A self-repairing sand-containing fog seal layer for light water-induced asphalt pavement and preparation method thereof

By introducing self-healing microcapsules and photopolymers into the sand-containing fog seal layer, the dual-phase self-healing technology of asphalt pavement is realized, which solves the problems of insufficient anti-cracking and anti-aging performance in traditional technology and significantly extends the service life of asphalt pavement. service life and meets green environmental protection requirements.

CN117965101BActive Publication Date: 2024-10-15BEIJING UNIV OF TECH
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410192901.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-21
Publication Date
2024-10-15
Estimated Expiration
2044-02-21

AI Technical Summary

Technical Problem

Traditional sand-containing fog seals are prone to internal micro-cracks, aging and fatigue damage under external vehicle loads and sunlight. They lack self-adjusting healing capabilities, resulting in insufficient anti-cracking and anti-aging properties of asphalt pavements.

Method used

Self-healing microcapsules and photopolymers are introduced into the sand-containing fog seal material, self-healing microcapsules are prepared through interfacial polymerization, and ultraviolet light is used to trigger coumarin-based polyurethane for self-healing, forming a two-phase self-healing technology.

Benefits of technology

Significantly improves the self-healing ability of the sealing layer, can automatically repair micro-cracks under ultraviolet light, prolongs the service life of asphalt pavement, avoids the problem of harsh conditions triggered by photothermal effects in traditional technology, and has the characteristics of green environmental protection and low carbon .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117965101B_ABST
    Figure CN117965101B_ABST
Patent Text Reader

Abstract

The invention discloses a kind of light water-induced asphalt pavement self-repairing sand-containing fog seal and its preparation method, belong to the technical field of road engineering materials, and the present invention is measured by mass, including the following raw materials: 95-100 parts of SBR modified emulsified asphalt, 28-30 parts of water-based epoxy resin, 13-15 parts of water-based curing agent, 2 parts of inorganic stabilizer, 1 part of defoamer, 28-30 parts of machine-made sand, 3-5 parts of self-healing microcapsules and 3-5 parts of photopolymer. The triggering conditions for the two self-repairing means provided by the present invention to play a function are easy to reach, avoiding the drawbacks of harsh triggering conditions such as photothermal effect. While the exciting conditions are green and environmentally friendly, the technical performance of the seal is more excellent, and the problem of early disease of asphalt pavement after a period of use can be solved better and longer, so as to restore the pavement performance and extend the service life of the pavement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of road engineering materials, and in particular relates to a self-repairing sand-containing fog seal layer of an asphalt pavement induced by light water and a preparation method thereof. Background Art

[0002] In recent years, with the rapid and high-quality development of my country's highway industry, the mileage and density of highways have continued to increase. In the current highway system, asphalt roads account for a considerable proportion. However, asphalt pavements generally have a short service life. After a period of use, the asphalt surface layer will show aging, wear, slight cracks, and surface asphalt loss.

[0003] In order to accelerate the construction of road projects, the development of long-life asphalt pavement to the greatest extent is the premise to ensure the economic and environmental protection of road construction. Compared with corrective maintenance, pre-maintenance focuses more on "preventing problems before they happen" and has the characteristics of high cost performance and convenient construction. In the current research, timely preventive maintenance of the pavement is the main measure to extend the life of the pavement.

[0004] Among many pre-maintenance technologies, the sand-containing mist seal has the excellent performance of extending the life of asphalt pavement, good durability and beautifying the pavement, improving the aging, wear, pockmarking, micro-cracks and other minor diseases of the road surface caused by asphalt aging. It is an excellent pavement pre-maintenance technology, and has a short construction period and even meets the construction technology characteristics of non-stop airport flights. In recent years, the sand-containing mist seal technology has gradually attracted widespread attention and research, and has been applied to the pavement surface of important places such as highways, bridge surfaces, and airport pavements. However, under external stimuli such as external vehicle loads and sunlight, the traditional sand-containing mist seal will have problems such as internal microcracks, aging, fatigue damage, and reduced strength after a period of use, and does not have excellent self-adjusting healing ability. After the seal has been used for a period of time, affected by external factors and natural conditions, the seal itself will also have problems such as aging of the binder matrix and the generation of internal micro-cracks.

[0005] Therefore, it is necessary to develop a sealing material with intrinsic self-healing properties to improve the long-term crack resistance and aging resistance of asphalt pavement. Summary of the invention

[0006] The purpose of the present invention is to provide a light-induced asphalt pavement self-repairing sand-containing fog seal and its preparation method to solve the problems existing in the above-mentioned prior art. The present invention proposes to simultaneously introduce microcrack-stimulated self-repairing microcapsules and polymers that can show good self-repairing ability only under light stimulation into the sand-containing fog seal material, thereby achieving the purpose of comprehensively enhancing the self-repair of the seal.

[0007] One of the technical solutions provided by the present invention:

[0008] A self-repairing sand-containing fog seal layer for light water-induced asphalt pavement comprises the following raw materials, measured by weight: 95-100 parts of SBR modified emulsified asphalt, 28-30 parts of water-based epoxy resin, 13-15 parts of water-based curing agent, 2 parts of inorganic stabilizer, 1 part of defoamer, 28-30 parts of machine-made sand, 3-5 parts of self-healing microcapsules and 3-5 parts of photopolymer.

[0009] The SBR modified emulsified asphalt has better viscosity and high and low temperature performance than ordinary emulsified asphalt; in addition, after adding the water-based epoxy resin, the material is more uniform as a whole, and the water-based epoxy resin can form a more uniform structure with the SBR modified emulsified asphalt-based material.

[0010] The waterborne epoxy resin is a liquid phase system material with epoxy resin particles as the dispersed phase and water as the continuous phase. It can be quickly cured at room temperature and in a humid environment. At the same time, the system has smaller interfacial tension, good stability and strong adhesion.

[0011] The water-based curing agent acts as a catalyst for the chemical cross-linking reaction of the water-based epoxy resin, promotes the function of the epoxy resin, and finally cures to form a spatial network structure; in addition, the water-based curing agent is used to adjust the drying time of the fog seal layer, so that the construction curing time can be controlled.

[0012] The inorganic stabilizer is CaCl2 to improve the storage stability of the emulsion.

[0013] The defoaming agent is a polyether-modified silicon defoaming agent to eliminate the foam generated during the preparation process.

[0014] The machine-made sand with good bonding properties with asphalt is selected, and the mass ratio of coarse sand to fine sand is 3:17, wherein the particle size of the coarse sand is 2.36mm-4.75mm, and the particle size of the fine sand is 0.3mm-2.36mm.

[0015] Preferably, the self-healing microcapsules are prepared by interfacial polymerization. The preparation method of the self-healing microcapsules comprises the following steps: using diphenylmethane diisocyanate (MDI) as an oil phase and an emulsifier aqueous solution as an aqueous phase, mixing the aqueous phase and the oil phase, shearing under an ice bath to obtain an oil-in-water emulsion, adding a chain extender to the emulsion, heating the reaction, and preparing the self-healing microcapsules.

[0016] The encapsulation mechanism with MDI as the oil phase is that when the chain extender is added to the emulsion, the amino group provided by the chain extender will undergo interfacial polymerization with the isocyanate functional groups on the surface of the oil phase to quickly generate a polyurea shell, thereby blocking the further penetration of the amino group and reacting with the MDI in the oil phase. Ultimately, part of the MDI is protected and encapsulated in the polyurea shell; the wall material and core material of the prepared self-healing microcapsules are made of the same raw material.

[0017] Self-healing microcapsules with polyurea shell encapsulating MDI were prepared by interfacial polymerization. The preparation method is simple, low-energy, green and environmentally friendly. TGA analysis showed that the initial decomposition temperature of the self-healing microcapsules was 264°C, which is much higher than the initial decomposition temperature of MDI 153°C, indicating that the self-healing microcapsules have good protection and thermal stability and excellent construction and workability.

[0018] More preferably, the volume ratio of the water phase to the oil phase is 4:1.

[0019] More preferably, the concentration of the emulsifier aqueous solution is 1 wt %, and the emulsifier is sodium lignin sulfonate (LS).

[0020] More preferably, the heating temperature is 50° C. and the heating time is 3 hours.

[0021] More preferably, the chain extender is ethylenediamine (EDA).

[0022] Preferably, the preparation method of the photopolymer comprises the following steps: under an inert gas atmosphere, adding a DMF solution of polytetramethylene glycol (PTMEG) to a DMF solution of MDI, heating, keeping warm and stirring during the adding process to form a prepolymer; treating a DMF solution of 7-hydroxy-4-methylcoumarin with a 356nm ultraviolet lamp to generate a coumarin dimer, adding the treated solution to the prepolymer, heating for reaction to obtain a self-healing polymer solution, drying the self-healing polymer solution, and obtaining a translucent polymer, which is the photopolymer.

[0023] More preferably, the molar ratio of MDI, PTMEG and 7-hydroxy-4-methylcoumarin is 2:1:2.

[0024] The present invention aims to improve the self-healing performance of the existing sand-containing fog seal and treat mild road surface diseases more efficiently. Therefore, self-repairing technology is introduced for sand-containing fog seal. Among them, the self-repairing function is embedded in the carrier binder using water-based epoxy modified emulsified asphalt. The overall structure of the carrier has a much stronger ability to resist external force damage than a simple water-based epoxy resin network or an asphalt colloid structure. Self-healing microcapsules are microcapsules prepared with liquefied MDI as the core material and wall material. The microcapsules rupture and release highly active isocyanate groups, which react with moisture (H2O) in the air on the one hand, and react with active secondary hydroxyl groups in waterborne epoxy resin modified asphalt to generate amines on the other hand. Subsequently, the amines polymerize with the remaining isocyanate groups to form a film to fill the internal microcracks, thereby achieving the purpose of repairing the asphalt performance. The photopolymer is a UV-triggered coumarin-based polyurethane prepared from MDI, PTMEG and 7-hydroxy-4-methylcoumarin. After microcracks are generated in the seal layer, the UV-triggered coumarin-based polyurethane under UV irradiation, the coumarin four-membered ring breaks and is reduced to the initial olefin, the mobility of the chain is improved, and the broken segments are easy to combine. At the same time, the number of photoactive groups (coumarin monomers) on both sides of the crack increases, which is conducive to the healing process. Subsequently, coumarin undergoes a [2+2] cyclodimerization reaction to achieve the purpose of self-healing, thereby improving the repair ability of the photopolymer. It can show good self-healing ability only under the stimulation of UV irradiation and is not limited by temperature. The present invention ultimately forms a two-phase self-repairing sand-containing fog sealing layer technology based on the self-repair of self-healing microcapsules and the cross-linking reaction of photopolymers.

[0025] The second technical solution provided by the present invention is:

[0026] A method for preparing the above-mentioned self-repairing sand-containing fog seal layer for light water-induced asphalt pavement comprises the following steps: weighing all raw materials according to parts by mass, mixing SBR modified emulsified asphalt and water-based epoxy resin, adding an inorganic stabilizer, and obtaining a water-based epoxy resin modified emulsified asphalt emulsion component A; adding a defoamer, machine-made sand, self-healing microcapsules and a photopolymer to a water-based curing agent, mixing, and obtaining an emulsion component B; mixing the component A and the component B, and stirring evenly to prepare the self-repairing sand-containing fog seal layer for light water-induced asphalt pavement.

[0027] Preferably, the mass ratio of the component A to the component B is 2:1.

[0028] The sand-containing fog seal material prepared by the present invention has excellent properties such as stable materials during preparation, simple excitation method, and easy reaction conditions; it does not require additional restrictions such as microwave heating, and has environmentally friendly characteristics of being green, environmentally friendly, and low-carbon. It is applied in road surface pre-maintenance to achieve dual-phase self-repair of early road surface damage to fully ensure the service life of the asphalt road surface.

[0029] The third technical solution provided by the present invention is:

[0030] An application of the above-mentioned self-repairing sand-containing fog seal layer of asphalt pavement caused by light water in asphalt pavement maintenance, spraying the self-repairing sand-containing fog seal layer of asphalt pavement caused by light water on the asphalt pavement, with an amount of 1kg / m 2 .

[0031] Preferably, an intelligent spraying vehicle is used to spray the asphalt pavement at high pressure.

[0032] Beneficial effects of the present invention:

[0033] The light-water-induced self-repairing sand-containing fog sealing technology for asphalt pavement proposed in the present invention is a two-phase self-repairing technology of microcapsule self-repair and photopolymer. The embedded self-healing microcapsules have good thermal stability, which provides excellent conditions for the survival of microcapsules. After the microcracks stimulate the microcapsules, the microcapsules release active isocyanate groups, which can not only react with moisture in the air, but also react with active secondary hydroxyl groups in the sealing layer binder-waterborne epoxy resin modified emulsified asphalt. The amines obtained by the reaction are then polymerized with other isocyanate groups to form a film to make up for the internal microcracks. Due to the problem of microcapsule content, microcapsules may not exist at the microcracks, so another chemical reaction self-repairing macromolecular photopolymer (UV-triggered coumarin-based polyurethane) is introduced. Ultraviolet light aging is one of the important reasons for the aging of asphalt pavement. The introduction of this photopolymer can slow down the aging rate of the seal layer and utilize ultraviolet light. It shows good self-healing properties after ultraviolet light irradiation. It can show good self-repairing ability only under ultraviolet light stimulation and is not limited by temperature. The product has excellent mechanical properties, high elasticity, low dissipation efficiency and good thermal stability.

[0034] The main advantage of the present invention is that after the seal layer is constructed, the triggering conditions for the two self-repairing means to function are easy to achieve, avoiding the drawbacks of strict triggering conditions such as photothermal effect (essentially heating). It is a green technology innovation, with lower energy consumption than microwave heating, the seal layer saves manpower and material resources in its self-repairing function, and the stimulating conditions (water and light) are green and environmentally friendly. At the same time, the technical performance of the seal layer is more excellent, which can better and longer solve the problem of early diseases of asphalt pavement after a period of use, and achieve the purpose of restoring pavement performance and extending the service life of the pavement. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0036] Figure 1The present invention is a process flow chart for preparing a self-repairing sand-containing fog seal layer for a light water-induced asphalt pavement. DETAILED DESCRIPTION

[0037] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0038] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0039] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0040] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present application description and examples are exemplary only.

[0041] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0042] The present invention introduces self-repairing technology into the base material of the sand-containing fog seal layer to repair the damage caused by aging and other factors, thereby extending the service life of the sand-containing fog seal layer. The self-repairing capsule technology is introduced. After the microcracks stimulate the capsule, the repair agent flows out and reacts with the water vapor in the air and the active hydroxyl groups in the aqueous carrier of the fog seal layer to form a series of reactions to form macromolecules, which polymerize into a film to make up for the microcracks inside the seal layer; a photochemical reaction polymer (ultraviolet light-triggered coumarin-based polyurethane) is introduced. Under ultraviolet light irradiation, the four-membered ring of coumarin breaks and is reduced to the initial olefin, the mobility of the chain is improved, and the broken segments are easy to combine. At the same time, the number of photoactive groups (coumarin monomers) on both sides of the crack increases, which is conducive to the healing process. Subsequently, coumarin undergoes a [2+2] cyclodimerization reaction to achieve the purpose of self-healing, thereby improving the repair ability of the polymer, and finally forming a two-phase self-repairing sand-containing fog seal layer technology based on microcapsule self-repair and photo-triggered polymer reconstruction cross-linking reaction.

[0043] The room temperature in the present invention refers to 25±2°C.

[0044] The “parts” in the embodiments of the present invention are all measured by mass.

[0045] The raw materials required in the examples of the present invention and the comparative examples were all purchased from commercial sources. SBR modified emulsified asphalt was purchased from Guangdong Dashun New Materials Co., Ltd., waterborne epoxy resin and waterborne curing agent were purchased from Xi'an Huaze Road Materials Co., Ltd., LS and EDA were purchased from Beijing Mairida Technology Co., Ltd., MDI and PTMEG were purchased from Beijing Inokai Technology Co., Ltd., DMF was purchased from Shanghai Mairuier Biochemical Technology Co., Ltd., and 7-hydroxy-4-methylcoumarin was purchased from Shanghai Titan Technology Co., Ltd.

[0046] Machine-made sand with good bonding properties with asphalt was selected, and the mass ratio of coarse sand to fine sand was 3:17, wherein the particle size of the coarse sand was 2.36 mm-4.75 mm, and the particle size of the fine sand was 0.3 mm-2.36 mm, and they were purchased from Hebei Wenhao Mineral Products Co., Ltd.

[0047] In the embodiment of the present invention, the water-based curing agent is triethylenetetramine, the defoaming agent is polyether-modified silicone oil, purchased from Qingdao Meiside Silicone Co., Ltd.; the inorganic stabilizer is CaCl2, purchased from Bainowei Biotechnology Co., Ltd.

[0048] Example 1

[0049] Preparation method of self-healing microcapsules:

[0050] LS was added into deionized water and mechanically stirred for 10 minutes to dissolve, to prepare an emulsifier aqueous solution with a concentration of 1 wt% as the water phase, and MDI was used as the oil phase, and the mixture was mixed at a water-oil volume ratio of 4:1. The mixed solution was sheared and stirred at a speed of 2500 r / min for 8 minutes in an ice bath to obtain an oil-in-water (O / W) emulsion; the container containing the above 300 mL emulsion was placed in a water bath, and 15 mL of EDA was added dropwise into the emulsion with a syringe. After the addition was completed, the water bath was heated to 50°C and reacted for 3 hours to prepare self-healing microcapsules.

[0051] Example 2

[0052] Preparation method of photopolymer

[0053] 0.05 mol MDI was dissolved in 100 mL DMF and added to a three-necked round-bottom flask. 0.025 mol PTMEG was dried in vacuum at 100 °C for 4 h to remove moisture, and then dissolved in 150 mL DMF. Under the protection of nitrogen, the DMF solution of PTMEG was slowly added to the three-necked flask at 80 °C using a pressure funnel and stirred for 3 h to form a prepolymer. 0.05 mol 7-hydroxy-4-methylcoumarin was dissolved in 100 mL DMF and heated under a 365 nm ultraviolet lamp (14.4 mW / cm 2 ) for 10 minutes to form a coumarin dimer; the irradiated solution was slowly added to a three-necked round-bottom flask using a funnel, and the reaction was continued at 80°C for 12 hours to obtain a self-healing polymer solution, which was then poured into a Teflon mold and dried at 50°C for 24 hours and then at 80°C for 2 hours to completely remove the solvent. The obtained translucent polymer with a molar ratio of MDI / PTMEG / 7-hydroxy-4-methylcoumarin of 2 / 1 / 2 was a UV-triggered coumarin-based polyurethane, that is, a photopolymer.

[0054] Embodiment 3-5

[0055] A preparation method for self-repairing sand-containing fog seal layer of light water-induced asphalt pavement

[0056] Weigh the raw materials according to the mass fractions in Table 1.

[0057] Table 1

[0058] SBR modified emulsified asphalt Waterborne Epoxy Resin Triethylenetetramine <![CDATA[CaCl2]]> Polyether modified silicone oil Machine-made sand Self-healing microcapsules Photopolymer Example 3 100 30 15 2 1 30 5 5 Example 4 97 29 14 2 1 29 4 4 Example 5 95 28 13 2 1 28 3 3

[0059] S1. The SBR modified emulsified asphalt and the waterborne epoxy resin were heated to 70°C, and then sheared at a rate of 1000 r / min, respectively. Then, the SBR modified emulsified asphalt was added to the waterborne epoxy resin, and then sheared at a rate of 3000 r / min for 60 min, and CaCl2 was added to obtain a waterborne epoxy resin modified emulsified asphalt emulsion component A;

[0060] S2. polyether-modified silicone oil, machine-made sand, self-healing microcapsules prepared in Example 1 and photopolymer prepared in Example 2 were sequentially added to triethylenetetramine, and stirred at a shear rate of 2000 r / min for 20 min to obtain emulsion component B;

[0061] S3. Component A and component B are mixed in a mass ratio of 2:1, and stirred continuously at a rate of 2500 r / min for 60 s to obtain a light water-induced self-repairing sand-containing fog seal layer for asphalt pavement.

[0062] It should be noted that Examples 3-5 have the same status and differ only in formulation and effect, which are all within the scope of the formulation of this patent. Only Example 3 is selected for comparison below. Figure 1 The present invention is a process flow chart for preparing a self-repairing sand-containing fog seal layer for a light water-induced asphalt pavement.

[0063] Comparative Example 1

[0064] The same as Example 3, except that no self-healing microcapsules are added in step S2.

[0065] Comparative Example 2

[0066] The same as Example 3, except that no photopolymer is added in step S2.

[0067] Comparative Example 3 Preparation method of ordinary water-based epoxy modified emulsified asphalt containing sand mist seal

[0068] The same as Example 3, except that no self-healing microcapsules and photopolymers are added in step S2.

[0069] Performance test

[0070] Crack resistance test:

[0071] The asphalt sand-containing fog seal samples of Example 3 and Comparative Examples 1-3 were coated on high modulus thin steel sheets for low-temperature brittle fracture, and then placed in a photo-oxidation box for treatment for 40 minutes. The difference in the repair ability of the sand-containing fog seals of Example 3 and Comparative Examples 1-3 for cracks was evaluated, respectively. This proves that the self-repairing effect of the dual-phase self-repairing sand-containing fog seal based on self-healing microcapsules and photopolymer cross-linking reaction of the present invention is good. The results are shown in Table 2.

[0072] Table 2

[0073] Test items Mechanical properties Example 3 The cracks are not visible and the stress curve is close to 91% of the original sample Comparative Example 1 The crack is partially healed and the stress curve is close to 43% of the original sample. Comparative Example 2 The crack is partially healed and the stress curve is close to 49% of the original sample. Comparative Example 3 Cracks only slightly healed

[0074] The above test results show that the light water-induced asphalt pavement self-repairing sand-containing fog seal provided by the present invention has a stronger effect on repairing film cracks than the single-phase self-repairing system, namely, Comparative Example 1 and Comparative Example 2; and the effect on repairing film cracks is much stronger than that of the ordinary water-based epoxy modified emulsified asphalt sand-containing fog seal, namely, Comparative Example 3.

[0075] Anti-wear performance test:

[0076] According to the wet wheel abrasion test in the "Highway Engineering Asphalt and Asphalt Mixture Test Procedure", the anti-wear performance of the asphalt sand-containing mist seal layer of Example 3 and Comparative Examples 1-3 was compared. Four groups of wet wheel abrasion test pieces were prepared, named A, B, C, and D respectively; then the wet wheel abrasion test was performed on them respectively, and the wear value WTAT was measured; then the four types of sand-containing mist seal layers were coated on the test pieces A, B, C, and D respectively, and the above test steps were repeated to measure the wear value WTAT, so as to analyze the anti-wear performance of the sand-containing mist seal layer. The results are shown in Table 3.

[0077] Table 3

[0078] A-original B-Original C-Original D-Original A-Example 3 B-Comparative Example 1 C-Comparative Example 2 D-Comparative Example 3 <![CDATA[WTAT(g / m 2 )]]> 181.2 189.6 168.7 190.3 90.7 120.6 100.3 130.8

[0079] The above test results show that after the four specimens were coated with the four types of sand-containing mist seal materials, the wear values ​​of the four specimens all showed a significant decrease, indicating that the sand-containing mist seal material of the present invention has a good consolidation effect on the loose aggregates on the surface of the specimens. Among them, the wear value of the specimen coated with the sand-containing mist seal material of Example 3 decreased by 49.9%, the wear value of the specimen coated with the sand-containing mist seal material of Comparative Example 1 decreased by 36.4%, the wear value of the specimen coated with the sand-containing mist seal material of Comparative Example 2 decreased by 40.5%, and the wear value of the specimen coated with the sand-containing mist seal material of Comparative Example 3 decreased by 31.3%, indicating that the anti-wear performance of the light water-induced asphalt pavement self-repairing sand-containing mist seal provided by the present invention is stronger than that of the single-phase self-repairing system, namely, Comparative Example 1 and Comparative Example 2; and much stronger than that of the ordinary water-based epoxy modified emulsified asphalt containing sand mist seal, namely, Comparative Example 3.

[0080] In summary, the self-repairing microcapsules and photopolymers (UV-triggered coumarin-based polyurethane) in the dual-phase self-repairing technology introduced by the present invention for the sand-containing fog seal layer are stable when not excited, the excitation conditions are simple and easy to obtain, and the repair after excitation is significant. It belongs to green technology innovation and meets the requirements of ecological and environmental protection.

[0081] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A self-repairing sand-containing fog seal layer for light water-induced asphalt pavement, characterized in that: The raw materials include, by weight: 95-100 parts of SBR modified emulsified asphalt, 28-30 parts of waterborne epoxy resin, 13-15 parts of waterborne curing agent, 2 parts of inorganic stabilizer, 1 part of defoamer, 28-30 parts of machine-made sand, 3-5 parts of self-healing microcapsules and 3-5 parts of photopolymer; The self-healing microcapsules are prepared by interfacial polymerization; The preparation method of the self-healing microcapsule comprises the following steps: using diphenylmethane diisocyanate as an oil phase and an emulsifier aqueous solution as a water phase, mixing the water phase and the oil phase, shearing under an ice bath to obtain an oil-in-water emulsion, adding a chain extender to the emulsion, heating for reaction, and preparing the self-healing microcapsule, wherein the chain extender is ethylenediamine; The preparation method of the photopolymer comprises the following steps: adding a DMF solution of polytetramethylene glycol to a DMF solution of diphenylmethane diisocyanate under an inert gas atmosphere, heating, keeping warm and stirring during the adding process to form a prepolymer; treating a DMF solution of 7-hydroxy-4-methylcoumarin with a 356nm ultraviolet lamp to generate a coumarin dimer, adding the treated solution to the prepolymer, heating for reaction to obtain a self-healing polymer solution, and drying the self-healing polymer solution to obtain a translucent polymer, namely the photopolymer.

2. The self-repairing sand-containing fog seal layer for light water-induced asphalt pavement according to claim 1 is characterized in that: The volume ratio of the water phase to the oil phase is 4:

1.

3. The self-repairing sand-containing fog seal layer for light water-induced asphalt pavement according to claim 2 is characterized in that: The molar ratio of the diphenylmethane diisocyanate, polytetramethylene glycol and 7-hydroxy-4-methylcoumarin is 2:1:

2.

4. A method for preparing a self-repairing sand-containing fog seal layer for a light water-induced asphalt pavement as claimed in any one of claims 1 to 3, characterized in that: All raw materials are weighed according to their mass parts, the SBR modified emulsified asphalt and the water-based epoxy resin are mixed, and an inorganic stabilizer is added to obtain a water-based epoxy resin modified emulsified asphalt emulsion component A; a defoamer, machine-made sand, self-healing microcapsules and photopolymer are added to the water-based curing agent, and the mixture is mixed to obtain an emulsion component B, and the component A and the component B are mixed and stirred evenly to prepare the light water-induced asphalt pavement self-repairing sand-containing fog seal layer.

5. The preparation method according to claim 4, characterized in that: The mass ratio of the A component to the B component is 2:

1.

6. An application of the light water-induced self-repairing sand-containing fog seal layer of asphalt pavement according to any one of claims 1 to 3 in asphalt pavement maintenance, characterized in that: The self-repairing sand-containing fog seal layer of the light water-induced asphalt pavement is sprayed on the asphalt pavement at a dosage of 1 kg / m 2 .

Citation Information

Patent Citations

  • Preparation method for microcapsules coating air-drying film forming material

    CN104147987A

  • Self-repairing waterborne epoxy / asphalt compound waterproof coating and preparation method thereof

    CN107446502A

  • Epoxy modified emulsified asphalt sand-fog-containing sealing layer material and preparation method and application thereof

    CN108070269A

  • Light- or heat-induced self-repairing elastomer as well as preparation method and application thereof

    CN111471154A

  • Photo-initiated self-repairing shape memory polyurethane as well as preparation method and application thereof