A manganese iron lithium borate composite material and its preparation method and application
By introducing manganese ions and doping metal ions into the lithium manganese iron borate material, and forming a carbon layer coating, the problem of sensitivity to water and oxygen is solved, the capacity and cycle performance are improved, and a higher voltage platform and Stability, suitable for high energy density lithium batteries.
Patent Information
- Application Number
- CN202410292230.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-13
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-03-13
AI Technical Summary
Lithium iron borate materials are sensitive to water and oxygen, resulting in a rapid decrease in specific capacity after exposure to air at room temperature, limiting their commercial application prospects.
By introducing manganese ions and doping metal ions during the preparation process, and forming a carbon layer coating, the voltage platform and ability to resist water and oxygen of the manganese iron lithium borate composite material are improved, and its conductivity and stability are enhanced.
It significantly improves the capacity and cycle performance of lithium manganese iron borate composite materials, enhances its resistance to water and oxygen, and prolongs its stability, making it suitable for high-energy-density lithium battery applications.
Smart Images

Figure BDA0004742606710000121 
Figure BDA0004742606710000141 
Figure BDA0004742606710000151
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of new energy lithium battery materials, and in particular to a lithium manganese iron borate composite material and a preparation method and application thereof. Background Art
[0002] Lithium iron phosphate material is currently the main lithium battery power material, with a theoretical specific capacity of 170mAh / g. The actual specific capacity of the product is generally 160mAh / g (0.1C, 25°C), while the ternary material can reach 220mAh / g (0.1C, 25°C). Lithium iron phosphate material is far behind this, but lithium iron phosphate material has the advantages of good safety, long service life and low cost, so lithium iron phosphate material has a wider range of applications.
[0003] In order to further improve the theoretical specific capacity of lithium iron phosphate materials, researchers have developed materials such as lithium iron manganese phosphate materials and lithium iron borate materials. Among them, lithium iron manganese phosphate materials have the characteristics of high voltage platform. The voltage platform of lithium iron phosphate is 3.4V, while the voltage platform of lithium iron manganese phosphate materials can reach 3.9V. Therefore, under the same gram capacity, the energy density of lithium iron manganese phosphate materials is about 15% higher. However, lithium iron manganese phosphate materials still have the following disadvantages: 1) The conductivity is extremely poor, which is worse than that of lithium iron phosphate materials, resulting in its particles cannot be too large, so the compaction density is not high. Once the compaction density increases, the capacity will drop sharply; 2) The structure of lithium iron manganese phosphate materials is unstable, and there will be serious problems of manganese dissolution and serious collapse of manganese structure, which will cause the reduction of the cycle performance of lithium iron manganese phosphate materials.
[0004] Compared with lithium iron manganese phosphate material, lithium iron borate material has higher specific capacity (about 220mAh / g) and better conductivity (conductivity of about 3.9×10 -7 S / cm), a very small volume change rate (about 2%), and the molar mass of borate is much smaller than that of phosphate (58.8g / mol for lithium iron borate material and 95g / mol for lithium iron manganese phosphate material), and lithium iron borate material can provide ionic and electronic conductivity at the same time. However, lithium iron borate material has a fatal flaw, that is, it is sensitive to water and oxygen. A small amount of air contact at room temperature will quickly reduce the specific capacity of the material to 70mAh / g. Therefore, this problem poses a great obstacle to the commercial application prospects of lithium iron phosphate materials. Summary of the invention
[0005] In view of the technical problems existing in the background technology, the present application provides a manganese iron lithium borate composite material and its preparation method and application, aiming to solve the problem that the lithium iron borate material is sensitive to water and oxygen, while improving the voltage platform and having a higher theoretical capacity and cycle performance.
[0006] In a first aspect, an embodiment of the present application provides a method for preparing a manganese iron lithium borate composite material, comprising the following steps:
[0007] S1) mixing a manganese salt, a ferrous salt and an acidic solution to obtain a ferromanganese mixed solution, and then mixing the ferromanganese mixed solution with urea to obtain a ferromanganese hydroxide precipitate after reaction;
[0008] S2) mixing the ferromanganese hydroxide precipitate and the boric acid solution, drying and calcining to obtain a calcined material;
[0009] S3) mixing the calcined material, lithium source, dopant, carbon source and water, drying and calcining to obtain a manganese iron lithium borate composite material, wherein the dopant is a source material that provides at least one metal ion with a valence state ≥ +4.
[0010] In the technical solution provided in the embodiment of the present application, the introduction of urea is conducive to the formation of a homogeneous manganese iron hydroxide precipitation, so as to introduce manganese into the lithium iron borate material to form lithium manganese iron borate, thereby improving the voltage platform of the lithium manganese iron borate composite material, and greatly increasing the resistance to water and oxygen. At the same time, a dopant and a carbon source are introduced during the preparation process, and metal ion doping and carbon layer coating are formed by calcination, which greatly improves the ionic conductivity and electronic conductivity of the lithium manganese iron borate composite material. It can be understood that the molar number of borate is smaller than that of phosphate, thereby improving the capacity and cycle performance of the lithium manganese iron borate composite material. Further, during the calcination process, the primary particle size of the lithium manganese iron borate composite material can be increased by limiting the calcination conditions, and the primary particle size of the lithium manganese iron borate composite material can be increased, which can improve the stability of the lithium manganese iron borate composite material.
[0011] In some embodiments, in step S1), the molar ratio of the manganese salt to the ferrous salt is (7-10): (2-5); and / or
[0012] The ratio of the total mole number of the manganese salt and the ferrous salt to the mole number of urea is 1:(3-5); and / or
[0013] The manganese salt is selected from at least one of manganese sulfate, manganese chloride and manganese acetate;
[0014] The ferrous salt is selected from at least one of ferrous sulfate, ferrous chloride and ferrous acetate; and / or
[0015] The concentration of the acidic solution is 0.01-0.05 mol / L, and the acidic solution is selected from a sulfuric acid solution, a hydrochloric acid solution or an acetic acid solution.
[0016] In some embodiments, in step S1), the reaction is carried out under heating and stirring, wherein the stirring speed is 200-500 r / min, the heating temperature is 80-100°C, and the reaction time is 1-5 h; and, after the reaction, filtering and washing are also included, and the washing is stopped after the conductivity of the washing water is ≤200 μS / cm.
[0017] In some embodiments, in step S2), the concentration of the boric acid solution is 2-5 mol / L, the molar ratio of the manganese ferrohydroxide precipitate to the boric acid is 1:(1.01-1.10); the drying is spray drying, the inlet air temperature of the spray drying is 250-300°C, the discharge temperature is 80-100°C, and the particle size of the material obtained by the spray drying is 5-30 μm;
[0018] In some embodiments, in step S2), the calcination is carried out in a rotary kiln, the rotation speed of the rotary kiln is 2-5 r / min; during the calcination, air is blown in and the induced draft fan is turned on, so that the humidity in the rotary kiln is ≤30%. The calcination can reduce the BET of the manganese ferroborate precursor and increase the primary particle size of the manganese ferroborate precursor, which is ultimately beneficial to increase the primary particle size of the manganese ferroborate lithium composite material and further improve the stability of the manganese ferroborate lithium composite material.
[0019] In some embodiments, in step S3), the carbon source is selected from soluble starch, the lithium source is selected from one or more of lithium carbonate, lithium acetate and lithium oxalate, the metal ion is Sn or Ti, and the dopant is selected from at least one of oxides, hydroxides and carbonates of metal ions; the ratio of the total molar number of manganese iron ions in the calcined material, the molar number of lithium ions in the lithium source and the molar number of metal ions in the dopant is 1: (1.01-1.05): (0.005-0.01); the amount of the carbon source added is such that the carbon content in the manganese iron lithium borate composite material is 2.0-5.0wt%. The metal ions of the dopant are selected from high-valent metal ions, which can form higher crystal defects with lithium manganese borate, and the doping effect is better.
[0020] In some embodiments, in step S3), the mixing method includes ball milling and sand milling performed in sequence, the solid content of the slurry obtained after the sand milling is 30-45wt%, and the particle size of the slurry obtained after the sand milling is 200-400nm; nitrogen is introduced during the calcination process, and the volume fraction of oxygen is ≤2ppm, the heating rate of the calcination is 1-5℃ / h; the calcination temperature is 700-800℃, and the time is 9-14h. In the calcination process, the calcination temperature is high and the calcination time is long, which can further increase the primary particle size of the manganese iron lithium borate composite material.
[0021] In a second aspect, an embodiment of the present application provides a lithium manganese iron borate composite material, which includes lithium manganese iron borate and a carbon layer coated on the surface of the lithium manganese iron borate, wherein the lithium manganese iron borate is doped with at least one metal ion with a valence state ≥ +4.
[0022] In this embodiment, the voltage platform and the ability to resist water and oxygen of the lithium manganese iron borate composite material are improved by manganese doping, and the ionic conductivity and electronic conductivity of the lithium manganese iron borate composite material are greatly improved by metal ion doping and the introduction of a carbon coating layer; ultimately, the capacity and cycle performance of the composite material are improved.
[0023] In a third aspect, an embodiment of the present application provides a positive electrode plate, comprising the above-mentioned lithium manganese iron borate composite material.
[0024] In this embodiment, the positive electrode plate includes the above-mentioned manganese iron lithium borate composite material, so it has the ability to resist oxygen and water, and also has a higher voltage platform and cycle performance and capacity.
[0025] In a fourth aspect, a secondary battery is provided in an embodiment of the present application, comprising the above-mentioned positive electrode plate.
[0026] In this embodiment, the secondary battery includes the above-mentioned positive electrode plate, and thus has the ability to resist oxygen and water, and also has a higher voltage platform and cycle performance and capacity.
[0027] In a fifth aspect, an embodiment of the present application provides an electrical device, comprising the above-mentioned secondary battery.
[0028] In this embodiment, the electrical device includes the above-mentioned secondary battery, so it has the ability to resist oxygen and water, and also has a higher voltage platform and cycle performance and capacity.
[0029] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the technical solution of the present application, the following is a brief introduction to the drawings used in the present application. Obviously, the drawings described below are only some embodiments of the present application, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0031] Figure 1 This is a SEM photo of the lithium manganese iron borate composite material prepared in Example 1 of the present invention;
[0032] Figure 2This is a charge and discharge curve diagram of the manganese iron borate lithium composite material prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0033] The following embodiments of the technical solution of the present application are described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.
[0034] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.
[0035] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.
[0036] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0037] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of the associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.
[0038] In the description of the embodiments of the present application, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).
[0039] In the description of the embodiments of the present application, the technical terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, which are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the embodiments of the present application.
[0040] In the description of the embodiments of the present application, unless otherwise clearly specified and limited, technical terms such as "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, and it can be the internal connection of two elements or the interaction relationship between two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the embodiments of the present application can be understood according to the specific circumstances.
[0041] In the prior art, lithium iron borate materials are sensitive to water and oxygen. A small amount of air contact at room temperature will reduce the stability of lithium iron phosphate materials, causing the specific capacity of lithium iron borate materials to decrease rapidly. In order to solve the technical problem that lithium iron phosphate materials are sensitive to water and oxygen, the present application provides a lithium iron manganese phosphate composite material and a preparation method thereof, a positive electrode sheet, a secondary battery and an electrical device, wherein manganese ions are introduced during the preparation process, and are combined with doped metal ions and a carbon layer to improve the resistance of the lithium iron manganese phosphate composite material to water and oxygen, and ultimately improve the capacity and cycle performance of the composite material as a positive electrode material, thereby improving the resistance, capacity and cycle performance of the positive electrode sheet, secondary battery and electrical device to water and oxygen.
[0042] In a first aspect, an embodiment of the present application provides a method for preparing a manganese iron lithium borate composite material, comprising the following steps:
[0043] S1) mixing a manganese salt, a ferrous salt and an acidic solution to obtain a ferromanganese mixed solution, and then mixing the ferromanganese mixed solution with urea to obtain a ferromanganese hydroxide precipitate after reaction;
[0044] S2) mixing the ferromanganese hydroxide precipitate and the boric acid solution, drying and calcining to obtain a calcined material;
[0045] S3) mixing the calcined material, the lithium source, the dopant, the carbon source and water, drying and calcining to obtain a manganese iron lithium borate composite material, wherein the dopant is a source material that provides at least one metal ion with a valence state ≥ +4.
[0046] Specifically, in the preparation process of the lithium iron manganese phosphate composite material, the present application first homogeneously precipitates manganese salts and ferrous salts under the action of urea to obtain manganese hydroxide precipitates to provide a basis for forming lithium iron manganese borate. Thereafter, the manganese hydroxide precipitates are mixed with boric acid and calcined to form a manganese iron borate material. Finally, the obtained manganese iron borate material, a lithium source, a dopant and a carbon source are mixed, and after calcination, a carbon layer-coated lithium iron manganese borate material is obtained, and at the same time, metal ions are doped in the lithium iron manganese borate, thereby obtaining a lithium iron manganese borate composite material.
[0047] In the technical solution of the embodiment of the present application, in the process of preparing the manganese iron lithium borate composite material, in step S1), firstly, a manganese salt, a ferrous salt and an acidic solution are mixed to obtain a manganese iron mixed solution; wherein, the manganese salt is selected from one or more of manganese sulfate, manganese chloride and manganese acetate, specifically, the manganese salt is selected from manganese sulfate, manganese chloride or manganese acetate, and the ferrous salt is selected from one or more of ferrous sulfate, ferrous chloride and ferrous acetate, specifically, the ferrous salt is selected from ferrous sulfate, ferrous chloride or ferrous acetate. The acidic solution is used to provide an acidic environment for the reaction, specifically, the concentration of the acidic solution is 0.01 to 0.05 mol / L, specifically, the concentration of the acidic solution is 0.01 to 0.02 mol / L, more specifically, the concentration of the acidic solution is 0.01 mol / L, 0.015 mol / L or 0.02 mol / L, etc. The acidic solution is selected from a sulfuric acid solution, a hydrochloric acid solution or an acetic acid solution, specifically, the acidic solution is selected from a sulfuric acid solution. The molar ratio of manganese salt to ferrous salt is (7-10):(2-5), specifically, the molar ratio of manganese salt to ferrous salt is (7-8):(2-3), more specifically, the molar ratio of manganese salt to ferrous salt is 7.5:2.5, 7:3 or 8:2, etc.
[0048] In step S1), after obtaining the manganese iron mixed solution, it is mixed with urea, and after the reaction, a manganese iron hydroxide precipitate is obtained; in this process, the added urea causes the manganese ions and ferrous ions to form a uniform precipitate, thereby finally achieving atomic-level mixing of the manganese iron elements of the manganese iron borate lithium, which is beneficial to ensure the stability of the material. Among them, the ratio of the total mole number of manganese salts and ferrous salts to the mole number of urea is 1: (3 to 5), specifically, the ratio of the total mole number of manganese salts and ferrous salts to the mole number of urea is 1: (3 to 4.5), more specifically, the ratio of the total mole number of manganese salts and ferrous salts to the mole number of urea is 1: 3, 1: 4 or 1: 4.5, etc. The reaction is carried out under heating and stirring, wherein the stirring speed is 200-500r / min, specifically, the stirring speed is 200-400r / min; the heating temperature is 80-100°C, the reaction time is 1-5h, specifically, the heating temperature is 95-100°C, the reaction time is 1-2h, more specifically, the heating temperature is 95°C, 98°C or 100°C, the reaction time is 1h, 1.5h or 2h, etc. After the reaction, filtering and washing are carried out in sequence to obtain manganese hydroxide ferroprecipitate; the filtering is carried out in a manner well known to those skilled in the art, and the washing is stopped after the conductivity of the washing water is ≤200μS / cm.
[0049] In step S2), the above-obtained ferromanganese hydroxide precipitate and boric acid solution are mixed, dried and then calcined to obtain a calcined material; in this step, ferromanganese borate is obtained by introducing boric acid and calcining. Wherein, the concentration of the boric acid solution is 2-5 mol / L, specifically, the concentration of the boric acid solution is 2-4 mol / L, more specifically, the concentration of the boric acid solution is 2 mol / L, 3 mol / L or 4 mol / L. The molar ratio of the ferromanganese hydroxide precipitate to boric acid is 1:(1.01-1.10), specifically, the molar ratio of the ferromanganese hydroxide precipitate to boric acid is 1:(1.01-1.03), more specifically, the molar ratio of the ferromanganese hydroxide precipitate to boric acid is 1:1.01, 1:1.02 or 1:1.03, etc. The drying is spray drying, the inlet air temperature of the spray drying is 250-300°C, the discharge temperature is 80-100°C, and the particle size of the material obtained by spray drying is 5-30μm; specifically, the inlet air temperature of the spray drying is 260-280°C, the discharge temperature is 90-95°C, and the particle size of the material obtained after spray drying is 8-20μm. After spray drying, calcination is carried out in a rotary kiln, and the rotation speed of the rotary kiln is 2-5r / min; during the calcination process, air is blown in and the induced draft fan is turned on, so that the humidity in the rotary kiln is ≤30%; specifically, the rotation speed of the rotary kiln is 2-4r / min, more specifically, the rotation speed of the rotary kiln is 2r / min, 3r / min or 4r / min, etc.
[0050] In step S3), the calcined material, lithium source, dopant, carbon source and water obtained above are finally mixed, dried and calcined to obtain a manganese iron lithium borate composite material. In this step, the introduction of the dopant and the introduction of the lithium source form a carbon coating layer and metal ion doping, respectively. The formation of the carbon coating layer can improve the electronic conductivity of the material, and the introduction of the dopant can improve the ionic conductivity of the manganese iron lithium borate composite material. Among them, the carbon source is selected from soluble starch, and the lithium source is selected from one or more of lithium carbonate, lithium acetate and lithium oxalate. The dopant is specifically a source material that provides at least one metal ion with a valence state ≥ +4, more specifically a source material that provides Ti ions or Sn ions. In a specific embodiment, the dopant is selected from at least one of the oxides, hydroxides and carbonates of Ti or Sn. For example, the dopant is selected from TiO 2 、Sn(OH) 4 or SnO 2 .
[0051] Among them, the ratio of the total molar number of manganese and iron ions in the calcined material, the molar number of lithium ions in the lithium source and the molar number of metal ions in the dopant is 1:(1.01-1.05):(0.005-0.01), specifically, the ratio of the total molar number of manganese and iron ions in the calcined material, the molar number of lithium ions in the lithium source and the molar number of metal ions in the dopant is 1:(1.02-1.05):(0.005-0.01), more specifically, the ratio of the total molar number of manganese and iron ions in the calcined material, the molar number of lithium ions in the lithium source and the molar number of metal ions in the dopant is 1:1.04:0.008, 1:1.05:0.01 or 1:1.02:0.005, etc. The amount of carbon source added is such that the carbon content in the manganese iron lithium borate composite material is 2.0-5.0wt%, specifically, the amount of carbon source added is such that the carbon content in the manganese iron lithium borate composite material is 2.0-3.5wt%, more specifically, the amount of carbon source added is such that the carbon content in the manganese iron lithium borate composite material is 2.0wt%, 2.9wt% or 3.5wt%, etc. In order to fully mix the above raw materials, the mixing method includes ball milling and sand milling in sequence, the solid content of the slurry obtained after sand milling is 30-45wt%, the particle size of the slurry obtained after sand milling is 200-400nm, specifically, the solid content of the slurry is 35-42wt%, and the particle size is 280-260nm.
[0052] Specifically, after sand grinding, it is preferably dried by spray drying, and then calcined. Nitrogen is introduced during the calcination process, and the volume fraction of oxygen is ≤2ppm to avoid the introduction of oxygen elements during the preparation process. The heating rate of calcination is 1-5°C / h; the calcination temperature is 700-800°C, and the time is 9-14h; specifically, the heating rate of calcination is 2-4°C / h, the calcination temperature is 730-780°C, and the time is 10-14h; more specifically, the calcination temperature is 750°C, 775°C or 780°C, etc., and the time is 9h, 12h or 14h, etc.
[0053] In a second aspect, an embodiment of the present application provides a manganese iron lithium borate composite material, which includes manganese iron lithium borate and a carbon layer coated on the surface of the manganese iron lithium borate, and the manganese iron lithium borate is also doped with at least one metal ion other than manganese ions, iron ions and lithium ions.
[0054] In the manganese iron borate lithium composite material of the present application, the manganese iron borate lithium is located in the core region, the carbon layer is coated on the surface of the manganese iron borate lithium, and the core region is doped with metal ions. Specifically, the metal ion is at least one metal ion with a valence state of ≥ +4, and more specifically, the metal ion is selected from Ti 4+ or Sn 4+ .
[0055] The present application introduces manganese into the manganese iron lithium borate composite material to enhance its resistance to water and oxygen, and the introduction of manganese can improve the voltage platform. At the same time, the introduction of manganese and the doping of metal ions can improve the ionic conductivity and the stability of the material, which is beneficial to the improvement of the cycle performance. Compared with phosphate, borate has a smaller molar number, so its capacity is higher.
[0056] In the lithium manganese iron borate composite material, the carbon layer is 2.0-5.0wt% of the lithium manganese iron borate composite material, and the doping amount of metal ions in the lithium manganese iron borate is 1000-3000ppm; more specifically, the carbon layer is 2.0-3.5wt% of the lithium manganese iron borate composite material, and the doping amount of metal ions in the lithium manganese iron borate is 1500-2700ppm.
[0057] In a third aspect, an embodiment of the present application provides a positive electrode plate, comprising the above-mentioned lithium manganese iron borate composite material.
[0058] In the positive electrode sheet, the manganese iron lithium borate composite material is used as the active material, and other components may include a conductive agent and a binder; the current collector in the positive electrode sheet is not particularly limited in this application.
[0059] In a fourth aspect, an embodiment of the present application provides a secondary battery, comprising the positive electrode plate described in the above scheme.
[0060] In the secondary battery, the negative electrode sheet is not particularly limited in this application.
[0061] In a fifth aspect, an embodiment of the present application provides an electrical device, comprising the above-mentioned secondary battery.
[0062] The electric device provided in the embodiment of the present application may be, but is not limited to, a mobile phone, a tablet, a laptop computer, an electric toy, an electric tool, a battery car, an electric car, a ship, a spacecraft, etc. Among them, the electric toy may include a fixed or mobile electric toy, such as a game console, an electric car toy, an electric ship toy, and an electric airplane toy, etc., and the spacecraft may include an airplane, a rocket, a space shuttle, and a spacecraft, etc.
[0063] Some specific embodiments are listed below. It should be noted that the embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used without specifying the manufacturer are all conventional products that can be obtained commercially.
[0064] Example 1
[0065] A method for preparing a lithium-ion battery positive electrode material, comprising the following steps:
[0066] (1) adding manganese sulfate and ferrous sulfate in a molar ratio of 7.5:2.5 to a 0.015 mol / L sulfuric acid solution, mixing and stirring to dissolve, to obtain a manganese-iron mixed solution, wherein the total molar number of manganese and iron ions is 2.5 mol / L; then adding urea, heating to 98° C. at a stirring speed of 300 r / min, reacting at this temperature for 1.5 hours, then filtering and washing, washing until the conductivity of the washing water is ≤200 μS / cm, then stopping washing to obtain manganese-iron hydroxide precipitate, wherein the ratio of the total molar number of manganese sulfate and ferrous sulfate to the molar number of urea is 1:4;
[0067] (2) adding the ferromanganese hydroxide precipitate to a 3 mol / L boric acid solution, stirring to form a slurry, and then spray drying, wherein the inlet air temperature during the spray drying process is 280° C., and the discharge temperature is 90° C., to obtain a spray-dried material with a particle size of 18 μm, wherein the molar ratio of the ferromanganese hydroxide precipitate to the boric acid is 1:1.02;
[0068] (3) placing the spray-dried material into a rotary kiln at a rotation speed of 3 r / min and calcining it, blowing air into the kiln during the calcination process, and simultaneously starting the induced draft fan to draw out water vapor, so that the humidity in the rotary kiln is ≤30%, the calcination temperature is 600° C., the calcination time is 5 h, and a calcined material is obtained;
[0069] (4) adding lithium carbonate, titanium dioxide and soluble starch to the calcined material, and then adding pure water, and then ball milling and sand milling, spray drying the sand-milled slurry with a solid content of 38 wt% and a particle size of 305 nm to obtain a spray-dried material;
[0070] The spray-dried material was placed in a roller kiln for calcination, and the temperature was raised to 775° C. at a heating rate of 2° C. / h, and calcined for 12 hours to obtain a manganese iron borate lithium composite material; the ratio of the total molar number of manganese iron in the calcined material to the molar number of lithium ions and titanium ions was 1:1.04:0.008, and a carbon source was added so that the carbon content of the final product was 2.9wt%; nitrogen was introduced during the calcination process to maintain the volume fraction of oxygen in the roller kiln ≤2ppm;
[0071] (5) The manganese iron borate lithium composite material calcined in step (4) is subjected to air flow crushing, sieving to remove iron, and vacuum packaging to obtain a manganese iron borate lithium product.
[0072] Figure 1 This is a SEM photo of the lithium manganese iron borate product prepared in this example. Figure 1 It can be seen that the primary particle size of the lithium manganese iron borate product prepared in this embodiment is about 200nm, the particles are relatively large, the sphericity is good, and the BET is small, thereby improving the stability of the material. According to the ratio of the raw materials in the preparation method, the chemical formula of the lithium manganese iron borate product obtained in this embodiment is Li 1.04 Fe 0.75 Mn 0.25 Ti 0.008 (BO 3 ) 1.02 / C.
[0073] Furthermore, the performance of the lithium manganese iron borate product was tested, wherein the compaction density was tested using a compaction density tester, with reference to the standard GB / T 24533-2019, where the test pressure was 3T; the powder internal resistance was tested using a four-probe method, with reference to the standard GB / T39978-2021, where the test pressure was 8MPa; and the particle size was tested using a laser particle size analyzer, with reference to the standard GB / T 24533-2019. The test results are shown in Table 1.
[0074] Furthermore, the electrochemical performance of the lithium manganese iron borate product was tested by a soft-pack battery cell. The positive electrode formula was: the mass ratio of the lithium manganese iron borate product prepared in this embodiment: PVDF: SP was 92:4:4, the pole piece compaction density was 2.3 g / mL, the current collector was carbon-coated aluminum foil, the electrolyte was lithium hexafluorophosphate, the concentration was 1 mol / L, the negative electrode was graphite, and the battery capacity was 12 Ah. The results are shown in Tables 1 and Figure 2 shown.
[0075] Table 1 Performance data of lithium manganese iron borate product prepared in Example 1
[0076]
[0077] Note: The contents of the above elements in Table 1 are percentages by mass of lithium manganese iron borate products.
[0078] It can be seen from Table 1 that the lithium manganese iron borate product prepared in the present application has a higher compaction density and higher cycle stability and capacity.
[0079] Depend on Figure 2 It can be seen that the lithium manganese iron borate product prepared in this embodiment has a high capacity, a high voltage platform, and there are two obvious discharge platforms.
[0080] The lithium manganese iron borate product prepared in this embodiment was placed in an atmospheric environment (humidity of 70%, oxygen volume concentration of 20.97%, temperature of 27.3° C.) to detect its stability. The corresponding table of placement time and capacity is shown in Table 2;
[0081] Table 2 Stability data of lithium manganese iron borate product prepared in this example
[0082] Placement time Material moisture 0.1C charging capacity 0.1C discharge capacity Discharge efficiency 0h 417ppm 209.5mAh / g 187.4mAh / g 89.45% 0.5h 1027ppm 198.5mAh / g 180.7mAh / g 91.03% 2h 1369ppm 195.2mAh / g 180.1mAh / g 92.26% 12h 1726ppm 194.7mAh / g 179.8mAh / g 92.35% 24h 1871ppm 194.4mAh / g 179.6mAh / g 92.39%
[0083] It can be seen from Table 2 that after 24 hours of storage at room temperature, the charging capacity of the lithium manganese iron borate product prepared in this embodiment decreased by 15.1 mAh / g, and the discharge capacity decreased by 7.8 mAh / g, and the charge and discharge capacity basically tended to be stable over time.
[0084] Comparative Example 1
[0085] The carbon-coated lithium iron borate prepared by a conventional solid phase method, i.e., a material obtained by mixing red iron oxide, lithium borate and glucose, was sand-milled, spray-dried and calcined to obtain a carbon-coated lithium iron borate having a carbon content of 3.5%. The carbon-coated lithium iron borate was finally placed in the same environment as in Example 1, i.e., a humidity of 70%, an oxygen volume concentration of 20.97% and a temperature of 27.3° C., and its stability was tested. The relationship between the placement time and the capacity is shown in Table 3;
[0086] Table 3 Stability data of lithium iron borate product prepared in this comparative example
[0087] Placement time Material moisture 0.1C charging capacity 0.1C discharge capacity Discharge efficiency 0h 589ppm 191.5mAh / g 172.5mAh / g 90.1% 0.5h 1359ppm 178.6mAh / g 157.4mAh / g 88.1% 2h 1745ppm 163.6mAh / g 141.3mAh / g 86.4% 12h 1998ppm 147.9mAh / g 120.5mAh / g 81.5% 24h 2580ppm 123.2mAh / g 110.7mAh / g 89.9%
[0088] It can be seen from Table 3 that, compared with Example 1, the lithium iron borate prepared by the conventional process has very poor ability to resist water vapor and oxygen, and its capacity decays quickly, and even after being placed for 24 hours, there is still a certain degree of decay.
[0089] Example 2
[0090] A method for preparing a positive electrode material for a lithium battery comprises the following steps:
[0091] (1) adding manganese chloride and ferrous chloride in a molar ratio of 7:3 to a 0.01 mol / L sulfuric acid solution, mixing and stirring to dissolve, to obtain a manganese-iron mixed solution, wherein the total molar number of manganese and iron ions is 2.5 mol / L; then adding urea, heating to 95° C. at a stirring speed of 200 r / min, reacting at this temperature for 2 hours, then filtering and washing, washing until the conductivity of the washing water is ≤200 μS / cm and then stopping washing to obtain a manganese-iron hydroxide precipitate, wherein the ratio of the total molar number of manganese chloride and ferrous chloride to the molar number of urea is 1:3;
[0092] (2) adding the ferromanganese hydroxide precipitate to a 2 mol / L boric acid solution, stirring to form a slurry, and then spray drying, wherein the inlet air temperature during the spray drying process is 250° C. and the outlet temperature is 80° C., to obtain a 5.2 μm spray-dried material, wherein the molar ratio of the ferromanganese hydroxide to the boric acid is 1:1.01;
[0093] (3) placing the spray-dried material into a rotary kiln at a rotation speed of 2 r / min for calcination, blowing air into the kiln during the calcination process, and simultaneously starting the induced draft fan to draw out water vapor, so that the humidity in the rotary kiln is ≤30%, the calcination temperature is 650° C., the calcination time is 4 h, and a calcined material is obtained;
[0094] (4) adding lithium carbonate, tin hydroxide and soluble starch to the calcined material, and then adding pure water, and then ball milling and sand milling, spray drying the sand-milled slurry with a solid content of 30 wt % and a particle size of 200 nm to obtain a spray-dried material;
[0095] The spray-dried material was placed in a roller kiln for calcination, and the temperature was raised to 800° C. at a heating rate of 1.5° C. / h, and calcined for 9 hours to obtain a manganese iron borate lithium composite material; the ratio of the total molar number of manganese iron to the molar number of lithium ions and tin ions in the calcined material was 1:1.05:0.01, and a carbon source was added so that the carbon content of the final product was 2.0wt%; nitrogen was introduced during the calcination process to maintain the volume fraction of oxygen in the roller kiln ≤2ppm;
[0096] (5) The manganese iron borate lithium composite material calcined in step (4) is subjected to air flow pulverization, sieving to remove iron, and vacuum packaging to obtain a manganese iron borate lithium product. According to the ratio of the raw materials in the preparation method, the chemical formula of the manganese iron borate lithium product obtained in this embodiment is Li 1.05 Fe 0.7 Mn 0.3 Sn 0.01 (BO 3 ) 1.01 / C.
[0097] The performance of the lithium manganese iron borate product prepared in this embodiment was tested according to the testing method of Example 1, and the results are shown in Table 4;
[0098] Table 4 Performance data of lithium manganese iron borate product prepared in Example 2
[0099]
[0100]
[0101] Note: The contents of the above elements in Table 4 are percentages by mass of the lithium manganese iron borate product.
[0102] It can be seen from Table 4 that the lithium manganese iron borate product prepared in the present application has a higher compaction density and higher cycle stability and capacity.
[0103] Example 3
[0104] A method for preparing a positive electrode material for a lithium battery comprises the following steps:
[0105] (1) adding manganese acetate and ferrous acetate in a molar ratio of 8:2 to a 0.02 mol / L sulfuric acid solution, mixing and stirring to dissolve, to obtain a manganese-iron mixed solution, wherein the total molar number of manganese and iron ions is 4.5 mol / L; then adding urea, heating to 100° C. at a stirring speed of 400 r / min, reacting at this temperature for 1 hour, then filtering and washing, washing until the conductivity of the washing water is ≤200 μS / cm, then stopping washing to obtain a manganese-iron hydroxide precipitate, wherein the ratio of the total molar number of manganese acetate and ferrous acetate to the molar number of urea is 1:4.5;
[0106] (2) adding the ferromanganese hydroxide precipitate to a 4 mol / L boric acid solution, stirring to form a slurry, and then spray drying, wherein the inlet air temperature during the spray drying process is 300° C. and the outlet temperature is 95° C., to obtain a spray-dried material with a particle size of 30 μm, wherein the molar ratio of the ferromanganese hydroxide to the boric acid is 1:1.03;
[0107] (3) placing the spray-dried material into a rotary kiln at a rotation speed of 4 r / min for calcination, blowing air into the kiln during the calcination process, and simultaneously starting the induced draft fan to draw out water vapor, so that the humidity in the rotary kiln is ≤30%, the calcination temperature is 650° C., the calcination time is 6 h, and a calcined material is obtained;
[0108] (4) adding lithium carbonate, tin oxide and soluble starch to the calcined material, and then adding pure water, and then subjecting the calcined material to ball milling and sand milling, spray drying the sand milled slurry having a solid content of 45 wt% and a particle size of 400 nm to obtain a spray dried material;
[0109] The spray-dried material was placed in a roller kiln for calcination, and the temperature was raised to 750°C at a heating rate of 2.5°C / h, and calcined for 14 hours to obtain a manganese iron borate lithium composite material; the ratio of the total molar number of manganese iron in the calcined material to the molar number of lithium ions and tin ions was 1:1.02:0.005, and the added carbon source made the carbon content of the final product 3.5wt%; during the calcination process, nitrogen was introduced to maintain the volume fraction of oxygen in the roller kiln ≤2ppm;
[0110] (5) The manganese iron borate lithium composite material calcined in step (4) is subjected to air flow pulverization, sieving to remove iron, and vacuum packaging to obtain a manganese iron borate lithium product. According to the ratio of the raw materials in the preparation method, the chemical formula of the manganese iron borate lithium product obtained in this embodiment is Li 1.02 Fe 0.8 Mn 0.2 Sn 0.005 (BO 3 ) 1.03 / C.
[0111] The performance of the lithium manganese iron borate product prepared in this example was tested according to the testing method of Example 1, and the results are shown in Table 5;
[0112] Table 5 Performance data of lithium manganese iron borate product prepared in Example 3
[0113]
[0114] Note: The contents of the above elements in Table 5 are percentages by mass of lithium manganese iron borate products.
[0115] It can be seen from Table 5 that the lithium manganese iron borate product prepared in the present application has a higher compaction density and higher cycle stability and capacity.
[0116] Comparative Example 2
[0117] The preparation method of the lithium manganese iron borate composite material is the same as that of Example 1, except that titanium dioxide is not added in step (4).
[0118] Table 6 Performance data of lithium manganese iron borate product prepared in Comparative Example 2
[0119]
[0120] Comparative Example 3
[0121] The preparation method of the lithium manganese iron borate composite material is the same as that of Example 1, except that urea is not added in step (1).
[0122] Table 7 Performance data of lithium manganese iron borate product prepared in Comparative Example 3
[0123]
[0124] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A method for preparing a manganese iron lithium borate composite material, comprising the following steps: S1) mixing a manganese salt, a ferrous salt and an acidic solution to obtain a manganese-iron mixed solution, and then mixing the manganese-iron mixed solution with urea to obtain a manganese-iron hydroxide precipitate after reaction; S2) mixing the ferromanganese hydroxide precipitate and the boric acid solution, drying and calcining to obtain a calcined material; S3) mixing the calcined material, lithium source, dopant, carbon source and water, drying and calcining to obtain a manganese iron lithium borate composite material, wherein the dopant is a source material that provides at least one metal ion with a valence state of ≥ +4; The molar ratio of the manganese salt to the ferrous salt is (7-10): (2-5); the molar ratio of the total molar number of the manganese salt and the ferrous salt to urea is 1: (3-5); the metal ion is Sn or Ti, and the dopant is selected from at least one of the oxide, hydroxide and carbonate of the metal ion.
2. The preparation method according to claim 1, characterized in that: In step S1), The manganese salt is selected from at least one of manganese sulfate, manganese chloride and manganese acetate; The ferrous salt is selected from at least one of ferrous sulfate, ferrous chloride and ferrous acetate; and / or The concentration of the acidic solution is 0.01-0.05 mol / L, and the acidic solution is selected from sulfuric acid solution, hydrochloric acid solution or acetic acid solution.
3. The preparation method according to claim 1, characterized in that: In step S1), the reaction is carried out under heating and stirring, wherein the stirring speed is 200-500 r / min, the heating temperature is 80-100°C, and the reaction time is 1-5 h; and, after the reaction, filtering and washing are also included, and the washing is stopped after the conductivity of the washing water is ≤200 μS / cm.
4. The preparation method according to claim 1, characterized in that: In step S2), the concentration of the boric acid solution is 2-5 mol / L, and the molar ratio of the manganese iron hydroxide precipitate to the boric acid is 1:(1.01-1.10).
5. The preparation method according to claim 1, characterized in that: In step S3), the carbon source is selected from soluble starch, and the lithium source is selected from one or more of lithium carbonate, lithium acetate and lithium oxalate.
6. The preparation method according to claim 1 or 5, characterized in that: In step S3), the ratio of the total molar number of manganese iron ions in the calcined material, the molar number of lithium ions in the lithium source and the molar number of metal ions in the dopant is 1: (1.01-1.05): (0.005-0.01); the amount of the carbon source added is such that the carbon content in the manganese iron lithium borate composite material is 2.0-5.0wt%; and / or During the calcination, nitrogen is introduced, and the volume fraction of oxygen is ≤2ppm. The heating rate of the calcination is 1-5°C / h; the calcination temperature is 700-800°C, and the calcination time is 9-14h.
7. The manganese iron lithium borate composite material prepared by the preparation method according to any one of claims 1 to 6, comprising manganese iron lithium borate and a carbon layer coated on the surface of the manganese iron lithium borate, wherein the manganese iron lithium borate is doped with at least one metal ion with a valence state ≥ +4.
8. A positive electrode sheet, characterized in that: The invention relates to a lithium manganese iron borate composite material prepared by the preparation method according to any one of claims 1 to 6 or a lithium manganese iron borate composite material according to claim 7.
9. A secondary battery, characterized in that: Including the positive electrode sheet as described in claim 8.
10. An electrical device, characterized in that: A secondary battery comprising the secondary battery according to claim 9.
Citation Information
Patent Citations
Lithium iron borate modified lithium manganate material and preparation method thereof
CN114142004A
Preparation method of ferroboron alloy coated lithium iron phosphate
CN114649518A
Boron-doped reduced graphene oxide coated lithium manganese iron phosphate composite material and preparation method thereof
CN116190612A
Lithium-manganese composite oxide granular secondary particle, method for production thereof and use thereof
US20050123832A1