A method for preparing graphene using coal gasification slag
By pre-oxidizing and reducing the residual carbon in coal gasification slag, high value-added graphene is prepared, which solves the problem of high cost of coal gasification slag processing and graphene preparation, realizes low-cost and environmentally friendly production of graphene, and expands waste recycling paths.
Patent Information
- Application Number
- CN202311813077.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-27
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-12-27
AI Technical Summary
Improper treatment of coal gasification slag leads to environmental pollution and resource waste, and existing graphene preparation materials are costly and contain heavy metals, which affects performance.
Graphene is prepared by pre-oxidizing and reducing the residual carbon in the coal gasification residue, using strong acids and oxidants for oxidative intercalation, and then using alkaline solutions for reduction. Specific steps include crushing and drying coal gasification slag, removing aluminosilicates, oxidative intercalation and ultrasonic dispersion, and finally reducing it with an alkaline solution to generate graphene.
It has successfully reduced the cost of graphene preparation, expanded the treatment path of coal gasification slag, realized the reuse of waste, and provided high value-added graphene materials, and the performance of graphene meets application requirements.
Smart Images

Figure CN117963900B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of coal-based solid waste resource treatment technology and graphene preparation technology, and specifically relates to a method for preparing graphene by utilizing coal gasification slag. Background Art
[0002] my country has abundant coal resources and huge demand for coal, but the direct burning of large amounts of coal will cause serious air pollution. Under the influence of this national energy structure, national actual needs and national sustainable development policies, coal gasification technology has developed rapidly as a clean coal technology. At the same time, the waste generated by coal gasification - coal gasification slag has increased by more than 1,000 tons per year, and its annual production in China has exceeded 60 million tons. Coal gasification slag (CGS) refers to a large amount of unburned carbon and ash components produced in the process of generating synthesis gas by thermochemical reaction between coal and gasification agents such as air, oxygen, and water vapor under high temperature and high pressure conditions. The main elements it contains are C, Si, Al, etc., and it contains a small amount of Ca, Fe, Mg, etc. At present, the main treatment methods for CSG in my country are landfill and stacking. This will not only cost a lot of transportation costs, but also seriously occupy land, pollute soil and water bodies, and still cause great harm to my country's environment. Due to the presence of residual carbon and heavy metals in CSG, its application in building materials and agriculture is limited. Therefore, it is of great significance to use CSG to prepare high value-added materials.
[0003] Graphene is a two-dimensional carbon material composed of carbon atoms stacked in different stacking methods in a periodic and closely stacked benzene ring structure (i.e., hexagonal honeycomb structure). It is the first two-dimensional material discovered in the world. Previous studies have confirmed that graphene has excellent electrical and optical properties; extremely high strength and good toughness; extremely high carrier mobility; very good thermal conductivity and other excellent properties. Graphene is widely used and can be applied to basic physics research, sensors, transistors, flexible displays, new energy batteries, seawater desalination, hydrogen storage materials, aerospace, photosensitive elements, composite materials, bioengineering and other fields. At present, the main material for preparing graphene is graphite. The raw material is single and expensive, and graphite contains heavy metals. Graphene prepared from graphite contains heavy metals, which affects the performance and pollutes the environment. Using some waste with high carbon content to prepare graphene can reduce costs and turn waste into treasure.
[0004] Previous studies have shown that compared with other graphene preparation methods, the redox method for preparing graphene has the characteristics of low consumption, low cost, high productivity and simple operation. The redox method for preparing graphene first removes the aluminosilicate in the raw material through a pre-oxidation process, then oxidizes the residual carbon in the raw material from which the aluminosilicate has been removed through an oxidation reaction to generate graphene oxide, and finally, increases the repulsive force between the graphene oxide sheets through a reduction reaction to generate graphene. Therefore, researchers in this field are committed to developing a method for preparing graphene using coal gasification slag. Summary of the invention
[0005] In order to solve the problem of how to utilize residual carbon in coal gasification slag and prepare high value-added graphene, the present invention provides a method for preparing graphene using coal gasification slag.
[0006] To achieve the above-mentioned purpose, the present invention is implemented by the following technical scheme: a method for preparing graphene using coal gasification slag, characterized in that: coal gasification slag with a high carbon content is pre-oxidized and then mixed with a strong acid and an oxidant in proportion, and in the process of oxidizing and intercalating the graphitized residual carbon in the gasification slag, the silicate minerals therein are dissolved, and on this basis, the graphene is obtained after reduction with an alkaline solution.
[0007] The specific steps include:
[0008] (1) Grind and dry coal gasification slag with a carbon content of more than 30% to a moisture content of less than 20%, and sieve for later use;
[0009] (2) Removal of aluminosilicate: Potassium persulfate and strong acid are mixed in proportion, heated in a water bath to 60-100°C, added to the coal gasification slag under medium-speed magnetic stirring, pre-oxidized for 8-12 hours, cooled to room temperature, then diluted with deionized water, filtered, and dried to obtain the coal gasification slag with the aluminosilicate removed;
[0010] (3) Preparation of graphene oxide GO: adding a strong acid to the coal gasification slag obtained in step (2) after removing aluminosilicate under medium-speed magnetic stirring, and then slowly adding a strong oxidant, reacting at 30-40° C. for 2-3 h, adding 80-120 mL of deionized water, and continuing to react for 2-3 h, adding deionized water again to wash until neutral, and then ultrasonicating in the aqueous solution for 1-2 h, filtering, and drying to obtain graphene oxide GO;
[0011] (4) Preparation of graphene: Deionized water is added to the graphene oxide obtained in step (3) to prepare a GO dispersion, a strong base is added to the GO dispersion at 50-90° C., mixed and reacted for 5-6 hours, and then deionized water is added to wash until neutral, filtered, and dried to obtain graphene.
[0012] Preferably, the coal gasification slag is crushed and passed through a 60-80 mesh sieve.
[0013] Preferably, in step (2), the strong acid is concentrated nitric acid, and the ratio of potassium persulfate, strong acid and coal gasification slag is 2.5g:5ml:5g; after filtration, the mixture is dried at 100-120°C for 8-14h.
[0014] Preferably, the strong acid in step (3) is a mixture of concentrated sulfuric acid and concentrated nitric acid, and the mixing volume ratio is 1:1; the strong oxidant is potassium permanganate or potassium dichromate; and the ratio of the coal gasification slag for removing aluminosilicates, the strong acid, and the strong oxidant is 2g:50mL:10g.
[0015] Preferably, the strong base in step (4) is sodium hydroxide or potassium hydroxide, and GO is dispersed in deionized water under ultrasonic conditions of 100 W and 40 kHz for 1 h; the concentration ratio of GO dispersion to strong base is 1-2 mg / ml:8 mol / L, and the volume ratio is 1-2 ml:150 ml.
[0016] The coal gasification slag used in the present invention is coal gasification fine slag with a carbon content of more than 20%.
[0017] The present invention successfully uses the redox method to prepare high-carbon gasification slag into graphene with high added value, expanding a new source of raw materials for graphene preparation. The prepared graphene raw material is the waste generated by coal gasification - coal gasification slag, which expands a new coal gasification slag treatment path and realizes the environmental protection demand of waste recycling. The prepared graphene raw material coal gasification slag has abundant output and low cost, which effectively reduces the preparation cost of graphene. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 A flow chart for preparing graphene using coal gasification slag;
[0019] Figure 2 is the SEM image of the prepared graphene oxide;
[0020] Figure 3 is the SEM image of the prepared graphene;
[0021] Figure 4 is the N2 adsorption-desorption curve of coal gasification slag-based graphene;
[0022] Figure 5 Degradation curves of bisphenol A by coal gasification slag / PMS system and graphene / PMS system; [catalyst] = 0.3 g·L -1 , [PMS]=10mmol, [bisphenol A]=20 mg·L -1 ,T=30℃. DETAILED DESCRIPTION
[0023] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0024] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs, and the disclosure and materials cited therein are hereby incorporated by reference.
[0025] Technical equivalents to the specific embodiments described that are apparent to those skilled in the art using no more than routine experimentation are intended to be encompassed by this application.
[0026] The experimental methods in the following examples are all conventional methods unless otherwise specified. The instruments and equipment used in the following examples are all conventional laboratory instruments and equipment unless otherwise specified; the experimental materials used in the following examples are all purchased from conventional biochemical reagent stores unless otherwise specified.
[0027] Example 1: A method for preparing graphene using coal gasification slag, comprising pre-oxidizing the coal gasification slag with a high carbon content, and then mixing it with a strong acid and an oxidant in proportion. During the process of oxidizing and intercalating the graphitized residual carbon in the gasification slag, aluminosilicate minerals are dissolved therein, and on this basis, graphene is obtained after reduction with an alkaline solution.
[0028] The specific steps are:
[0029] (1) The coal gasification slag was dried and passed through a 60-mesh sieve for later use. The chemical composition and element analysis of the coal gasification slag were determined. The results are shown in Tables 1 and 2.
[0030] Table 1: Chemical composition of coal gasification slag
[0031]
[0032] Table 2: Industrial analysis of coal gasification slag
[0033]
[0034] (2) Take 2.5 g of potassium persulfate and 5 mL of concentrated nitric acid in a beaker, heat it to 80 °C in a water bath, add 5 g of coal gasification slag under medium-speed magnetic stirring, react for 10 h, cool to room temperature, dilute with deionized water, filter, and dry to obtain coal gasification slag with most of the aluminosilicate removed.
[0035] (3) Weigh 2 g of the coal gasification slag obtained after drying in a beaker, add 50 mL of a mixture of concentrated sulfuric acid and concentrated nitric acid (1:1) under medium-speed magnetic stirring, then slowly add 10 g of potassium permanganate, react at 35 ° C for 2 h, add 100 mL of deionized water, continue to react for 2 h, add 100 mL of deionized water again to wash until neutral, ultrasonicate the sample in the aqueous solution for 1 h, filter, and dry to obtain graphene oxide (GO). The SEM image of graphene oxide is shown in the figure Figure 2 shown.
[0036] (4) Under enhanced ultrasonic treatment (100 W, 40 kHz, 1 h), 150 mg of the GO obtained after drying was weighed and dispersed in 150 mL of deionized water to obtain a GO dispersion.
[0037] (5) At a temperature of 50-90°C, 1 mL of sodium hydroxide solution (8 mol / L) was added to the above GO dispersion, mixed and reacted for 5-6 hours, and then washed with deionized water until neutral, filtered, and dried to obtain graphene. The physical adsorption N2 adsorption-desorption curve of the obtained graphene material is as follows: Figure 3 As shown in the SEM images Figure 4 shown.
[0038] (6) Using the graphene prepared above as a catalyst to activate PMS to degrade phenolic organic pollutants, the experiment specifically includes the following steps:
[0039] 1) Add 100 mL of the prepared 20 mg·L -1 654 mg of PMS was added to each of the bisphenol A solutions, and the PMS concentration was 10 mmol·L -1 30 mg of coal gasification slag was added to one beaker, and 30 mg of the above graphene was added to another beaker, and the degradation reaction timing began.
[0040] 2) 1 mL of sample was taken using a disposable syringe at time intervals of 0, 5, 10, 20, 30, 60, 90 and 120 min, respectively. The sample was filtered through a 0.22 μm PES filter and added to a 2 mL brown chromatographic bottle. 0.5 mL of methanol was added to the chromatographic bottle in advance to terminate the ongoing free radical reaction in the sample. The concentration of bisphenol A in the solution was determined by liquid chromatography.
[0041] 3) After the degradation experiment is completed, the solution is filtered to obtain the catalyst after the reaction, which is dispersed in 100 mL of ethanol. After ultrasonic treatment for 45 min, the effect of adsorption on the degradation removal rate of bisphenol A is eliminated, and the concentration of bisphenol A in the solution is measured by liquid chromatography to obtain the concentration of bisphenol A adsorbed by the catalyst. Thus, the concentration of bisphenol A degraded by the catalyst can be known. The degradation curves of bisphenol A by the coal gasification slag / PMS system and the graphene / PMS system are shown in Figure 2. Figure 5 shown.
[0042] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing graphene using coal gasification slag, characterized in that: After pre-oxidation, coal gasification slag with high carbon content is mixed with strong acid and oxidant in proportion, and in the process of oxidizing and intercalating the graphitized residual carbon in the gasification slag, the aluminosilicate minerals therein are dissolved, and on this basis, graphene is obtained after reduction with an alkaline solution; specifically, the following steps are included: (1) Grind and dry coal gasification slag with a carbon content of more than 20% to a moisture content of ≤20%, and sieve for later use; (2) Removal of aluminosilicate: Potassium persulfate and strong acid are mixed in proportion, heated in a water bath to 60-100°C, added to the gasification slag under magnetic stirring, pre-oxidized for 8-12 hours, cooled to room temperature, then diluted with deionized water, filtered, and dried to obtain the gasification slag with aluminosilicate removed; the strong acid is concentrated nitric acid, and the ratio of potassium persulfate, strong acid, and gasification slag is 2.5g:5mL:5g; after filtration, dry at 100-120°C for 8-14 hours; (3) Preparation of graphene oxide GO: adding a strong acid to the coal gasification slag obtained in step (2) after removing aluminosilicate under magnetic stirring conditions, and then slowly adding a strong oxidant, reacting at 30-40°C for 2-3h, adding 80-120mL of deionized water, continuing the reaction for 2-3h, adding deionized water again to wash until neutral, and then ultrasonicating in an aqueous solution for 1-2h, filtering, and drying to obtain graphene oxide GO; the strong acid is a mixture of concentrated sulfuric acid and concentrated nitric acid, and the mixing volume ratio is 1:1; the strong oxidant is potassium permanganate or potassium dichromate; the ratio of the coal gasification slag after removing aluminosilicate, the strong acid, and the strong oxidant is 2g:50mL:10g; (4) preparing graphene: mixing the graphene oxide obtained in step (3) with deionized water to prepare a GO dispersion, adding a strong base to the GO dispersion at 50-90° C., mixing and reacting for 5-6 hours, adding deionized water to wash until neutral, filtering, and drying to obtain graphene; The strong base is sodium hydroxide or potassium hydroxide, and GO is dispersed in deionized water under ultrasonic conditions of 100W and 40kHz for 1h; the concentration ratio of GO dispersion to the strong base is 1-2mg / mL:8mol / L, and the volume ratio is 1-2ml:150mL.
2. The method according to claim 1, characterized in that: The coal gasification slag is crushed and passed through a 60-80 mesh sieve.