] Step S16, second forming forging: after heating the fifth bar blank to 945-950° C. and keeping the temperature, forging the fifth bar blank to obtain a sixth bar blank.

[0037] Step S17, third forming forging: after heating the sixth bar blank to 940-945° C. and keeping the temperature, forging the sixth bar blank to obtain a bar product.

[0038] It can be understood that in the embodiment of the present application, a 4500T press can be used to forge the TC11 titanium alloy bar.

[0039] It should be noted that in the forging method provided in the embodiment of the present application, the temperature of the rod raw material can be first set to less than or equal to 800°C, and then the rod raw material can be sent into a heating furnace, and the rod raw material can be heated to 850°C and kept warm for a period of time, and then the rod raw material can be further heated to 1160-1175°C and kept warm for a period of time, and then the rod raw material can be forged to obtain a first rod blank.

[0040] In the embodiment of the present application, the holding time after the bar raw material is heated to 850°C and the holding time after the bar raw material is heated to 1160-1175°C are not limited, and the holding time can be determined according to the diameter of the bar raw material. It can be understood that when the diameter of the bar raw material is large, the holding time can be set longer; when the diameter of the bar raw material is small, the holding time can be set shorter. After that, the bar raw material can be forged. For the convenience of description, the product obtained after forging the bar raw material can be referred to as the first bar blank.

[0041] It should be noted that, in the first forging process, the forging form of the bar raw material is not limited. For example, a special anvil can be used to stretch the bar raw material and a universal anvil can be used to upset the bar raw material.

[0042] In addition, in the embodiment of the present application, the terminal temperature after the first reforging can be set to be greater than or equal to 850° C., and the cooling method after the first reforging is set to post-forging air cooling.

[0043] After the first modification forging, the second modification forging can be performed. Specifically, the first bar blank can be sent into a heating furnace, the first bar blank can be heated to 850°C and kept warm for a period of time, and then the first bar blank can be further heated to 1075-1085°C and kept warm for a period of time, and then the first bar blank can be forged to obtain the second bar blank.

[0044] In the embodiment of the present application, the holding time after the first bar blank is heated to 850°C and the holding time after the first bar blank is heated to 1075-1085°C are not limited, and the holding time can be determined according to the diameter of the first bar blank. It can be understood that when the diameter of the first bar blank is large, the holding time can be set longer; when the diameter of the bar raw material is small, the holding time can be set shorter. After that, the first bar blank can be forged. For the convenience of description, the product obtained after forging the first bar blank can be referred to as the second bar blank.

[0045] It should be noted that in the second reforging, the forging form of the first bar blank is not limited. For example, a special anvil can be used to stretch the first bar blank and a universal anvil can be used to upset the first bar blank.

[0046] In addition, in the embodiment of the present application, the terminal temperature after the second reforging can be set to be greater than or equal to 850° C., and the cooling method after the second reforging is set to post-forging air cooling.

[0047] After the second modification forging, the third modification forging can be performed. Specifically, the second bar blank can be sent into a heating furnace, the second bar blank can be heated to 850°C and kept warm for a period of time, and then the second bar blank can be further heated to 1035-1045°C and kept warm for a period of time, and then the second bar blank can be forged to obtain the third bar blank.

[0048] In the embodiment of the present application, the holding time after the second bar blank is heated to 850°C and the holding time after the second bar blank is heated to 1035-1045°C are not limited, and the holding time can be determined according to the diameter of the second bar blank. It can be understood that when the diameter of the second bar blank is large, the holding time can be set longer; when the diameter of the bar raw material is small, the holding time can be set shorter. After that, the second bar blank can be forged. For the convenience of description, the product obtained after forging the second bar blank can be referred to as the third bar blank.

[0049] It should be noted that in the third forging, the forging form of the second bar blank is not limited. For example, the second bar blank can be stretched using a special anvil and the second bar blank can be upset using a universal anvil.

[0050] In addition, in the embodiment of the present application, the terminal temperature after the third forging can be set to be greater than or equal to 850° C., and the cooling method after the third forging is set to air cooling after forging.

[0051] After the third modification forging, the fourth modification forging can be carried out. Specifically, the third bar blank can be sent into a heating furnace, the third bar blank can be heated to 850°C and kept warm for a period of time, and then the third bar blank can be further heated to 935-945°C and kept warm for a period of time, and then the third bar blank can be forged to obtain a fourth bar blank.

[0052] In the embodiment of the present application, the holding time after the third bar blank is heated to 850°C and the holding time after the third bar blank is heated to 935-945°C are not limited, and the holding time can be determined according to the diameter of the third bar blank. It can be understood that when the diameter of the third bar blank is large, the holding time can be set longer; when the diameter of the third bar blank is small, the holding time can be set shorter. After that, the third bar blank can be forged. For the convenience of description, the product obtained after forging the third bar blank can be referred to as the fourth bar blank.

[0053] It should be noted that in the fourth modification forging, the forging form of the third bar blank is not limited. For example, the third bar blank can be stretched using a special anvil and the third bar blank can be upset using a universal anvil.

[0054] In addition, in the embodiment of the present application, the terminal temperature after the fourth reforging can be set to be greater than or equal to 850° C., and the cooling method after the fourth reforging is set to post-forging air cooling.

[0055] After the fourth modification forging, the first forming forging can be carried out. Specifically, the fourth bar blank can be sent into a heating furnace, the fourth bar blank is heated to 950-955° C. and kept warm for a period of time, and then the fourth bar blank is forged to obtain the fifth bar blank.

[0056] In the embodiment of the present application, the holding time after the fourth bar blank is heated to 950-955°C is not limited, and the holding time can be determined according to the diameter of the fourth bar blank. It can be understood that when the diameter of the fourth bar blank is large, the holding time can be set longer; when the diameter of the fourth bar blank is small, the holding time can be set shorter. After that, the fourth bar blank can be forged. For the convenience of description, the product obtained after forging the fourth bar blank can be referred to as the fifth bar blank.

[0057] It should be noted that, in the first forming forging, the forging form of the fourth bar blank is not limited. For example, the fourth bar blank can be stretched using a special anvil.

[0058] In addition, in the embodiment of the present application, the terminal temperature after the first forming forging can be set to be greater than or equal to 850° C., and the cooling method after the first forming forging is set to post-forging air cooling.

[0059] After the first forming forging, the second forming forging can be performed. Specifically, the fifth bar blank can be sent into a heating furnace, the fifth bar blank is heated to 945-950° C. and kept warm for a period of time, and then the fifth bar blank is forged to obtain a sixth bar blank.

[0060] In the embodiment of the present application, the holding time after the fifth bar blank is heated to 945-950°C is not limited, and the holding time can be determined according to the diameter of the fifth bar blank. It can be understood that when the diameter of the fifth bar blank is large, the holding time can be set longer; when the diameter of the fifth bar blank is small, the holding time can be set shorter. After that, the fifth bar blank can be forged. For the convenience of description, the product obtained after forging the fifth bar blank can be called the sixth bar blank.

[0061] It should be noted that, in the second forming forging, the forging form of the fifth bar blank is not limited. For example, the fifth bar blank can be stretched using a special anvil.

[0062] In addition, in the embodiment of the present application, the terminal temperature after the second forming forging can be set to be greater than or equal to 850° C., and the cooling method after the second forming forging is set to post-forging air cooling.

[0063] After the second forming forging, the third forming forging can be performed. Specifically, the sixth bar blank can be sent into a heating furnace, the sixth bar blank is heated to 940-945°C and kept warm for a period of time, and then the sixth bar blank is forged to obtain a bar product.

[0064] In the embodiment of the present application, the holding time after the sixth bar blank is heated to 940-945°C is not limited, and the holding time can be determined according to the diameter of the sixth bar blank. It can be understood that when the diameter of the sixth bar blank is large, the holding time can be set longer; when the diameter of the sixth bar blank is small, the holding time can be set shorter. After that, the sixth bar blank can be forged. For the convenience of description, the product obtained after forging the sixth bar blank can be referred to as a bar product. It can be understood that the bar product is the final required TC11 titanium alloy bar.

[0065] It should be noted that, in the third forming forging, the forging form of the sixth bar blank is not limited. For example, the sixth bar blank can be stretched using a special anvil.

[0066] In addition, in the embodiment of the present application, the terminal temperature after the third forming forging can be set to be greater than or equal to 850° C., and the cooling method after the third forming forging is set to post-forging air cooling.

[0067] In the forging method of TC11 titanium alloy bar provided in the embodiment of the present application, by setting the heating temperature, the first reforging to the fourth reforging are completed by four fires, and the first forming forging to the third forming forging are completed by three fires. Therefore, in the embodiment of the present application, the forging of TC11 titanium alloy can be completed with fewer fires, and the problems of uneven final low-magnification structure and unqualified flaw detection caused by uneven deformation of the forging blank at high temperature can be solved, and the qualified rate of reforging and the qualified rate of internal structure of forging production can be improved. In addition, in the forging method provided in the embodiment of the present application, the method of reforging and forming forging can effectively improve the original grain structure that remains undeformed at the high temperature of the blank, and can further improve the qualified rate of reforging and the qualified rate of internal structure of forging production.

[0068] It should be noted that in the forging method of TC11 titanium alloy bar provided in the embodiment of the present application, the cross-sectional shape of the bar raw material is circular; the cross-sectional shape of the first bar blank obtained after the first modification forging of the bar raw material is square; the cross-sectional shape of the second bar blank obtained after the second modification forging of the first bar blank is square; the cross-sectional shape of the third bar blank obtained after the third modification forging of the second bar blank is square; the cross-sectional shape of the fourth bar blank obtained after the fourth modification forging of the third bar blank is square; the cross-sectional shape of the fifth bar blank obtained after the first forming forging of the fourth bar blank is circular; the cross-sectional shape of the sixth bar blank obtained after the second forming forging of the fifth bar blank is circular; the cross-sectional shape of the bar product obtained after the third forming forging of the sixth bar blank is circular. For the convenience of description, "φ" is used to represent the diameter of the circular cross-section, and "□" is used to represent the side length of the square cross-section.

[0069] On this basis, in the forging method of TC11 titanium alloy bar provided in the application embodiment, the holding time in the first forging modification is: heating the bar raw material to 850°C and keeping it warm for the first time period; continuing to heat the bar raw material to 1160-1175°C and keeping it warm for the second time period t2. The holding time for the second forging modification is: heating the first bar blank to 850°C and keeping it warm for the third time period t3; continuing to heat the first bar blank to 1075-1085°C and keeping it warm for the fourth time period t4. The holding time for the third forging modification is: heating the second bar blank to 850°C and keeping it warm for the fifth time period t5; continuing to heat to 1035-1045°C and keeping it warm for the sixth time period t6. The holding time for the fourth forging modification is: heating the third bar to 850°C and keeping it warm for the seventh time period t7; continuing to heat the third bar blank to 935-945°C and keeping it warm for the eighth time period t8. Among them, t 1 =0.45min / mm×d 1 , t2 =0.5min / mm×d 1 , the cross-section shape of the rod raw material is circular, d1 is the diameter of the circular cross-section of the rod raw material; t 3 =0.4min / mm×d 2 , t 4 =0.45min / mm×d 2 , the cross-sectional shape of the first bar blank is a square, d 2 is the side length of the square cross section of the first bar blank; t 5 =0.4min / mm×d 3 , t 6 =0.35min / mm×d 3 , the cross-sectional shape of the second bar blank is a square, and d3 is the side length of the square cross-sectional shape of the second bar blank; t 7 =0.35min / mm×d 4 , t 8 =0.25min / mm×d 4 The cross-sectional shape of the third bar blank is a square, and d4 is the side length of the square cross-sectional shape of the third bar blank.

[0070] It can be understood that the above formula can be used to calculate the holding time. For example, for a rod raw material with a diameter of φ690 mm, t 1 =690×0.45=310.5min,t 2 =690×0.5=345min.

[0071] Similarly, referring to the above description, t 3 and t 4 , calculate t based on the diameter of the second bar blank 5 and t 6 , calculate t based on the diameter of the third bar blank 7 and t 8 .

[0072] For example, in some embodiments of the present application, the specification of the bar raw material is φ690×900mm, the specification of the first bar blank is □570×1035±15mm, the specification of the second bar blank is □570×1035±15mm, the specification of the third bar blank is □570×1035±15mm, the specification of the fourth bar blank is □570×1035±15mm, the specification of the fifth bar blank is φ450×2100±15mm, the specification of the sixth bar blank is φ355×3300±15mm (which can be evenly divided into 3 pieces, each with a specification of φ355×1100±5mm), and the specification of the bar product is φ240×2400±15mm. Then the above t 3 =228min,t 4 =256.5min,t 5 =228min,t 6 =199.5min,t 7 =199.5min,t 8 =142.5min.

[0073] It should be noted that, in some embodiments of the present application, for the convenience of setting, the above t 1 to 8 For example, in some embodiments of the present application, t 1 Set to 310min, and set t 2 Set to 345min, and set t 3 Set to 230min, and set t 4 Set to 255min, and set t 5 Set to 230min, and set t 6 Set to 200min, and set t 7 Set to 200min, and set t 8 Set to 145min.

[0074] Through the above settings, in the forging method of TC11 titanium alloy bar provided in the embodiment of the present application, the holding time is set according to the diameter of the bar raw material, the diameter of the first bar blank, the diameter of the second bar blank and the diameter of the third bar blank, so that the material can gradually reach a uniform temperature and the grains can grow uniformly, thereby changing the structure, performance and shape of the material. In addition, through the above settings, the holding time is not wasted, and the forging efficiency of the TC11 titanium alloy bar can be further improved.

[0075] On this basis, in some embodiments of the present application, the holding time of the first forming forging is: heating the fourth bar blank to 950-955° C. and holding it for a ninth time period t9 The holding time of the second forming forging is to heat the fifth bar blank to 945-950°C and keep it for the tenth time period t10. The holding time of the third forming forging is to heat the sixth bar blank to 940-945°C and keep it for the eleventh time period t11. 9 =(0.45-0.5min / mm)×d 5 , the cross-sectional shape of the fourth bar blank is a square, d 5 is the side length of the square section of the fourth bar blank; t 10 =(0.4-0.45min / mm)×d 6 , the cross-sectional shape of the fifth bar blank is circular, d 6 is the diameter of the circular cross section of the fifth bar blank; t 11 =(0.35-0.4min / mm)×d 7 , the cross-sectional shape of the sixth bar blank is circular, d 7 is the diameter of the circular cross section of the sixth bar blank.

[0076] It can be understood that the above formula can be used to calculate the holding time. For example, for the fourth bar blank having a square cross-section with a side length of 570 mm, t 9 = 256.5-285min; For the fifth bar blank having a circular cross-section diameter of 450mm, t 10 = 180-202.5min; For the sixth bar blank having a circular cross-section diameter of 355mm, t 11 =124.5-142min.

[0077] It should be noted that, in some embodiments of the present application, for the convenience of setting, the above t 9 to 11 For example, in some embodiments of the present application, t 9 Set to 285min, and set t 10 Set to 205min, and set t 11 Set to 145min.

[0078] Through the above arrangement, in the forging method of the TC11 titanium alloy bar provided in the embodiment of the present application, the above formula is used to determine the holding time during the forming forging stage, which can further make the material gradually reach a uniform temperature, so that the grains grow uniformly, thereby changing the structure, performance and shape of the material. In addition, through the above arrangement, the holding time is not wasted, and the forging efficiency of the TC11 titanium alloy bar can be further improved.

[0079] In addition, in some embodiments of the present application, the first modification forging, the second modification forging, the third modification forging and the fourth modification forging all include a first drawing forging, a first upsetting forging, a second drawing forging and a second upsetting forging performed sequentially.

[0080] It can be understood that in the embodiment of the present application, a special anvil can be used to lengthen the bar raw material, and a universal anvil can be used to upset the bar raw material.

[0081] Thus, the first forging modification includes two stretching forgings and two upsetting forgings, the second forging modification includes two stretching forgings and two upsetting forgings, the third forging modification includes two stretching forgings and two upsetting forgings, and the fourth forging modification includes two stretching forgings and two upsetting forgings.

[0082] Through the above-mentioned arrangement, in the forging method of TC11 titanium alloy bar provided in the embodiment of the present application, two upsetting forgings and stretching forgings are arranged in the first modification forging, the second modification forging, the third modification forging and the fourth modification forging, which can further make the internal structure of the TC11 bar more uniform and further improve the forging efficiency of the TC11 titanium alloy bar.

[0083] On this basis, in some embodiments of the present application, the first stretching forging of the first reforging and the size of each stretching forging of the subsequent reforging are the same. The second upsetting forging of the first reforging and the size of each upsetting forging of the subsequent reforging are the same.

[0084] It can be understood that the first drawing forging of the first modification forging and each drawing forging of the subsequent modification forging refer to the first drawing forging and the second drawing forging of the first modification forging, the first drawing forging and the second drawing forging of the second modification forging, the first drawing forging and the second drawing forging of the third modification forging, the first drawing forging and the second drawing forging of the fourth modification forging. The second upsetting forging of the first modification forging and each upsetting forging of the subsequent modification forging refer to the second upsetting forging of the first modification forging, the first upsetting forging and the second upsetting forging of the second modification forging, the first upsetting forging and the second upsetting forging of the third modification forging, and the first upsetting forging and the second upsetting forging of the fourth modification forging.

[0085] For example, in some embodiments of the present application, the specification of the bar raw material is φ690×900mm, the specification after the first rough forging of the first reforming forging is φ730×800mm, the specification after the first drawing forging of the first reforming forging is □570×1035mm, the specification after the second rough forging after the first reforming forging is φ690×705mm, and the specification after the second drawing forging after the first reforming forging is □570×1035. In the second reforming forging, the third reforming forging and the fourth reforming forging, the specification of the bar is cycled between □570×1035mm and □690×705mm.

[0086] Through the above arrangement, in the forging method of the TC11 titanium alloy bar provided in the embodiment of the present application, the forging process of the TC11 titanium alloy bar can be simplified, and the forging efficiency of the TC11 titanium alloy bar can be further improved.

[0087] In addition, in some embodiments of the application, forging the bar raw material in the first forging modification includes: using a first type anvil to stretch the bar raw material; forging the first bar blank in the second forging modification includes: using a second type anvil to stretch the first bar blank; forging the second bar blank in the third forging modification includes: using a third type anvil to stretch the second bar blank; forging the third bar blank in the fourth forging modification includes: using a fourth type anvil to stretch the third bar blank; wherein the first type anvil, the second type anvil, the third type anvil and the fourth type anvil are all V-shaped anvils.

[0088] It can be understood that the V-shaped anvil is a vertically symmetrical structure, and the upper and lower V-shaped anvils are provided with symmetrical V-shaped openings, and the TC11 titanium alloy rod can be forged between the V-shaped openings.

[0089] It should be noted that in the embodiment of the present application, the sizes of the V-shaped openings of the first anvil, the second anvil, the third anvil and the fourth anvil can be set differently to adapt to the first forging modification, the second forging modification, the third forging modification and the fourth forging modification respectively.

[0090] On this basis, refer to Figure 2 and Figure 3The V-shaped anvil 1 includes a first bevel 11, a second bevel 12 and a first top surface 13, a V-shaped opening is formed between the first bevel 11 and the second bevel 12, the first bevel 11 and the second bevel 12 are symmetrically arranged about the center line of the V-shaped opening, a first rounded corner is arranged at the position where the first bevel 11 and the second bevel 12 are connected, and a second rounded corner is arranged at the position where the first bevel 11 and the first top surface 13 are connected and at the position where the second bevel 12 and the first top surface 13 are connected. The angle α between the first bevel and the second bevel of the first type anvil, the second type anvil, the third type anvil and the fourth type anvil increases successively. The first rounded corners R of the first type anvil, the second type anvil, the third type anvil and the fourth type anvil 1 The radius of the first type anvil, the second type anvil, the third type anvil and the fourth type anvil increases successively. 2 The radius decreases successively.

[0091] It should be noted that in some embodiments of the present application, the size of the angle between the first bevel and the second bevel of the first anvil, the second anvil, the third anvil and the fourth anvil can be set according to the target specifications of the first bar blank, the second bar blank, the third bar blank and the fourth bar blank.

[0092] On this basis, in some embodiments of the present application, the angle between the first bevel and the second bevel of the first type anvil, the angle between the first bevel and the second bevel of the second type anvil, the angle between the first bevel and the second bevel of the third type anvil, and the angle between the first bevel and the second bevel of the fourth type anvil can be set to 60°, 70°, 80°, and 90°, respectively. Further, the radius of the second rounded corners of the first type anvil, the second type anvil, the third type anvil, and the fourth type anvil can be set to d 1 / 4,d 1 / 5,d 1 / 6 and d 1 / 7. Further, the opening heights H of the first type anvil, the second type anvil, the third type anvil and the fourth type anvil can be set to d 1 / 2,d 1 / 2.5,d 1 / 3 and d 1 / 4.5; wherein d1 is the diameter of the rod raw material.

[0093] In addition, in some embodiments of the present application, the radius of the first rounded corner of the first type anvil, the second type anvil, the third type anvil, and the fourth type anvil can be set to increase with the increase of the diameter of the rod material. For example, in some embodiments of the present application, for a rod material with a diameter of 690 mm, the radius of the first rounded corner of the first type anvil can be set to 15 mm, the radius of the first rounded corner of the second type anvil can be set to 20 mm, the radius of the first rounded corner of the third type anvil can be set to 25 mm, and the radius of the first rounded corner of the fourth type anvil can be set to 30 mm. For other values ​​of the diameter of the rod material, the radius of the first rounded corner of the first type anvil, the radius of the first rounded corner of the second type anvil, the radius of the first rounded corner of the third type anvil, and the radius of the first rounded corner of the fourth type anvil can be enlarged or reduced in proportion to the above dimensions.

[0094] In general, the size parameters of the first type anvil, the second type anvil, the third type anvil and the fourth type anvil can be set by referring to the table below.

[0095]

[0096]

[0097] It should be noted that, refer to Figure 3 , half the width B of the V-shaped opening refers to the distance between the center line of the V-shaped opening and the intersection of the first inclined surface or the extension line of the second inclined surface and the extension line of the first top surface.

[0098] In addition, in some embodiments of the application, forging the fourth bar stock in the first forming forging includes: using the fifth type anvil to stretch the fourth bar stock; forging the fifth bar stock in the second forming forging includes: using the sixth type anvil to stretch the fifth bar stock; forging the sixth bar stock in the third forming forging includes: using the seventh type anvil to stretch the sixth bar stock; wherein the fifth type anvil, the sixth type anvil and the seventh type anvil are all arc-shaped anvils. Figure 4 and Figure 5 The arc-shaped anvil 2 includes an arc surface 21 and a second top surface 22, a third rounded corner is provided between the arc surface 21 and the second top surface 22, and the radius R of the third rounded corner of the fifth type anvil, the sixth type anvil and the seventh type anvil is 3 Decrease in sequence.

[0099] It can be understood that, since the product obtained after the third forming and forging is a bar product, the third forming and forging process is a process of chamfering and rounding.

[0100] On this basis, in some embodiments of the present application, the radii of the third rounded corners of the fifth type anvil, the sixth type anvil and the seventh type anvil may be set to d 1 / 5,d1 / 6 and d 1 / 7. Further, the radius R corresponding to the arc surface of the fifth type anvil, the sixth type anvil and the seventh type anvil can be 4 Set to d 1 / 3,d 1 / 4 and d 1 / 5. Among them, d 1 is the diameter of the bar raw material.

[0101] In addition, in some embodiments of the present application, the half width b of the arc surface of the fifth type anvil, the sixth type anvil and the seventh type anvil can be set to 3d in sequence. 1 / 10,3d 1 / 11 and 3d 1 / 12. In addition, the opening heights h of the fifth, sixth and seventh anvils can be set to 3d 1 / 10+50mm、3d 1 / 11+45mm、3d 1 / 12+40mm.

[0102] In general, the size parameters of the fifth, sixth and seventh anvils can be set by referring to the following table.

[0103]

[0104] It should be noted that, refer to Figure 5 , half of the width of the arcuate surface b refers to the distance between the center line of the arcuate surface and the intersection of the extension line of the arcuate surface and the extension line of the second top surface.

[0105] It can be understood that after forging the bar raw materials using the TC11 titanium alloy bar forging method provided in the embodiment of the present application to obtain bar products, physical and chemical inspections can be carried out on samples of approximately φ230×200 mm at the end of each batch of bar products, and the inspections can be carried out in accordance with the forging bar execution standards. For example, chemical composition, mechanical properties, macrostructure, macrostructure, etc. can be inspected.

[0106] Afterwards, the bar product can be machined to process the outer circle and both end faces of the bar product. For example, the surface roughness of the bar product can be machined to Ra3.2.

[0107] In the embodiments of the present application, the terms "first" and "second" are used for descriptive purposes only and are not to be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of the embodiments of the present application, unless otherwise specified, "multiple" means two or more.

[0108] In addition, in the embodiments of the present application, directional terms such as "up", "down", "left" and "right" are defined relative to the orientation of the components in the drawings. It should be understood that these directional terms are relative concepts. They are used for relative description and clarification, and they may change accordingly according to the changes in the orientation of the components in the drawings.

[0109] In the embodiments of the present application, unless otherwise clearly specified and limited, the term "connection" should be understood in a broad sense. For example, "connection" can be a fixed connection, a detachable connection, or an integral connection; it can be a direct connection or an indirect connection through an intermediate medium.

[0110] In the embodiments of the present application, the terms "include", "comprises" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the sentence "comprises a ..." does not exclude the presence of other identical elements in the process, method, article or device including the element.

[0111] In the embodiments of the present application, words such as "exemplary" or "for example" are used to indicate examples, illustrations or descriptions. Any embodiment or design described as "exemplary" or "for example" in the embodiments of the present application should not be interpreted as being more preferred or more advantageous than other embodiments or designs. Specifically, the use of words such as "exemplary" or "for example" is intended to present related concepts in a specific way.

[0112] The serial numbers of the embodiments of the present application are only for description and do not represent the advantages and disadvantages of the embodiments. The above are only preferred embodiments of the present application, and do not limit the patent scope of the present application. Any equivalent structure or equivalent process transformation made by using the contents of the present application specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present application.

Claims

1. A forging method for TC11 titanium alloy bars, characterized in that: The forging method comprises: The first forging process: heating the bar material to 850°C and keeping the temperature, and then heating the bar material to 1160-1175°C and keeping the temperature, and then forging the bar material to obtain a first bar blank; wherein forging the bar material includes: using a first anvil to perform elongation forging on the bar material; Second reforging: heating the first bar blank to 850° C. and keeping the temperature, and then heating to 1075-1085° C. and keeping the temperature, forging the first bar blank to obtain a second bar blank; wherein forging the first bar blank includes: performing elongation forging on the first bar blank using a second anvil; The third reforging forging: heating the second bar blank to 850° C. and keeping the temperature, and then heating the second bar blank to 1035-1045° C. and keeping the temperature, and then forging the second bar blank to obtain a third bar blank; wherein the forging of the second bar blank includes: using a third anvil to perform elongation forging on the second bar blank; Fourth reforging: heating the third bar blank to 850° C. and keeping the temperature, and then heating to 935-945° C. and keeping the temperature, and then forging the third bar blank to obtain a fourth bar blank; wherein forging the third bar blank includes: performing elongation forging on the third bar blank using a fourth anvil; Wherein, the first type anvil, the second type anvil, the third type anvil and the fourth type anvil are all V-shaped anvils; the V-shaped anvil comprises a first inclined surface, a second inclined surface and a first top surface, a V-shaped opening is formed between the first inclined surface and the second inclined surface, the first inclined surface and the second inclined surface are symmetrically arranged about the center line of the V-shaped opening, a first chamfer is arranged at a position where the first inclined surface and the second inclined surface are connected, and a second chamfer is arranged at a position where the first inclined surface, the second inclined surface and the first top surface are connected; The included angles between the first inclined surface and the second inclined surface of the first type anvil, the second type anvil, the third type anvil and the fourth type anvil increase in sequence; The radii of the first rounded corners of the first type anvil, the second type anvil, the third type anvil and the fourth type anvil increase in sequence; The radius of the second rounded corners of the first type anvil, the second type anvil, the third type anvil and the fourth type anvil decreases successively; the angles between the first inclined surface and the second inclined surface of the first type anvil, the second type anvil, the third type anvil and the fourth type anvil are 60°, 70°, 80° and 90° respectively; The radii of the second chamfered corners of the first type anvil, the second type anvil, the third type anvil and the fourth type anvil are d1 / 4, d1 / 5, d1 / 6 and d1 / 7 respectively; The opening heights of the first type anvil, the second type anvil, the third type anvil and the fourth type anvil are d1 / 2, d1 / 2.5, d1 / 3 and d1 / 4.5 respectively; wherein d1 is the diameter of the bar raw material; First forming forging: heating the fourth bar blank to 950-955° C. and keeping the temperature, and then forging the fourth bar blank to obtain a fifth bar blank; Second forming forging: heating the fifth bar blank to 945-950° C. and keeping the temperature, and then forging the fifth bar blank to obtain a sixth bar blank; The third forming forging: after heating the sixth bar blank to 940-945° C. and keeping the temperature, forging the sixth bar blank to obtain a bar product.

2. The forging method of TC11 titanium alloy bar according to claim 1, characterized in that: The holding time in the first forging is: heating the bar material to 850°C and keeping it warm for a first time period t1; continuing to heat it to 1160-1175°C and keeping it warm for a second time period t2; The holding time of the second forging is: heating the first bar blank to 850° C. and keeping it for a third time period t3; continuing to heat it to 1075-1085° C. and keeping it for a fourth time period t4; The holding time of the third forging is: heating the second bar blank to 850° C. and keeping it for a fifth time period t5; continuing to heat it to 1035-1045° C. and keeping it for a sixth time period t6; The holding time of the fourth forging is: heating the third bar blank to 850° C. and keeping it for a seventh time period t7; continuing to heat it to 935-945° C. and keeping it for an eighth time period t8; Wherein, t1=0.45min / mm×d1, t2=0.5min / mm×d1, the cross-sectional shape of the rod raw material is circular, and d1 is the diameter of the circular cross-sectional shape of the rod raw material; t3=0.4min / mm×d2, t4=0.45min / mm×d2, the cross-sectional shape of the first bar blank is a square, and d2 is the side length of the square cross-sectional shape of the first bar blank; t5=0.4min / mm×d3, t6=0.35min / mm×d3, the cross-sectional shape of the second bar blank is a square, and d3 is the side length of the square cross-sectional shape of the second bar blank; t7=0.35min / mm×d4, t8=0.25min / mm×d4, the cross-sectional shape of the third bar blank is a square, and d4 is the side length of the square cross-sectional shape of the third bar blank.

3. The forging method of TC11 titanium alloy bar according to claim 2, characterized in that: The holding time of the first forming forging is: heating the fourth bar blank to 950-955° C. and holding the temperature for a ninth time period t9; The holding time of the second forming forging is: heating the fifth bar blank to 945-950°C and holding it for a tenth time period t 10 ; The holding time of the third forming forging is: heating the sixth bar blank to 940-945°C and keeping it warm for an eleventh time period t 11 ; Wherein, t9=(0.45-0.5min / mm)×d5, the cross-sectional shape of the fourth bar blank is a square, and d5 is the side length of the square cross-sectional shape of the fourth bar blank; t 10 =(0.4-0.45min / mm)×d6, the cross-sectional shape of the fifth bar blank is circular, and d6 is the diameter of the circular cross-sectional shape of the fifth bar blank; t 11 =(0.35-0.4min / mm)×d7, the cross-sectional shape of the sixth bar blank is circular, and d7 is the diameter of the circular cross-sectional shape of the sixth bar blank.

4. The forging method of TC11 titanium alloy bar according to claim 1, characterized in that: The first modification forging, the second modification forging, the third modification forging and the fourth modification forging all include a first upsetting forging, a first stretching forging, a second upsetting forging and a second stretching forging performed in sequence.

5. The forging method of TC11 titanium alloy bar according to claim 4, characterized in that: The dimensions of the first stretching forging of the first reforming forging and each stretching forging of the subsequent reforming forging are the same; The second upsetting forging of the first reforming forging and each upsetting forging of the subsequent reforming forging have the same size.

6. The forging method of TC11 titanium alloy bar according to claim 1, characterized in that: Forging the fourth bar blank in the first forming forging includes: performing stretching forging on the fourth bar blank using a fifth anvil; The forging of the fifth bar blank in the second forming forging includes: performing stretching forging on the fifth bar blank using a sixth type anvil; The forging of the sixth bar blank in the third forming forging includes: performing stretching forging on the sixth bar blank using a seventh type anvil; Among them, the fifth type anvil, the sixth type anvil and the seventh type anvil are all arc-shaped anvils, and the arc-shaped anvil includes an arc surface and a second top surface, and a third chamfer is arranged between the arc surface and the second top surface, and the radius of the third chamfer of the fifth type anvil, the sixth type anvil and the seventh type anvil decreases successively.

7. The forging method of TC11 titanium alloy bar according to claim 6, characterized in that: The radii of the third chamfered corners of the fifth type anvil, the sixth type anvil and the seventh type anvil are d1 / 5, d1 / 6 and d1 / 7 respectively; The radii corresponding to the arcuate surfaces of the fifth type anvil, the sixth type anvil and the seventh type anvil are d1 / 3, d1 / 4 and d1 / 5 respectively; wherein d1 is the diameter of the rod raw material.

Citation Information

Patent Citations

  • Efficient forging method using curved-surface swage blocks

    CN101513664A

  • Turning method implemented during upper-flat and lower-V anvil stretching

    CN103042152A

  • Blank forging process method for TC11 titanium alloy disc forge piece

    CN115846556A

  • Preparation method of ultrahigh-strength titanium alloy forge piece

    CN116770204A

  • Forging forming method for improving flaw detection level of titanium alloy bar

    CN117324522A