Ultra-high strength cold-rolled steel sheet with excellent hole expansion properties and its manufacturing method

By designing cold-rolled steel sheets with specific compositions and heat treatment processes, the problem of temperature deviation caused by water cooling has been solved, achieving high strength and excellent hole expansion properties, improving the operability and material uniformity of roll forming, and reducing equipment and process costs.

CN117980524BActive Publication Date: 2026-11-17POHANG IRON & STEEL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202280063997.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-09-23
Filing Date
2022-09-23
Publication Date
2026-11-17
Estimated Expiration
2042-09-23

AI Technical Summary

Technical Problem

Existing high-strength steel plates are prone to temperature deviations during water cooling, resulting in poor shape quality and uneven material, which limits the operability and application of roll forming. Furthermore, hot pressing equipment investment and process costs are high.

Method used

Cold-rolled steel sheets with specific compositions containing elements such as C, Si, Mn, P, S, Al, Cr, Mo, Ti, Nb, B, and N are used. Through fine microstructure design and controlled heat treatment processes, including slow cooling and rapid cooling, tempered martensite or mixed martensite microstructures are formed, ensuring high strength and excellent porosity.

Benefits of technology

It achieves tensile strength of over 1470MPa and excellent pore expansion properties, solves the temperature deviation problem, improves the operability and material uniformity of roll forming, and reduces equipment and process costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117980524B_ABST
    Figure CN117980524B_ABST
Patent Text Reader

Abstract

This invention relates to an ultra-high strength cold-rolled steel sheet with excellent hole expansion properties and its manufacturing method, and more specifically, to an ultra-high strength cold-rolled steel sheet with excellent hole expansion properties that can be mainly used in automotive collision and structural components and its manufacturing method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to an ultra-high strength cold-rolled steel sheet with excellent hole expansion properties and its manufacturing method, and more specifically, to an ultra-high strength cold-rolled steel sheet with excellent hole expansion properties that can be mainly used in automotive collision and structural components and its manufacturing method. Background Technology

[0002] Steel sheets used in automobiles need to be lightweight to protect the environment, while simultaneously meeting the conflicting goals of ensuring crash safety for passengers. To this end, various steel sheets for automobiles are being developed, including dual-phase (DP) steel, transformation-induced plasticity (TRIP) steel, and complex-phase (CP) steel. However, the achievable tensile strength limit in these advanced high-strength steels (AHSS) is approximately 1200 MPa. Therefore, hot press forming is gaining attention. In this process, to ensure crash safety, structural components are formed at high temperatures and then rapidly cooled (water-cooled) in direct contact with the die to ensure final strength. However, due to high equipment investment costs and high heat treatment and processing costs, its application has not yet been widely adopted.

[0003] Furthermore, roll forming, a more productive process compared to conventional stamping and hot pressing, involves creating complex shapes through segmented roll forming. It is typically used for forming components from ultra-high-strength materials with low elongation, and its application is expanding. Steel sheets used in this roll forming process are primarily manufactured in continuous annealing equipment equipped with water cooling. However, its drawbacks include poor shape quality due to temperature variations in the width and length directions during water cooling, leading to decreased operability and material deviations at different locations. Therefore, alternative methods for rapid cooling via water cooling need to be developed. Summary of the Invention

[0004] Technical problems to be solved

[0005] One aspect of the present invention is to provide an ultra-high strength cold-rolled steel sheet with excellent hole expansion properties and a method for manufacturing the same.

[0006] Technical solution

[0007] One embodiment of the present invention provides an ultra-high strength cold-rolled steel sheet with excellent hole expansion properties. The cold-rolled steel sheet, by weight percent, comprises: C: 0.2-0.4%, Si: less than 0.5% (excluding 0%), Mn: 1.0-2.0%, P: less than 0.03% (excluding 0%), S: less than 0.015% (excluding 0%), Al: less than 0.1% (excluding 0%), Cr: less than 0.5% (excluding 0%), Mo: less than 0.2% (excluding 0%), Ti: less than 0.1% (excluding 0%), Nb: less than 0.1% (excluding 0%), B: less than 0.005% (excluding 0%), N: less than 0.01% (excluding 0%), with the balance being Fe and other unavoidable impurities. The microstructure of the cold-rolled steel sheet consists of a single-phase tempered martensite or a mixed microstructure of martensite and tempered martensite. The microstructure has a F content of 45 μm × 45 μm per unit area. HAGB For more than 60% of the area, L HAGB It is 8mm or more.

[0008] (wherein, the F) HAGB L represents the fraction of grains with large-angle grain boundaries. HAGB This indicates the total length of grain boundaries with large angles, where a large angle grain boundary is defined as a grain boundary where the orientation difference angle between adjacent grains is 15° or more.

[0009] Another embodiment of the present invention provides a method for manufacturing ultra-high strength cold-rolled steel sheet with excellent hole expansion properties, the method comprising the following steps: heating a steel billet to a temperature of 1100-1300°C, wherein the steel billet, by weight%, comprises: C: 0.2-0.4%, Si: less than 0.5% (except 0%), Mn: 1.0-2.0%, P: less than 0.03% (except 0%), S: less than 0.015% (except 0%), Al: less than 0.1% (except 0%), Cr: less than 0.5% (except 0%), Mo: less than 0.2% (except 0%), Ti: less than 0.1% (except 0%), Nb: less than 0.1% (except 0%), B: less than 0.005% (except 0%), N: less than 0.01%. (Except for 0%), the balance of Fe and other unavoidable impurities; hot finishing rolling of the heated billet at a temperature above Ar3 to obtain hot-rolled steel sheet; coiling the hot-rolled steel sheet at a temperature below 720°C; cold rolling the coiled hot-rolled steel sheet to obtain cold-rolled steel sheet; annealing the cold-rolled steel sheet at a temperature range of 780-900°C; slowly cooling the annealed cold-rolled steel sheet at a cooling rate of less than 5°C / second to 650-750°C; rapidly cooling the slowly cooled cold-rolled steel sheet at a cooling rate of more than 40°C / second to below 150°C; and reheating and over-aging heat treatment of the rapidly cooled cold-rolled steel sheet at 180-240°C.

[0010] Invention Effects

[0011] According to one aspect of the present invention, an ultra-high strength cold-rolled steel sheet with excellent hole expansion properties and a tensile strength of 1470 MPa or higher can be provided, as well as a method for manufacturing the same. Attached Figure Description

[0012] Figure 1 These are photographs taken using an optical microscope to observe Invention Example 5 and Comparative Example 5 according to an embodiment of the present invention.

[0013] Figure 2 These are photographs of large-angle and small-angle grain boundaries after measuring and analyzing the fine structure of Invention Example 5 and Comparative Example 5 according to an embodiment of the present invention using electron backscatter diffraction attached to a scanning electron microscope.

[0014] Best practice

[0015] The following describes an ultra-high strength cold-rolled steel sheet with excellent hole-expanding properties according to an embodiment of the present invention. First, the alloy composition of the present invention will be described. Unless otherwise stated, the alloy composition content described below is expressed in weight %.

[0016] C: 0.2-0.4%

[0017] Carbon (C) is an element added to ensure the strength of martensite; for the aforementioned effect, it is preferable to add 0.2% or more of C. However, when the C content exceeds 0.4%, weldability may deteriorate. Therefore, the C content is preferably in the range of 0.2-0.4%. The lower limit of the C content is more preferably 0.21%, and even more preferably 0.22%. The upper limit of the C content is more preferably 0.3%, even more preferably 0.29%, and most preferably 0.28%.

[0018] Si: less than 0.5% (except 0%)

[0019] Si is a ferrite stabilizing element, but its disadvantage is that it promotes ferrite formation during slow cooling after annealing in a continuous annealing furnace with a slow cooling zone, thereby weakening the strength. Furthermore, during annealing, surface enrichment and oxidation caused by Si pose a risk of indentation defects. Therefore, the Si content is preferably in the range of 0.5% or less. More preferably, the Si content is 0.4% or less, and even more preferably 0.3% or less.

[0020] Mn: 1.0-2.0%

[0021] Mn is an element that inhibits ferrite formation and facilitates austenite formation. When the Mn content is less than 1.0%, ferrite is easily formed during slow cooling; on the other hand, when the Mn content exceeds 2.0%, bending workability, resistance to delayed fracture, and weldability may decrease. Therefore, the Mn content is preferably in the range of 1.0-2.0%. The lower limit of the Mn content is more preferably 1.3%, and even more preferably 1.5%.

[0022] P: Below 0.03% (except 0%)

[0023] P is an impurity element. When the content of P exceeds 0.03%, weldability decreases, the risk of steel brittleness increases, and the possibility of indentation defects increases. Therefore, it is preferable to limit the upper limit of the P content to 0.03%. The content of P is more preferably 0.025% or less, and even more preferably 0.02% or less.

[0024] S: Less than 0.015% (except 0%)

[0025] Similar to P, S is an impurity element and an element that impairs the ductility and weldability of steel sheets. When the S content exceeds 0.015%, the likelihood of impairing the ductility and weldability of the steel sheet is high; therefore, it is preferable to limit the upper limit of the S content to 0.015%. More preferably, the S content is 0.01% or less, and even more preferably 0.005% or less.

[0026] Al: Less than 0.1% (except 0%)

[0027] Al is an alloying element that expands the ferrite phase transformation range. However, when using a continuous annealing process with a slow cooling range as shown in this invention, it has the disadvantage of promoting ferrite formation. Furthermore, the formation of AlN may lead to a decrease in high-temperature hot rollability. Therefore, the upper limit of the Al content is limited to 0.1%. The Al content is more preferably 0.07% or less, and even more preferably 0.05% or less.

[0028] Cr: less than 0.5% (except 0%)

[0029] Cr is an alloying element that readily ensures low-temperature phase transformation structures by suppressing ferrite phase transformation. In the case of a continuous annealing process with slow cooling, as shown in this invention, it has the advantage of suppressing ferrite formation. However, when the Cr content exceeds 0.5%, the resistance to delayed fracture may deteriorate, and carbides such as CrC may form, impairing hole expansion and bending workability. Furthermore, excessive alloy addition may lead to increased costs. Therefore, the Cr content is preferably in the range of 0.5% or less. More preferably, the Cr content is 0.4% or less, and even more preferably 0.3% or less.

[0030] Mo: less than 0.2% (except 0%)

[0031] Mo has the effect of improving the hardenability of steel, generating fine Mo-containing carbides that serve as hydrogen trapping sites, and improving resistance to delayed fracture by refining martensite. However, when the Mo content is 0.2% or more, the chemical conversion treatability may deteriorate, and there is an increase in cost; therefore, it is preferable to limit the range of the Mo content. Thus, the Mo content is preferably in the range of less than 0.2%. The lower limit of the Mo content is more preferably 0.03%, further preferably 0.05%, and most preferably 0.1%.

[0032] Ti: Less than 0.1% (except 0%)

[0033] Ti is a nitride-forming element and is used to scavenge nitrogen in steel by causing nitrogen to precipitate as TiN. Without the addition of Ti, cracks may occur during continuous casting due to the formation of AlN. However, when the Ti content exceeds 0.1%, in addition to the removal of dissolved nitrogen, the precipitation of additional carbides may lead to a decrease in martensitic strength, and the formation of carbonitrides such as TiC and TiN may impair porosity and bending workability. Therefore, the Ti content is preferably in the range of 0.1% or less. More preferably, the Ti content is 0.07% or less, and even more preferably 0.05% or less. Furthermore, for the scavenging effect and to suppress AlN formation, the amount of Ti added can be 48 / 14*[N] or more stoichiometric equivalents.

[0034] Nb: less than 0.1% (except 0%)

[0035] Nitrogen oxides (Nb) are elements that segregate at austenite grain boundaries and suppress austenite grain coarsening during annealing heat treatment. However, when the Nb content exceeds 0.1%, the precipitation of carbides, nitrides, etc., increases, thereby reducing the machinability of the base material, and the cost increases as the alloying amount becomes excessive. Therefore, the Nb content is preferably in the range of 0.1% or less. More preferably, the Nb content is 0.08% or less, and even more preferably 0.06% or less.

[0036] B: Less than 0.005% (excluding 0%)

[0037] The element B is used to suppress ferrite formation, thus providing the advantage of suppressing ferrite formation during cooling after annealing in this invention. However, when the content of B exceeds 0.005%, ductility may decrease. Therefore, the content of B is preferably in the range of 0.005% or less. More preferably, the content of B is 0.004% or less, and most preferably 0.003% or less.

[0038] N: Less than 0.01% (except 0%)

[0039] N is an impurity element. When the content of N exceeds 0.01%, the risk of cracking during continuous casting increases significantly due to the formation of AlN and the like. Therefore, it is preferable to limit the upper limit of the N content to 0.01%. The content of N is more preferably 0.008% or less, and most preferably 0.006% or less.

[0040] In addition to the steel composition described above, the remaining components may include Fe and unavoidable impurities. Unavoidable impurities are those that may be unintentionally introduced during conventional steel manufacturing processes, and therefore cannot be completely eliminated; their meaning is easily understood by those skilled in the art of conventional steel manufacturing. Furthermore, this invention does not completely exclude the addition of other components besides the steel composition described above.

[0041] In addition, the cold-rolled steel sheet of the present invention may further contain one or more of Cu and Ni, less than 0.5% and less than 0.5%.

[0042] Cu: less than 0.5%

[0043] Cu improves corrosion resistance and inhibits hydrogen intrusion by coating the steel plate surface. However, when the Cu content exceeds 0.5%, it may cause surface defects. Therefore, the Cu content is preferably in the range of 0.5% or less. More preferably, the Cu content is 0.4% or less, and even more preferably 0.3% or less.

[0044] Ni: below 0.5%

[0045] Similar to Cu, Ni also improves corrosion resistance and reduces surface defects that are easily caused by the addition of Cu. However, when the Ni content exceeds 0.5%, the formation of oxide scale in the furnace becomes uneven, which may contribute to surface defects. Therefore, the Ni content is preferably in the range of 0.5% or less. More preferably, the Ni content is 0.4% or less, and even more preferably 0.3% or less.

[0046] In addition, the cold-rolled steel sheet of the present invention may further contain less than 0.05% Sb.

[0047] Sb: below 0.05%

[0048] Sb is an element that inhibits surface oxidation or nitriding, thus contributing to increased strength and improved resistance to delayed fracture. However, when the Sb content exceeds 0.05%, castability may deteriorate, and resistance to delayed fracture may decrease. Therefore, the Sb content is preferably in the range of 0.05% or less. More preferably, the Sb content is 0.04% or less, and even more preferably 0.03% or less.

[0049] The microstructure of an ultra-high strength cold-rolled steel sheet with excellent porosity according to one embodiment of the present invention will now be described.

[0050] The microstructure of the cold-rolled steel sheet of the present invention preferably consists of a single-phase tempered martensite microstructure or a mixed microstructure of martensite and tempered martensite. As described above, by making the microstructure consist of a single-phase tempered martensite microstructure or a mixed microstructure of martensite and tempered martensite, high yield strength and excellent porosity can be obtained. The microstructure of the present invention is more preferably a single-phase tempered martensite microstructure, but since tempering does not occur completely during the manufacturing process, it can also consist of a mixed microstructure of martensite and tempered martensite. In the present invention, the fraction of the mixed microstructure of martensite and tempered martensite is not particularly limited, but for example, the fraction of tempered martensite in the mixed microstructure can be 80% or more, more preferably 90% or more.

[0051] Furthermore, the F per unit area of ​​the fine tissue of the present invention is 45μm×45μm. HAGB Preferably, it is 60% or more in area, L HAGB Preferably, it is 8mm or more. At this time, the F... HAGB L represents the fraction of grains with large-angle grain boundaries. HAGB This represents the total length of grain boundaries with large-angle grain boundaries, where a large-angle grain boundary is defined as a grain boundary where the orientation difference angle between adjacent grains is 15° or greater. When the F... HAGB Less than 60% of the area or the L HAGB When the diameter is less than 8mm, the hole expansion capability deteriorates.

[0052] Furthermore, the average grain size of the original austenite in the cold-rolled steel sheet of the present invention can be less than 6 μm. When the average grain size of the original austenite exceeds 6 μm, there may be disadvantages such as poor hole expansion and bending workability.

[0053] The cold-rolled steel sheet of the present invention provided as described above has a tensile strength (TS) of 1470 MPa or more and a tensile strength (TS)(MPa) × hole expansion ratio (HER)(%) of 73500 MPa·% or more, thus ensuring both ultra-high strength and excellent hole expansion properties.

[0054] The following describes a method for manufacturing an ultra-high strength cold-rolled steel sheet with excellent hole expansion properties according to one embodiment of the present invention.

[0055] First, the steel billet having the above alloy composition is heated to a temperature of 1100-1300°C. When the heating temperature is below 1100°C, a sharp increase in hot rolling load occurs; when the heating temperature exceeds 1300°C, the amount of surface oxide scale increases, which may lead to material loss. Therefore, the heating temperature of the steel billet is preferably in the range of 1100-1300°C.

[0056] Subsequently, the heated steel billet is hot-finished at a temperature above Ar3 to obtain hot-rolled steel sheet. Ar3 is the temperature at which ferrite begins to appear when austenite is cooled. When the finishing rolling temperature is below Ar3, rolling occurs in the two-phase region of ferrite and austenite, or in the ferrite region, thereby forming a mixed-grain structure, and may cause malfunctions in the hot rolling equipment due to variations in the hot rolling load. The hot finishing rolling temperature is more preferably above 800°C, further preferably above 850°C, and most preferably above 900°C.

[0057] Subsequently, the hot-rolled steel sheet is coiled at a temperature below 720°C. When the coiling temperature exceeds 720°C, excessive oxide film is generated on the surface of the steel sheet, which may lead to defects. As the coiling temperature decreases, the strength of the hot-rolled steel sheet increases, resulting in an increased rolling load for subsequent cold rolling processes. However, this is not a factor that makes actual production impossible; therefore, the lower limit of the coiling temperature is not particularly limited in this invention. The coiling temperature is more preferably below 700°C, further preferably below 680°C, and most preferably below 650°C.

[0058] Subsequently, the hot-rolled steel sheet that has been coiled is cold-rolled to obtain a cold-rolled steel sheet. In this invention, the cold rolling process is not particularly limited, and all processes commonly used in this art can be utilized. Furthermore, a pickling process can be performed prior to the cold rolling process.

[0059] Subsequently, the cold-rolled steel sheet is annealed at a temperature range of 780-900°C. When the annealing temperature is below 780°C, the strength may decrease due to the formation of a large amount of ferrite. Furthermore, when joining with other steels annealed at 800°C or higher, material deviations may occur due to the temperature gradient between the top and end portions of the steel. On the other hand, when the annealing temperature exceeds 900°C, the durability of the continuous annealing furnace deteriorates, potentially causing difficulties in product manufacturing. Therefore, the annealing temperature preferably falls within the range of 780-900°C. The lower limit of the annealing temperature is more preferably 800°C, further preferably 820°C, and most preferably 840°C. The upper limit of the annealing temperature is more preferably 880°C, and further preferably 860°C.

[0060] Subsequently, the cold-rolled steel sheet subjected to the annealing heat treatment is slowly cooled to 650-750°C at a cooling rate of less than 5°C / second. Generally, in a continuous annealing furnace, a slow cooling zone exists after the annealing heat treatment. That is, slow cooling occurs within a certain range after the annealing heat treatment process. Typically, in the case of a continuous annealing furnace including a slow cooling zone, there is a slow cooling zone of 100-200 m after annealing. The disadvantage is that after annealing at high temperatures, the slow cooling leads to the formation of soft phases such as ferrite, making the manufacture of ultra-high strength steel difficult. For example, in the case of a 160 m slow cooling zone, with a steel sheet throughput speed of 160 m / min, the holding time in the slow cooling zone is 60 seconds, and with an annealing temperature of 830°C and a final temperature of 650°C in the slow cooling zone, the cooling rate of the slow cooling zone is very low, only 3°C / second. Therefore, the possibility of forming soft phases such as ferrite becomes very high. In addition, in order to make the cooling rate during slow cooling after annealing exceed 5°C / second, an additional cooling device needs to be introduced, which may lead to problems such as manufacturing costs or equipment replacement.

[0061] Therefore, in this invention, the cold-rolled steel sheet, after being slowly cooled, is rapidly cooled at a rate of 40°C / second or higher to below 150°C. This rapid cooling process allows the fine microstructure to transform into martensite. When the rapid cooling rate is less than 40°C / second or the rapid cooling termination temperature exceeds 150°C, the martensitic phase transformation cannot proceed sufficiently, thus making it difficult to ensure the fine microstructure desired by this invention. The rapid cooling rate is more preferably 50°C / second or higher, more preferably 60°C / second or higher, and most preferably 70°C / second or higher. The rapid cooling termination temperature is more preferably below 140°C, and more preferably below 130°C.

[0062] Subsequently, the rapidly cooled cold-rolled steel sheet is reheated and over-aged at 180-240°C. This reheating and over-aging heat treatment transforms the martensite obtained through the rapid cooling process into tempered martensite. When the reheating and over-aging heat treatment temperature is below 180°C, tempering is insufficient, resulting in low yield strength and insufficient toughness. When the reheating and over-aging heat treatment temperature exceeds 240°C, the large precipitation and coarsening of carbides leads to poor bending workability. The lower limit of the reheating and over-aging heat treatment temperature is more preferably 190°C, and even more preferably 200°C. The upper limit of the reheating and over-aging heat treatment temperature is more preferably 230°C, and even more preferably 220°C. Furthermore, the over-aging heat treatment can last for more than 400 seconds. When the over-aging heat treatment time is less than 400 seconds, tempering is insufficient, resulting in low yield strength. Furthermore, in this invention, the over-aging heat treatment time is not particularly limited, but due to the characteristics of continuous annealing equipment, it is difficult to exceed 1000 seconds. The lower limit of the over-aging heat treatment time is more preferably 500 seconds, and even more preferably 600 seconds. Detailed Implementation

[0063] The present invention will now be described in more detail through embodiments. However, these embodiments are merely illustrative of implementation of the invention, and the invention is not limited to these embodiments. This is because the scope of the invention is determined by the contents of the claims and the contents reasonably deduced therefrom.

[0064] (Example)

[0065] Molten steel with the alloy composition described in Table 1 is cast into ingots, which are then rolled to produce billets. These billets are heated to 1200°C and held for 1 hour, then hot-rolled at 900°C and placed in a furnace preheated to 550°C and held for 1 hour, followed by furnace cooling to simulate hot-rolled coiling. The hot-rolled steel sheet is pickled, then cold-rolled with a 50% cold-rolling reduction, and then subjected to annealing, slow cooling, rapid cooling, reheating, and over-aging heat treatment under the conditions described in Table 2 to produce cold-rolled steel sheets.

[0066] The microstructure and mechanical-physical properties of the cold-rolled steel sheet manufactured as described above were measured and are shown in Table 3 below.

[0067] At this point, fine tissue is measured using an optical microscope, and the relationship is established using [Equation 1] Fm=(Fk×10 6 ) / ((0.67n+z)×V 2The average grain size of the original austenite was measured. In Equation 1, Fm represents the average grain size of the original austenite, Fk represents the total area of ​​the microstructure photograph, z represents the number of grains contained within the circle, n represents the number of grains spanning the circle, and V represents the magnification when measuring the microstructure. When measuring the average grain size of the original austenite, a circle with a diameter of 140 μm was drawn on a microstructure photograph measured using a 1000x optical microscope for measurement.

[0068] Additionally, regarding F HAGB and L HAGB Fine tissue was measured using electron backscatter diffraction (EBSD) over a measurement area of ​​45 μm × 45 μm and a measurement interval of 0.75 μm, and then analyzed using TSL-OIM software with a threshold of 15°.

[0069] Tensile strength (TS) and yield strength (YS) are measured by performing a tensile test at a strain rate of 0.01 / s after cutting a JIS 5 size tensile test piece in a direction perpendicular to the rolling direction.

[0070] Hole expansion ratio (HER) was measured according to ISO 16630 standard. The specimen size was 120mm × 120mm, and the initial hole diameter was 10mm according to the 12% clearance standard. The stamping holding load was 20 tons, and the test speed was 12mm / minute.

[0071] For R / t (bending characteristics), cold-rolled steel sheets are processed into specimens with a width of 100 mm and a length of 30 mm. Then, a 90° bending test is performed at a test speed of 100 mm / min. Cracks in the bent part are then confirmed using a microscope. The R / t value is obtained by dividing the minimum bending radius (R) that does not produce cracks by the thickness (t) of the specimen.

[0072] [Table 1]

[0073]

[0074] [Table 2]

[0075]

[0076]

[0077] [Table 3]

[0078]

[0079]

[0080] As can be seen from Tables 1 to 3, in the cases of Invention Examples 1 to 8, which meet the conditions of the present invention, excellent tensile strength and tensile strength × porosity values ​​are observed. On the other hand, in the cases of Comparative Examples 1 to 12, it is evident that since the conditions of the present invention are not met, the tensile strength or tensile strength × porosity values ​​desired by the present invention cannot be guaranteed.

[0081] Figure 1 These are photographs of Invention Example 5 and Comparative Example 5 observed using an optical microscope. Figure 1 It can be seen that in the case of Invention Example 5, the average particle size of the original austenite is fine, while in the case of Comparative Example 5, it can be seen that the average particle size of the original austenite is relatively large.

[0082] Figure 2 These are photographs of large-angle and small-angle grain boundaries after measuring the fine structure of Invention Example 5 and Comparative Example 5 using electron backscatter diffraction measurement attached to a scanning electron microscope. Figure 2 It can be seen that, in the case of invention example 5, F HAGB and L HAGB It has a high value; on the other hand, in the case of Comparative Example 5, it can be seen that F HAGB and L HAGB The value is low.

Claims

1. A high-strength cold-rolled steel sheet with excellent hole expansion properties, comprising, by weight%,: C: 0.2-0.4%, Si: less than 0.5% and excluding 0%, Mn: 1.0-2.0%, P: less than 0.03% and excluding 0%, S: less than 0.015% and excluding 0%, Al: less than 0.1% and excluding 0%, Cr: less than 0.5% and excluding 0%, Mo: less than 0.2% and excluding 0%, Ti: less than 0.1% and excluding 0%, Nb: less than 0.1% and excluding 0%, B: less than 0.005% and excluding 0%, N: less than 0.01% and excluding 0%, with the balance being Fe and other unavoidable impurities. The microstructure of the cold-rolled steel sheet consists of a single-phase tempered martensite structure or a mixed structure of martensite and tempered martensite. The fine tissue has an F density of 45μm × 45μm per unit area. HAGB For more than 60% of the area, L HAGB 8mm or more wherein The F HAGB represents a fraction of grains having large-angle grain boundaries, L HAGB represents the total length of grain boundaries having large-angle grain boundaries, the large-angle grain boundaries referring to grain boundaries between adjacent grains having a misorientation angle of 15° or more.

2. The ultra-high strength cold-rolled steel sheet with excellent hole expandability according to claim 1, wherein, The cold-rolled steel sheet further comprises one or more of Cu and Ni, less than 0.5%.

3. The ultra-high strength cold-rolled steel sheet with excellent hole expandability according to claim 1, wherein, The cold-rolled steel sheet further contains less than 0.05% Sb.

4. The ultra-high-strength cold-rolled steel sheet with excellent hole expansionability according to claim 1, wherein The average grain size of the original austenite in the cold-rolled steel sheet is less than 6 μm.

5. The ultra-high strength cold-rolled steel sheet with excellent hole expandability according to claim 1, wherein, The tensile strength TS of the cold-rolled steel sheet is above 1470MPa, and the value of tensile strength TS × hole expansion ratio HER is above 73500MPa·% (where tensile strength is in MPa and hole expansion ratio is in 0.5%).

6. A method for manufacturing ultra-high strength cold-rolled steel sheets with excellent hole expansion properties, comprising the following steps: The steel billet is heated to a temperature of 1100-1300℃, and the steel billet contains, by weight%,: C: 0.2-0.4%, Si: less than 0.5% and excluding 0%, Mn: 1.0-2.0%, P: less than 0.03% and excluding 0%, S: less than 0.015% and excluding 0%, Al: less than 0.1% and excluding 0%, Cr: less than 0.5% and excluding 0%, Mo: less than 0.2% and excluding 0%, Ti: less than 0.1% and excluding 0%, Nb: less than 0.1% and excluding 0%, B: less than 0.005% and excluding 0%, N: less than 0.01% and excluding 0%, the balance being Fe and other unavoidable impurities; The heated steel billet is hot-finished at a temperature above Ar3 to obtain hot-rolled steel sheet; The hot-rolled steel sheet is coiled at a temperature below 720°C; The hot-rolled steel sheet that has been coiled is cold-rolled to obtain a cold-rolled steel sheet; The cold-rolled steel sheet is subjected to annealing heat treatment in a temperature range of 780-900℃; The cold-rolled steel sheet that has undergone the annealing heat treatment is slowly cooled at a cooling rate of less than 5°C / second to 650-750°C. The cold-rolled steel sheet, which had been slowly cooled, was rapidly cooled at a rate of 40-47°C / second until it reached below 150°C; and The rapidly cooled cold-rolled steel sheet is then reheated and subjected to over-aging heat treatment at 180-240°C.

7. The method of manufacturing an ultra-high strength cold-rolled steel sheet with excellent hole expandability according to claim 6, wherein, The billet further comprises less than 0.5% Cu and less than 0.5% Ni.

8. The method of manufacturing an ultra-high-strength cold-rolled steel sheet with excellent hole expandability according to claim 6, wherein The billet further contains less than 0.05% Sb.

9. The method of manufacturing an ultra-high strength cold-rolled steel sheet with excellent hole expandability according to claim 6, wherein, The over-aging heat treatment is performed for more than 400 seconds.

Citation Information

Patent Citations

  • High-strength galvanized steel sheet and its manufacturing method

    JP6323617B1

  • Cold rolled steel sheet with ultra-high strength, and manufacturing method therefor

    WO2021117989A1