A self-lithium-supplemented cathode material, its preparation method, and its application.

By coating the core surface of the lithium battery cathode material with LiM alloy, self-lithiation is achieved, solving the problem of lithium loss in the first cycle of lithium battery, improving charging capacity and cycle performance, and making it suitable for mass production.

CN117996031BActive Publication Date: 2026-11-17SVOLT ENERGY TECHNOLOGY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410162582.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-05
Publication Date
2026-11-17
Estimated Expiration
2044-02-05

AI Technical Summary

Technical Problem

Existing lithium battery cathode materials suffer significant lithium loss during the first charge cycle due to the formation of the SEI film, resulting in a lower discharge capacity than the charging capacity. Furthermore, common lithium replenishing agents generate gas during charging and have poor processing performance.

Method used

By coating the surface of the LiNiM core in the cathode material with LiM alloy, self-lithiation is achieved, which compensates for the Li+ consumed by the formation of the SEI film in the anode, thereby improving the charging capacity and cycle performance.

Benefits of technology

It significantly improves the charging capacity and cycle performance of the cathode material, enhances the electrochemical performance of lithium batteries, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004698858870000131
    Figure BDA0004698858870000131
Patent Text Reader

Abstract

This invention discloses a self-lithiated cathode material, its preparation method, and its applications. The self-lithiated cathode material includes a cathode material core and a shell covering the surface of the cathode material core. The cathode material core has the chemical formula LiNiM, and the shell comprises a LiM alloy material, wherein M is at least one of Mn, Al, Fe, or Zr. Compared with conventional cathode materials, the self-lithiated cathode material of this invention has higher specific capacity and better long-cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of cathode materials for batteries, specifically relating to a self-lithium-replenishing cathode material, its preparation method, and its application. Background Technology

[0002] With the rapid development of new energy vehicles and the continuous expansion of the market, the demand for lithium batteries is constantly increasing. At the same time, people's requirements for lithium batteries are also getting higher and higher, and high-capacity, long-cycle batteries are becoming more and more popular.

[0003] Layered binary materials like LiNiM (where M is Mn, Al, Fe, or Zr) possess high specific capacity and reversible specific capacity. However, during the first charging cycle, the formation of an SEI film leads to a significant loss of active lithium, resulting in a lower discharge capacity than charge capacity and leaving some cathode material idle. Lithium replenishment agents can release a large number of lithium ions during the first charging cycle, preventing lithium loss from the cathode material and thus improving the cathode capacity.

[0004] Currently, common cathode lithium replenishers include inorganic lithium replenishers (including lithium silicate lithium replenishers and halogen lithium replenishers), cathode-like compound lithium replenishers (including Li5FeO4 and Li2NiO2), and organic lithium compound lithium replenishers (including Li2C4O4 and Li4C4O4). These lithium replenishers can improve battery capacity to some extent; however, they generate gas during charging and have poor processing performance.

[0005] Therefore, designing a cathode material that produces no gas and has excellent processing performance is of great significance. Summary of the Invention

[0006] To address the aforementioned problems in existing technologies, the present invention aims to provide a self-lithiated cathode material, its preparation method, and its applications. This invention achieves self-lithiation of the cathode material by coating the surface of the LiNiM core with a LiM alloy. This self-lithiation technology can compensate for the Li consumed in the formation of the SEI film on the anode. + This can significantly improve the charging capacity of the cathode material and enhance its cycle performance.

[0007] To achieve the above objectives, the present invention adopts the following technical solution:

[0008] In a first aspect, the present invention provides a self-lithiated cathode material, the self-lithiated cathode material comprising a binary cathode material core and a shell covering the surface of the cathode material core, the cathode material core having the chemical formula LiNiM, and the shell comprising a LiM alloy material, wherein M is at least one of Mn, Al, Fe or Zr.

[0009] This invention achieves self-lithiation of the cathode material by coating the surface of the LiNiM core with a LiM alloy. This self-lithiation technology can compensate for the Li consumed in the formation of the SEI film on the anode. + This can significantly improve the charging capacity of the cathode material and enhance its cycle performance.

[0010] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. The technical objectives and beneficial effects of the present invention can be better achieved and realized through the following preferred technical solutions.

[0011] Preferably, the chemical formula of the self-lithiated cathode material is xLiNiM·yLiM, where x+y=1, and 0.03≤y≤0.05. For example, y can be 0.03, 0.032, 0.035, 0.037, 0.04, 0.041, 0.043, 0.045, 0.047, or 0.05, etc.

[0012] Preferably, the particle size of the cathode material core is in the range of 30 μm to 40 μm, and the particle size can be, for example, 30 μm, 31 μm, 32 μm, 33 μm, 34 μm, 35 μm, 36 μm, 37 μm, 38 μm, 39 μm, or 40 μm; the particle size of the LiM alloy material is in the range of 1 μm to 5 μm, and the particle size can be, for example, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, or 5 μm. Within the above-mentioned particle size range, a better coating effect can be obtained.

[0013] Preferably, in the cathode material core, the molar ratio of Li to the total molar sum of Ni and M is 1 to 1.05, for example, 1, 1.10, 1.02, 1.03, 1.04, or 1.05. This ratio can be simplified as Li / (Ni+M), that is, Li / (Ni+M) = 1 to 1.05.

[0014] Preferably, in the LiM alloy material, the molar ratio of Li to M is 0.01 to 10, for example, 0.01, 0.05, 0.1, 0.2, 0.3, 0.5, 0.7, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5 or 10, etc.

[0015] In a second aspect, the present invention provides a method for preparing a self-lithium-supplemented cathode material as described in the first aspect, the method comprising the following steps:

[0016] (1) Provide cathode material core and LiM alloy material;

[0017] (2) Add the cathode material core to the solution of the modifier, so that the modifier is adsorbed on the surface of the cathode material core, and obtain a surface-modified cathode material core;

[0018] (3) The surface-modified cathode material core and the LiM alloy material are dispersed in a solvent, so that the LiM alloy material is adsorbed onto the surface of the cathode material core to obtain the cathode material.

[0019] The preparation method of this invention is simple, and the prepared cathode material has good electrochemical performance, making it suitable for large-scale production.

[0020] Preferably, the positive electrode material core in step (1) has the chemical formula LiNiM, where M is at least one of Mn, Al, Fe, or Zr. The positive electrode material core is prepared by mixing a precursor prepared by hydrothermal method with a lithium salt and then sintering. The present invention does not specifically limit the equipment used for sintering; for example, it can be a muffle furnace.

[0021] By using a hydrothermal method to prepare the precursor and then preparing the cathode material core, the cathode material can achieve a uniform particle size distribution, good sphericity, and denser particle packing.

[0022] Preferably, the hydrothermal preparation of the precursor includes the following steps:

[0023] Salts of various metal elements in the precursor are dissolved in a solvent, a complexing agent and a precipitating agent are added, the mixture is stirred and placed in a reaction vessel, and heated in an oil bath to achieve a hydrothermal reaction to obtain the precursor.

[0024] Optionally, after the hydrothermal reaction is complete, centrifugation, solid phase collection, washing, and drying are performed.

[0025] Preferably, the preparation method of the LiM alloy material in step (1) is a high-temperature alloying method, which includes the following steps: mixing and grinding Li and M, and calcining at high temperature under an inert atmosphere to obtain the LiM alloy material. The present invention does not specifically limit the equipment used for high-temperature calcination; for example, it can be a tube furnace.

[0026] Optionally, after high-temperature calcination, the product from high-temperature calcination is thoroughly ground to obtain LiM alloy material powder.

[0027] Preferably, the gas in the inert atmosphere includes at least one of N2, Ar, and He.

[0028] Preferably, the high-temperature calcination temperature is 800℃~1000℃, for example, it can be 800℃, 825℃, 850℃, 870℃, 880℃, 900℃, 925℃, 950℃, 960℃, 980℃ or 1000℃, etc.; the high-temperature calcination time is 10h~12h, for example, 10h, 10.5h, 11h, 11.5h or 12h, etc.

[0029] Preferably, the solution of the modifier in step (2) is an aqueous solution of polyvinylpyrrolidone.

[0030] Preferably, the mass fraction of the modifier solution is 5% to 10%, for example, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9% or 10%.

[0031] Preferably, in step (2), after adding the cathode material core to the solution of the modifier, the mixture is stirred. Stirring allows the modifier to be more fully adsorbed onto the surface of the cathode material core.

[0032] Optionally, in step (2), after adsorption, the solution containing the cathode material core is separated and dried to obtain a surface-modified cathode material core. The separation method can be vacuum filtration.

[0033] The present invention does not specifically limit the solvent used in step (3), for example, it can be NMP.

[0034] Preferably, the dispersion method in step (3) is ultrasound.

[0035] Thirdly, the present invention provides a positive electrode comprising the self-lithiated positive electrode material as described in the first aspect.

[0036] Preferably, the positive electrode further includes a conductive agent and a binder.

[0037] The present invention does not specifically limit the type of conductive agent; for example, it can be Super P.

[0038] The present invention does not specifically limit the type of adhesive, for example, it can be PVDF.

[0039] Fourthly, the present invention provides a lithium-ion battery, comprising a positive electrode, a negative electrode, a separator, and an electrolyte, wherein the positive electrode is the positive electrode described in the third aspect.

[0040] The numerical range described in this invention includes not only the points listed above, but also any points within the ranges not listed above. Due to space limitations and for the sake of brevity, this invention will not exhaustively list all the specific points included in the range. Compared with existing technologies, this invention has the following beneficial effects:

[0041] (1) This invention achieves self-lithiation of the cathode material by coating the surface of the LiNiM core with LiM alloy. This self-lithiation technology can compensate for the Li consumed by the formation of the SEI film in the anode. + This invention can significantly improve the charging specific capacity of cathode materials and enhance their cycle performance. Compared with conventional cathode materials, the self-compensated lithium-ion cathode material of this invention has higher specific capacity and better long-cycle performance.

[0042] (2) The preparation method of the present invention is simple, and the prepared cathode material has good electrochemical performance and is suitable for large-scale production. Detailed Implementation

[0043] The technical solution of the present invention will be further illustrated below through specific embodiments.

[0044] Example 1

[0045] This embodiment provides a self-lithiated cathode material, comprising a binary cathode material core and a shell covering the surface of the binary cathode material core. The chemical formula of the binary cathode material core is LiNiAl, the chemical formula of the shell is Li2Al, the chemical formula of the self-lithiated cathode material is 0.96LiNiAl·0.04Li2Al, the particle size of the cathode material core is in the range of 30μm to 40μm, and the particle size of the LiM alloy material is in the range of 1μm to 5μm.

[0046] The self-lithiated cathode material provided in this embodiment includes the following steps:

[0047] The high-temperature alloying method for synthesizing Li2Al includes the following steps: 2 mol of lithium and 1 mol of aluminum are mixed and ground, and then calcined at 900℃ for 10 h under an Ar atmosphere to obtain Li2Al alloy.

[0048] 1 mol of nickel sulfate and 1 mol of aluminum sulfate were dissolved in deionized water. Ammonia complexing agent and sodium hydroxide precipitant were added. After thorough stirring, the mixture was placed in a polytetrafluoroethylene reactor and heated in an oil bath. After the reaction was completed, the mixture was centrifuged, the solid phase was collected, washed, and dried to obtain the precursor NiAl. The precursor was mixed with lithium hydroxide at a molar ratio of 1:1.05 and sintered in a muffle furnace to obtain the LiNiAl binary cathode material.

[0049] 7g of polyvinylpyrrolidone (PVP) was dissolved in 93g of deionized water to prepare a 7% solution. LiNiAl binary cathode material was added, and the mixture was stirred thoroughly to allow PVP to be fully adsorbed onto the surface of LiNiAl particles. Stirring was stopped, the upper liquid was vacuum filtered, and the mixture was dried to obtain surface-modified LiNiAl particles. The surface-modified LiNiAl particles were then dissolved in NMP to disperse them fully. Li2Al alloy powder was added and ultrasonically dispersed to allow Li2Al to be fully adsorbed onto the surface of the LiNiAl particles. After drying, a bilayer cathode material with a LiNiAl core and a Li2Al coating was obtained, which is a self-lithium-added cathode material.

[0050] Example 2

[0051] This embodiment provides a self-lithiated cathode material, comprising a binary cathode material core and a shell covering the surface of the binary cathode material core. The chemical formula of the binary cathode material core is LiNiZr, the chemical formula of the shell is LiZr, the chemical formula of the self-lithiated cathode material is 0.97LiNiZr·0.03LiZr, the particle size of the cathode material core is in the range of 30μm to 40μm, and the particle size of the LiM alloy material is in the range of 1μm to 5μm.

[0052] The method for preparing the self-lithiated cathode material provided in this embodiment includes the following steps:

[0053] The high-temperature alloying method for synthesizing LiZr includes the following steps: 1 mol of lithium and 1 mol of zirconium are mixed and ground, and then calcined at 800℃ for 9 hours under N2 atmosphere to obtain LiZr alloy.

[0054] 1 mol of nickel sulfate and 1 mol of zirconium sulfate were dissolved in deionized water, and ammonia complexing agent and sodium hydroxide precipitant were added. After thorough stirring, the mixture was placed in a polytetrafluoroethylene reactor and heated in an oil bath. After the reaction was completed, the mixture was centrifuged, the solid phase was collected, washed, and dried to obtain the precursor NiZr. The precursor was mixed with lithium hydroxide at a molar ratio of 1:1.05 and sintered in a muffle furnace to obtain the LiNiZr binary cathode material.

[0055] 5g of polyvinylpyrrolidone (PVP) was dissolved in 95g of deionized water to obtain a 5% (w / w) solution. LiNiZr cathode material was added, and the mixture was stirred thoroughly to allow PVP to be fully adsorbed onto the surface of the LiNiZr particles. Stirring was stopped, and the upper liquid was vacuum filtered and dried to obtain surface-modified LiNiZr particles. The surface-modified LiNiZr particles were then dissolved in NMP to disperse them fully. LiZr alloy powder was added, and the mixture was ultrasonically dispersed to allow LiZr to be fully adsorbed onto the surface of the LiNiZr particles. After drying, a bilayer cathode material with a LiNiZr core and a LiZr coating was obtained, which is a self-lithiated cathode material.

[0056] Example 3

[0057] This embodiment provides a self-lithiated cathode material, comprising a binary cathode material core and a shell covering the surface of the binary cathode material core. The chemical formula of the binary cathode material core is LiNiFe, the chemical formula of the shell is Li3Fe, the chemical formula of the self-lithiated cathode material is 0.95LiNiFe·0.05Li3Fe, the particle size of the cathode material core is in the range of 30μm to 40μm, and the particle size of the LiM alloy material is in the range of 1μm to 5μm.

[0058] The preparation method of the self-lithiated cathode material provided in this embodiment includes the following steps: synthesizing Li3Fe by high-temperature alloying, specifically including the following steps: mixing and grinding 3 mol of lithium and 1 mol of iron, and calcining at 1000℃ for 8 hours under He atmosphere to obtain Li3Fe alloy.

[0059] 1 mol of nickel sulfate and 1 mol of ferrous sulfate were dissolved in deionized water. Ammonia complexing agent and sodium hydroxide precipitant were added, and the mixture was stirred thoroughly before being placed in a polytetrafluoroethylene reactor. The reactor was heated in an oil bath. After the reaction was completed, the mixture was centrifuged, the solid phase was collected, washed, and dried to obtain the precursor NiFe. The precursor was mixed with lithium hydroxide at a molar ratio of 1:1.05 and sintered in a muffle furnace to obtain the LiNiFe binary cathode material.

[0060] 6g of polyvinylpyrrolidone (PVP) was dissolved in 94g of deionized water to prepare a 6% (w / w) solution. LiNiFe cathode material was added, and the mixture was stirred thoroughly to allow PVP to be fully adsorbed onto the surface of the LiNiFe particles. Stirring was stopped, and the upper liquid was vacuum filtered and dried to obtain surface-modified LiNiFe particles. The surface-modified LiNiFe particles were then dissolved in NMP to disperse them fully. Li3Fe alloy powder was added and ultrasonically dispersed to allow Li3Fe to be fully adsorbed onto the surface of the LiNiFe particles. After drying, a bilayer cathode material with a LiNiFe core and a Li3Fe coating was obtained, which is a self-lithiated cathode material.

[0061] Example 4

[0062] This embodiment provides a self-lithiated cathode material, comprising a binary cathode material core and a shell covering the surface of the binary cathode material core. The chemical formula of the binary cathode material core is LiNiMn, the chemical formula of the shell is LiMn3, the chemical formula of the self-lithiated cathode material is 0.97LiNiMn·0.03LiMn3, the particle size of the cathode material core is in the range of 30μm to 40μm, and the particle size of the LiM alloy material is in the range of 1μm to 5μm.

[0063] The self-lithiated cathode material provided in this embodiment includes the following steps:

[0064] The high-temperature alloying method for synthesizing LiMn3 includes the following steps: 1 mol of lithium and 3 mol of manganese are mixed and ground, and then calcined at 900℃ for 10 h under an Ar atmosphere to obtain a LiMn3 alloy.

[0065] 1 mol of nickel sulfate and 1 mol of manganese sulfate were dissolved in deionized water, and ammonia complexing agent and sodium hydroxide precipitant were added. After thorough stirring, the mixture was placed in a polytetrafluoroethylene reactor and heated in an oil bath. After the reaction was completed, the mixture was centrifuged, the solid phase was collected, washed, and dried to obtain the precursor NiMn. The precursor was mixed with lithium hydroxide at a molar ratio of 1:1.05 and sintered in a muffle furnace to obtain the LiNiMn binary cathode material.

[0066] 8g of polyvinylpyrrolidone was dissolved in 92g of deionized water to prepare an 8% (w / w) solution. LiNiMn cathode material was added, and the mixture was stirred thoroughly to allow PVP to be fully adsorbed onto the surface of LiNiFe particles. Stirring was stopped, and the upper liquid was vacuum filtered and dried to obtain surface-modified LiNiMn particles. The surface-modified LiNiMn particles were then dissolved in NMP to disperse them fully. LiMn3 alloy powder was added and ultrasonically dispersed to allow LiMn3 to be fully adsorbed onto the surface of the LiNiMn particles. After drying, a bilayer cathode material with a LiNiMn core and a LiMn3 coating was obtained, which is a self-lithiated cathode material.

[0067] Example 5

[0068] This embodiment provides a self-lithiated cathode material, comprising a binary cathode material core and a shell covering the surface of the binary cathode material core. The chemical formula of the binary cathode material core is LiNiAl, the chemical formula of the shell is Li2Al3, the chemical formula of the self-lithiated cathode material is 0.96LiNiAl·0.04Li2Al3, the particle size of the cathode material core is in the range of 30μm to 40μm, and the particle size of the LiM alloy material is in the range of 1μm to 5μm.

[0069] The self-lithiated cathode material provided in this embodiment includes the following steps:

[0070] The high-temperature alloying method for synthesizing Li2Al3 includes the following steps: 2 mol of lithium and 3 mol of aluminum are mixed and ground, and then calcined at 1000℃ for 8 hours under a He atmosphere to obtain a Li2Al3 alloy.

[0071] 1 mol of nickel sulfate and 1 mol of aluminum sulfate were dissolved in deionized water. Ammonia complexing agent and sodium hydroxide precipitant were added. After thorough stirring, the mixture was placed in a polytetrafluoroethylene reactor and heated in an oil bath. After the reaction was completed, the mixture was centrifuged, the solid phase was collected, washed, and dried to obtain the precursor NiAl. The precursor was mixed with lithium hydroxide at a molar ratio of 1:1.05 and sintered in a muffle furnace to obtain the LiNiAl binary cathode material.

[0072] 9g of polyvinylpyrrolidone was dissolved in 91g of deionized water to prepare a 9% (w / w) solution. LiNiAl cathode material was added, and the mixture was stirred thoroughly to allow PVP to be fully adsorbed onto the surface of the LiNiAl particles. Stirring was stopped, and the upper liquid was vacuum filtered and dried to obtain surface-modified LiNiAl particles. The surface-modified LiNiAl particles were then dissolved in NMP to disperse them fully. Li2Al3 alloy powder was added and ultrasonically dispersed to allow Li2Al to be fully adsorbed onto the surface of the LiNiAl particles. After drying, a bilayer cathode material with a LiNiAl core and a Li2Al3 coating was obtained, which is a self-lithiated cathode material.

[0073] Example 6

[0074] This embodiment provides a self-lithiated cathode material, which differs from Embodiment 1 in that the chemical formula of the self-lithiated cathode material is 0.98LiNiAl·0.02Li2Al.

[0075] 1 mol of nickel sulfate and 1 mol of aluminum sulfate were dissolved in deionized water. Ammonia complexing agent and sodium hydroxide precipitant were added. After thorough stirring, the mixture was placed in a polytetrafluoroethylene reactor and heated in an oil bath. After the reaction was completed, the mixture was centrifuged, the solid phase was collected, washed, and dried to obtain the precursor NiAl. The precursor was mixed with lithium hydroxide at a molar ratio of 1:1.05 and sintered in a muffle furnace to obtain the LiNiAl binary cathode material.

[0076] 10g of polyvinylpyrrolidone (PVP) was dissolved in 90g of deionized water to prepare a 10% solution. LiNiAl binary cathode material was added, and the mixture was stirred thoroughly to allow PVP to be fully adsorbed onto the surface of LiNiAl particles. Stirring was stopped, and the upper liquid was vacuum filtered and dried to obtain surface-modified LiNiAl particles. The surface-modified LiNiAl particles were then dissolved in NMP to disperse them fully. Li2Al alloy powder was added and ultrasonically dispersed to allow Li2Al to be fully adsorbed onto the surface of LiNiAl particles. After drying, a bilayer cathode material with a LiNiAl core and a Li2Al coating was obtained, which is a self-lithiated cathode material.

[0077] Example 7

[0078] This embodiment provides a self-lithiated cathode material, which differs from Embodiment 1 in that the chemical formula of the self-lithiated cathode material is 0.94LiNiAl·0.06Li2Al.

[0079] 1 mol of nickel sulfate and 1 mol of aluminum sulfate were dissolved in deionized water. Ammonia complexing agent and sodium hydroxide precipitant were added. After thorough stirring, the mixture was placed in a polytetrafluoroethylene reactor and heated in an oil bath. After the reaction was completed, the mixture was centrifuged, the solid phase was collected, washed, and dried to obtain the precursor NiAl. The precursor was mixed with lithium hydroxide at a molar ratio of 1:1.05 and sintered in a muffle furnace to obtain the LiNiAl binary cathode material.

[0080] 7g of polyvinylpyrrolidone (PVP) was dissolved in 93g of deionized water to prepare a 7% (w / w) solution. LiNiAl binary cathode material was added, and the mixture was stirred thoroughly to allow PVP to be fully adsorbed onto the surface of the LiNiAl particles. Stirring was stopped, and the upper liquid was vacuum filtered and dried to obtain surface-modified LiNiAl particles. The surface-modified LiNiAl particles were then dissolved in NMP to disperse them fully. Li2Al alloy powder was added and ultrasonically dispersed to allow Li2Al to be fully adsorbed onto the surface of the LiNiAl particles. After drying, a bilayer cathode material with a LiNiAl core and a Li2Al coating was obtained, which is a self-lithiated cathode material.

[0081] Example 8

[0082] This embodiment provides a self-compensating lithium cathode material, which differs from Embodiment 1 in that the core particle size of the cathode material is in the range of 30μm to 40μm, and the particle size of the LiM alloy material is in the range of 8μm to 10μm.

[0083] 1 mol of nickel sulfate and 1 mol of aluminum sulfate were dissolved in deionized water. Ammonia complexing agent and sodium hydroxide precipitant were added. After thorough stirring, the mixture was placed in a polytetrafluoroethylene reactor and heated in an oil bath. After the reaction was completed, the mixture was centrifuged, the solid phase was collected, washed, and dried to obtain the precursor NiAl. The precursor was mixed with lithium hydroxide at a molar ratio of 1:1.05 and sintered in a muffle furnace to obtain the LiNiAl binary cathode material.

[0084] 6g of polyvinylpyrrolidone (PVP) was dissolved in 94g of deionized water to prepare a 6% (w / w) solution. LiNiAl binary cathode material was added, and the mixture was stirred thoroughly to allow PVP to be fully adsorbed onto the surface of LiNiAl particles. Stirring was stopped, the upper liquid was vacuum filtered, and the mixture was dried to obtain surface-modified LiNiAl particles. The surface-modified LiNiAl particles were then dissolved in NMP to disperse them fully. Li2Al alloy powder was added, and the mixture was ultrasonically dispersed to allow Li2Al to be fully adsorbed onto the surface of the LiNiAl particles. After drying, a bilayer cathode material with a LiNiAl core and a Li2Al coating was obtained, which is a self-lithiated cathode material.

[0085] Example 9

[0086] This embodiment provides a self-compensating lithium cathode material. The difference between its preparation method and that of Example 1 is that polyvinylpyrrolidone was not used to modify the LiNiAl particles.

[0087] 1 mol of nickel sulfate and 1 mol of aluminum sulfate were dissolved in deionized water. Ammonia complexing agent and sodium hydroxide precipitant were added. After thorough stirring, the mixture was placed in a polytetrafluoroethylene reactor and heated in an oil bath. After the reaction was completed, the mixture was centrifuged, the solid phase was collected, washed, and dried to obtain the precursor NiAl. The precursor was mixed with lithium hydroxide at a molar ratio of 1:1.05 and sintered in a muffle furnace to obtain the LiNiAl binary cathode material.

[0088] The LiNiAl binary cathode material is thoroughly mixed and stirred with Li2Al alloy powder to obtain a bilayer cathode material with a LiNiAl core and a Li2Al coating on the surface, which is also a self-lithiated cathode material.

[0089] Comparative Example 1

[0090] This comparative example provides a binary cathode material, the preparation method of which includes the following steps:

[0091] 1 mol of nickel sulfate and 1 mol of aluminum sulfate were dissolved in deionized water. Ammonia complexing agent and sodium hydroxide precipitant were added. After thorough stirring, the mixture was placed in a polytetrafluoroethylene reactor and heated in an oil bath. After the reaction was completed, the mixture was centrifuged, the solid phase was collected, washed, and dried to obtain the precursor NiAl. The precursor was mixed with lithium hydroxide at a molar ratio of 1:1.05 and sintered in a muffle furnace to obtain the LiNiAl binary cathode material.

[0092] Battery fabrication and performance testing:

[0093] (I) Battery fabrication:

[0094] Take an appropriate amount of the positive electrode material from Examples 1 to 9 and Comparative Example 1, mix it with conductive carbon black and polyvinylidene fluoride adhesive (solid content 6.05%), and homogenize it according to the ratio of positive electrode material: conductive carbon black: polyvinylidene fluoride adhesive (mass ratio) = 92:4:4. Coat the homogenate onto aluminum foil to prepare a positive electrode sheet.

[0095] The above-mentioned positive electrode, separator, and lithium sheet are assembled into a cell. After electrolyte injection, the cells are assembled into a coin cell using a BR2032 casing to obtain a battery.

[0096] (II) Performance Testing:

[0097] Electrochemical tests were performed on a battery performance testing system, with a test voltage range of 3.0V to 4.3V. The batteries were subjected to charge-discharge cycle tests at a discharge efficiency of 0.2C, followed by two weeks of cycles, and then 500 cycles at 2C. The average value of each group was taken. The test results for the average initial discharge specific capacity and the room temperature cycle retention rate (i.e., 500-cycle retention rate) are shown in Table 1.

[0098] Table 1

[0099]

[0100] As shown in Table 1, the bilayer core-shell cathode materials prepared in Examples 1-9 exhibit superior electrochemical performance compared to Comparative Example 1. Specifically, the material prepared under the specific synthesis conditions in Example 1 demonstrates superior electrochemical performance compared to materials prepared under other conditions.

[0101] A comparison of Example 1 with Examples 6-8 shows that the self-lithiated cathode material prepared with a double-layer core-shell structure can exhibit superior performance under suitable processing conditions and material ratios.

[0102] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.

[0103] The applicant declares that the detailed method of the present invention is illustrated by the above embodiments, but the present invention is not limited to the above detailed method, that is, it does not mean that the present invention must rely on the above detailed method to be implemented. Those skilled in the art should understand that any improvements to the present invention, equivalent substitutions of the raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A self-lithium-replenishing cathode material, characterized in that, The self-supplementing lithium-ion cathode material includes a cathode material core and a shell covering the surface of the cathode material core. The cathode material core has the chemical formula LiNiM, and the shell includes a LiM alloy material, wherein M is at least one of Mn, Al, Fe, or Zr. The cathode material core is surface-modified, and the surface-modifying agent is polyvinylpyrrolidone. The cathode material core is prepared by mixing a precursor prepared by hydrothermal method with a lithium salt and sintering. The hydrothermal method for preparing the precursor includes dissolving the salts of each metal element in the precursor in a solvent, adding a complexing agent and a precipitating agent, stirring, placing it in a reaction vessel, and heating it in an oil bath to achieve a hydrothermal reaction to obtain the precursor.

2. The self-lithiated cathode material according to claim 1, characterized in that, The chemical formula of the self-lithiated cathode material is xLiNiM·yLiM, where x+y=1 and 0.03≤y≤0.

05.

3. The self-lithiated cathode material according to claim 1 or 2, characterized in that, The particle size of the cathode material core is in the range of 30µm to 40µm, and the particle size of the LiM alloy material is in the range of 1µm to 5µm.

4. The self-lithiated cathode material according to claim 1 or 2, characterized in that, In the cathode material core, the molar ratio of Li to the total molar sum of metallic Ni and M is 1 to 1.

05.

5. The self-lithiated cathode material according to claim 4, characterized in that, In the LiM alloy material, the molar ratio of Li to M is 0.01~10.

6. A method for preparing a self-lithiated cathode material as described in any one of claims 1-5, characterized in that, The preparation method includes the following steps: (1) Provide the cathode material core and LiM alloy material; (2) Add the cathode material core to the solution of the modifier, so that the modifier is adsorbed on the surface of the cathode material core, and obtain a surface-modified cathode material core; (3) The surface-modified cathode material core and the LiM alloy material are dispersed in a solvent, so that the LiM alloy material is adsorbed onto the surface of the cathode material core to obtain the cathode material.

7. The method for preparing the self-lithiated cathode material according to claim 6, characterized in that, The core of the cathode material in step (1) has the chemical formula LiNiM, where M is at least one of Mn, Al, Fe or Zr. The core of the cathode material is prepared by mixing a precursor prepared by hydrothermal method with lithium salt and sintering.

8. The method for preparing the self-lithiated cathode material according to claim 6, characterized in that, The preparation method of the LiM alloy material in step (1) is a high-temperature alloying method, which includes the following steps: mixing and grinding Li and M, and calcining at high temperature under an inert atmosphere to obtain the LiM alloy material.

9. The method for preparing the self-lithiated cathode material according to claim 8, characterized in that, The gas in the inert atmosphere includes at least one of N2, Ar and He.

10. The method for preparing the self-lithiated cathode material according to claim 8, characterized in that, The high-temperature calcination temperature is 800℃~1000℃, and the high-temperature calcination time is 10h~12h.

11. The method for preparing the self-lithiated cathode material according to claim 6, characterized in that, The solution of the modifier in step (2) is an aqueous solution of polyvinylpyrrolidone.

12. The method for preparing the self-lithiated cathode material according to claim 6, characterized in that, The mass fraction of the modifier solution is 5% to 10%.

13. The method for preparing the self-lithiated cathode material according to claim 6, characterized in that, In step (2), the cathode material core is added to the solution of the modifier and then stirred.

14. The method for preparing the self-lithiated cathode material according to claim 6, characterized in that, The dispersion method described in step (3) is ultrasound.

15. A positive electrode, characterized in that, The cathode comprises the self-lithiated cathode material according to any one of claims 1-5.

16. The positive electrode according to claim 13, characterized in that, The positive electrode also includes a conductive agent and a binder.

17. A lithium-ion battery, comprising a positive electrode, a negative electrode, a separator, and an electrolyte, characterized in that, The positive electrode is the positive electrode described in claim 15 or 16.

Citation Information

Patent Citations

  • Positive electrode material of lithium battery and preparation method thereof

    CN112038592A

  • Composite cathode material and preparation method thereof and lithium ion battery

    CN112271280A