A porous microcarrier and a method for producing the same
By using raw materials such as hyperbranched polyquaternium amino acids, chitosan quaternary ammonium salts and sodium alginate, combined with emulsification and supercritical drying technology, porous microcarriers with high mechanical mechanical properties and good biocompatibility are prepared to solve the problem of It solves the problems of small surface area and insufficient mechanical strength of microcarriers in the existing technology, achieves high-density cell culture and structural stability, and is suitable for industrial production.
Patent Information
- Application Number
- CN202410262567.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-07
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-03-07
AI Technical Summary
During the manufacturing process, existing porous microcarriers have problems such as small surface area, insufficient mechanical strength, easy breakage, and the need for high temperature or freeze-dehydration drying, resulting in structural damage and organic matter residues, which affects cell culture efficiency and product performance.
Porous microcarriers are prepared using non-toxic and harmless raw materials such as hyperbranched polyquaternary ammonium amino acids, chitosan quaternary ammonium salts and sodium alginate, through aqueous phase dispersion and oil phase emulsification, supercritical drying and UV sterilization. , avoid high temperature or freeze-dehydration drying, and enhance mechanical properties and biocompatibility.
It improves the specific surface area and mechanical properties of porous microcarriers, reduces production costs and environmental impact, achieves high-density cell culture and structural stability, and is suitable for industrial continuous production.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of porous materials, and in particular to a porous microcarrier and a production method thereof. Background Art
[0002] Microcarrier technology is an effective means to achieve large-scale cell culture. Adherent cell culture requires a large surface for cell attachment and growth. The emergence of microcarriers can provide sufficient adhesion sites for adherent cells, achieve large-scale cell suspension culture, greatly improve culture efficiency, reduce culture volume, and achieve multi-polar amplification.
[0003] Most of the existing porous microcarriers are surface-type, with a small area for cell attachment and growth, and low cell culture efficiency. During the production process, rotary vacuum drying or freeze drying is required for drying, and there is a phenomenon of particle agglomeration. If the temperature is not selected appropriately, the structure of the microcarrier may be destroyed, affecting product performance. In the existing methods, the microcarrier needs to be dehydrated with anhydrous ethanol or other organic matter. After dehydration, rotary vacuum drying or freeze drying will cause some organic matter to remain, affecting subsequent use. In addition, the porous microcarriers on the market also have more or less technical defects such as easy detachment of cells, insufficient mechanical strength, easy breakage of microcarriers due to mechanical stirring during cell culture, and short maintenance time of high-density cell culture.
[0004] In order to solve the above problems, a Chinese invention patent with the authorization announcement number CN1253556C discloses a porous microcarrier for animal cell culture and a preparation method thereof, which belongs to the field of biochemical engineering and cell engineering. The method comprises the following steps: (1) dissolving: dissolving cotton wool with a cuprammonia solution; (2) granulating: spraying the cotton wool cuprammonia solution through a sharp hole into an oily freezing liquid with a temperature below -30°C to form microspheres containing ice crystals; (3) pore-forming: regenerating the cotton wool microspheres with concentrated sulfuric acid and dissolving the ice crystals therein to form porous microspheres; (4) modifying: modifying the surface of the porous microspheres with 2-diethylaminoethyl chloride hydrochloride to cross-link the -DEAE weakly alkaline anion exchange group; (5) washing and sterilizing. The porous microcarrier prepared by the method for culturing animal cells has a high cell density and a large specific surface area, can protect cells from mechanical damage, has high mechanical strength, can be sterilized under high pressure and recycled, and has low cost. However, the porous microcarrier preparation process requires the use of concentrated sulfuric acid, which is not environmentally friendly; a special sharp-hole injector is required, which requires a large investment in equipment.
[0005] It can be seen that the development of a porous microcarrier with a large specific surface area, good mechanical properties, and a well-preserved porous structure during the production process, and no need for high temperature or freeze-dehydration and drying, and its production method meet market demand, have broad market value and application prospects, and are of great significance to promoting the development of microcarrier technology and adherent cell culture. Summary of the invention
[0006] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a porous microcarrier with a large specific surface area, good mechanical properties, and a porous structure of the microcarrier that is well preserved during the production process and does not require high temperature or freeze-dehydration drying, and a production method thereof.
[0007] To achieve the above object, the technical solution adopted by the present invention is: a method for producing a porous microcarrier, comprising the following steps:
[0008] Step S1, preparation of aqueous dispersion: adding hyperbranched polyquaternary ammonium amino acid and chitosan quaternary ammonium salt to alkali solution, dispersing them evenly at 50-60° C., then adding sodium alginate thereto, and continuing to stir and react for 1-5 hours to obtain an aqueous dispersion;
[0009] Step S2, selecting the oil phase: taking vegetable oil as the oil phase;
[0010] Step S3, preparation of W / O emulsion: mixing the aqueous phase dispersion prepared in step S1 with the oil phase, and emulsifying with an emulsifier at room temperature to obtain a W / O emulsion;
[0011] Step S4, collecting microcarriers: stirring the W / O emulsion prepared in step S3 at room temperature for 5-10 hours, filtering out the upper organic phase, collecting microcarriers, and washing the collected microcarriers;
[0012] Step S5, supercritical drying and sterilization: The cleaned microcarriers are subjected to supercritical drying and then sterilized to obtain porous microcarriers.
[0013] Preferably, the mass ratio of the hyperbranched polyquaternary ammonium amino acid, chitosan quaternary ammonium salt, alkali solution and sodium alginate in step S1 is (3-5):1:(15-25):(0.8-1.2).
[0014] Preferably, there is no special requirement for the source of the hyperbranched polyquaternary ammonium amino acid. In one embodiment of the present invention, the hyperbranched polyquaternary ammonium amino acid is prepared according to the method of Example 1 in the authorization announcement number CN112080259B.
[0015] Preferably, the chitosan quaternary ammonium salt is chitosan quaternary ammonium salt HACC-102, which is provided by Xi'an Jushengyuan Biotechnology Co., Ltd.
[0016] Preferably, the alkali solution is any one of an aqueous solution of sodium hydroxide, an aqueous solution of potassium hydroxide, an aqueous solution of sodium carbonate, and an aqueous solution of potassium carbonate.
[0017] Preferably, the concentration of the alkali solution is 0.1-0.5 mol / L.
[0018] Preferably, the vegetable oil is at least one of peanut oil, safflower oil, rapeseed oil and corn oil.
[0019] Preferably, the mass ratio of the aqueous dispersion system to the oil phase in step S3 is 1:(80-100).
[0020] Preferably, the cleaning in step S4 is specifically as follows: first, ultrasonic cleaning is performed using petroleum ether for 2-4 minutes, then ultrasonic cleaning is performed using fully pre-cooled acetone for 3-5 minutes, and then ultrasonic cleaning is performed using water for 5-8 minutes; finally, ultrasonic cleaning is performed using anhydrous ethanol for 3-5 minutes; and microwave assistance is used during the ultrasonic cleaning process.
[0021] Preferably, the frequency of the microwave is 1.8-2.4 GHz, and the power ranges from 400-1000 W.
[0022] Preferably, the ultrasonic frequency of the ultrasonic cleaning is 35-60kHz, and the power range is 150-320W.
[0023] Preferably, the supercritical drying fluid in step S5 is carbon dioxide, the pressure is 9-16 MPa, the temperature is 30°C to 50°C, the fluid flow rate is 900 to 1500 L / h, and the supercritical drying time (heat preservation and pressure holding time) is 15 to 45 min.
[0024] Preferably, the sterilization treatment in step S5 is ultraviolet sterilization, using a suspended ultraviolet lamp with a power of 30-40 W for direct irradiation, the microcarriers are irradiated within a distance of 30 cm, and the irradiation time is 25-35 min.
[0025] Due to the application of the above technical solution, the present invention has the following beneficial effects:
[0026] (1) The method for producing porous microcarriers disclosed in the present invention has simple process, convenient operation and control, small impact on the environment, low dependence on equipment, low energy consumption, high preparation efficiency and finished product qualification rate, is suitable for industrial continuous production, and has high promotion and application value.
[0027] (2) The porous microcarrier disclosed in the present invention uses non-toxic and harmless materials such as hyperbranched polyquaternary ammonium amino acids, chitosan quaternary ammonium salts, and sodium alginate as raw materials, which can effectively avoid toxicity caused by the raw materials, give the product good biocompatibility and tissue compatibility, and reduce the impact of the preparation process on the environment; the quaternary ammonium salt structure on the hyperbranched polyquaternary ammonium amino acids and chitosan quaternary ammonium salts can undergo ion exchange reaction with sodium alginate to form an ion cross-linked structure, which can enhance the mechanical properties of the microspheres and improve the cell affinity of the microspheres. The porous microspheres are prepared by combining these raw materials for the first time, and the hyperbranched polyamino acids, chitosan, organic salts and alginic acid structures are introduced at the same time. The interaction between them can improve the particle size and pore size stability of the porous microcarriers; in the process of culturing cells, the cells can not only adhere to the carrier surface, but also enter the internal pores to grow, and form effective cell-cell connections in three-dimensional space, realizing true three-dimensional culture, increasing the cell culture area, and being conducive to protecting cells.
[0028] (3) The porous microcarrier disclosed in the present invention uses vegetable oil as the oil phase, which not only has abundant raw material sources and low cost, but also has good safety and will not introduce biological toxicity. Microwave assistance is used in the cleaning process of the microcarrier to improve the cleaning efficiency, improve the porous structure and structural stability, reduce the residual organic components, and avoid the impact on subsequent use.
[0029] (4) The porous microcarrier disclosed in the present invention is dried and sterilized by supercritical drying and ultraviolet light sterilization, which reduces energy consumption, avoids the problems of microcarrier agglomeration, incomplete drying, and affecting the stability of the pore structure caused by inappropriate temperature selection, and keeps the porous structure intact. Through the reasonable selection of each step and process parameter of the production method, they cooperate with each other to give the product a large specific surface area, good mechanical properties, and the porous structure of the microcarrier is kept intact during the production process, without the need for high temperature or freeze-dehydration drying. DETAILED DESCRIPTION
[0030] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art may think of other obvious variations.
[0031] Example 1
[0032] A method for producing a porous microcarrier comprises the following steps:
[0033] Step S1, preparation of aqueous dispersion: adding hyperbranched polyquaternary ammonium amino acid and chitosan quaternary ammonium salt into alkali solution, dispersing them evenly at 50° C., then adding sodium alginate thereto, and continuing to stir and react for 1 hour to obtain an aqueous dispersion;
[0034] Step S2, selecting the oil phase: taking vegetable oil as the oil phase;
[0035] Step S3, preparation of W / O emulsion: mixing the aqueous phase dispersion prepared in step S1 with the oil phase, and emulsifying with an emulsifier at room temperature to obtain a W / O emulsion;
[0036] Step S4, collecting microcarriers: stirring the W / O emulsion prepared in step S3 at room temperature for 5-10 hours, filtering out the upper organic phase, collecting microcarriers, and washing the collected microcarriers;
[0037] Step S5, supercritical drying and sterilization: The cleaned microcarriers are subjected to supercritical drying and then sterilized to obtain porous microcarriers.
[0038] The mass ratio of the hyperbranched polyquaternary ammonium amino acid, chitosan quaternary ammonium salt, alkali solution and sodium alginate in step S1 is 3:1:15:0.8; the hyperbranched polyquaternary ammonium amino acid is prepared according to the method of Example 1 in the authorization announcement number CN112080259B; the chitosan quaternary ammonium salt is chitosan quaternary ammonium salt HACC-102, which is provided by Xi'an Jushengyuan Biotechnology Co., Ltd.
[0039] The alkali solution is an aqueous solution of sodium hydroxide; the concentration of the alkali solution is 0.1 mol / L; the vegetable oil is peanut oil; the mass ratio of the aqueous phase dispersion system to the oil phase in step S3 is 1:80; the cleaning in step S4 is specifically as follows: first, ultrasonic cleaning is performed using petroleum ether for 2 minutes, then ultrasonic cleaning is performed using fully pre-cooled acetone for 3 minutes, and then ultrasonic cleaning is performed using water for 5 minutes; finally, ultrasonic cleaning is performed using anhydrous ethanol for 3 minutes; microwave assistance is used during the ultrasonic cleaning process; the frequency of the microwave is 1.8 GHz, and the power is 400 W; the ultrasonic frequency of the ultrasonic cleaning is 35 kHz, and the power is 150 W.
[0040] The supercritical drying fluid in step S5 is carbon dioxide, the pressure is 9 MPa, the temperature is 30°C, the fluid flow rate is 900 L / h, and the supercritical drying time (time for keeping warm and keeping pressure) is 45 min; the sterilization treatment in step S5 is ultraviolet sterilization, and a suspended ultraviolet lamp with a power of 30 W is used for direct irradiation. The microcarrier is irradiated within a distance of 30 cm, and the irradiation time is 25 min.
[0041] After testing, the porous microcarrier produced by the above-mentioned porous microcarrier production method has a surface pore size of 22 μm, a porosity of 95.9%, and a mechanical strength of 335 kPa.
[0042] Example 2
[0043] A method for producing a porous microcarrier comprises the following steps:
[0044] Step S1, preparation of aqueous dispersion: adding hyperbranched polyquaternary ammonium amino acid and chitosan quaternary ammonium salt into alkaline solution, dispersing them evenly at 53° C., then adding sodium alginate thereto, and continuing to stir and react for 2 hours to obtain an aqueous dispersion;
[0045] Step S2, selecting the oil phase: taking vegetable oil as the oil phase;
[0046] Step S3, preparation of W / O emulsion: mixing the aqueous phase dispersion prepared in step S1 with the oil phase, and emulsifying with an emulsifier at room temperature to obtain a W / O emulsion;
[0047] Step S4, collecting microcarriers: stirring the W / O emulsion prepared in step S3 at room temperature for 5-10 hours, filtering out the upper organic phase, collecting microcarriers, and washing the collected microcarriers;
[0048] Step S5, supercritical drying and sterilization: The cleaned microcarriers are subjected to supercritical drying and then sterilized to obtain porous microcarriers.
[0049] The mass ratio of the hyperbranched polyquaternary ammonium amino acid, chitosan quaternary ammonium salt, alkali solution and sodium alginate in step S1 is 3.5:1:17:0.9; the hyperbranched polyquaternary ammonium amino acid is prepared according to the method of Example 1 in the authorization announcement number CN112080259B; the chitosan quaternary ammonium salt is chitosan quaternary ammonium salt HACC-102, provided by Xi'an Jushengyuan Biotechnology Co., Ltd.; the alkali solution is an aqueous solution of potassium hydroxide; the concentration of the alkali solution is 0.2 mol / L; the vegetable oil is safflower oil.
[0050] The mass ratio of the aqueous phase dispersion system to the oil phase in step S3 is 1:85; the cleaning in step S4 is specifically as follows: first, ultrasonic cleaning is performed using petroleum ether for 2.5 minutes, then ultrasonic cleaning is performed using fully precooled acetone for 3.5 minutes, and then ultrasonic cleaning is performed using water for 6 minutes; finally, ultrasonic cleaning is performed using anhydrous ethanol for 3.5 minutes; microwave assistance is used during the ultrasonic cleaning process; the frequency of the microwave is 2 GHz, and the power is 600 W; the ultrasonic frequency of the ultrasonic cleaning is 45 kHz, and the power is 200 W.
[0051] The supercritical drying fluid in step S5 is carbon dioxide, the pressure is 11MPa, the temperature is 35°C, the fluid flow rate is 1100L / h, and the supercritical drying time (time for keeping warm and keeping pressure) is 35min; the sterilization treatment in step S5 is ultraviolet sterilization, and a suspended ultraviolet lamp with a power of 33W is used for direct irradiation. The microcarrier is irradiated within a distance of 30cm, and the irradiation time is 27min.
[0052] After testing, the porous microcarrier produced by the above-mentioned porous microcarrier production method has a surface pore size of 25 μm, a porosity of 97.1%, and a mechanical strength of 331 kPa.
[0053] Example 3
[0054] A method for producing a porous microcarrier comprises the following steps:
[0055] Step S1, preparation of aqueous dispersion: adding hyperbranched polyquaternary ammonium amino acid and chitosan quaternary ammonium salt into alkali solution, dispersing them evenly at 55° C., then adding sodium alginate thereto, and continuing to stir and react for 3 hours to obtain an aqueous dispersion;
[0056] Step S2, selecting the oil phase: taking vegetable oil as the oil phase;
[0057] Step S3, preparation of W / O emulsion: mixing the aqueous phase dispersion prepared in step S1 with the oil phase, and emulsifying with an emulsifier at room temperature to obtain a W / O emulsion;
[0058] Step S4, collecting microcarriers: stirring the W / O emulsion prepared in step S3 at room temperature for 7.5 hours, filtering out the upper organic phase, collecting microcarriers, and washing the collected microcarriers;
[0059] Step S5, supercritical drying and sterilization: The cleaned microcarriers are subjected to supercritical drying and then sterilized to obtain porous microcarriers.
[0060] The mass ratio of the hyperbranched polyquaternary ammonium amino acid, chitosan quaternary ammonium salt, alkali solution and sodium alginate in step S1 is 4:1:20:1; the hyperbranched polyquaternary ammonium amino acid is prepared according to the method of Example 1 in the authorization announcement number CN112080259B; the chitosan quaternary ammonium salt is chitosan quaternary ammonium salt HACC-102, provided by Xi'an Jushengyuan Biotechnology Co., Ltd.; the alkali solution is an aqueous solution of sodium carbonate; the concentration of the alkali solution is 0.3 mol / L; the vegetable oil is mustard seed oil.
[0061] The mass ratio of the aqueous phase dispersion system to the oil phase in step S3 is 1:90; the cleaning in step S4 is specifically as follows: first, ultrasonic cleaning is performed using petroleum ether for 3 minutes, then ultrasonic cleaning is performed using fully precooled acetone for 4 minutes, and then ultrasonic cleaning is performed using water for 6.5 minutes; finally, ultrasonic cleaning is performed using anhydrous ethanol for 4 minutes; microwave assistance is used during the ultrasonic cleaning process; the frequency of the microwave is 2.1 GHz, and the power is 700 W; the ultrasonic frequency of the ultrasonic cleaning is 50 kHz, and the power is 260 W.
[0062] The supercritical drying fluid in step S5 is carbon dioxide, the pressure is 13MPa, the temperature is 40°C, the fluid flow rate is 1200L / h, and the supercritical drying time (time for keeping warm and keeping pressure) is 25min; the sterilization treatment in step S5 is ultraviolet sterilization, and a suspended ultraviolet lamp with a power of 35W is used for direct irradiation. The microcarrier is irradiated within a distance of 30cm, and the irradiation time is 30min.
[0063] After testing, the porous microcarrier produced by the above-mentioned porous microcarrier production method has a surface pore size of 20 μm, a porosity of 98.5%, and a mechanical strength of 325 kPa.
[0064] Example 4
[0065] A method for producing a porous microcarrier comprises the following steps:
[0066] Step S1, preparation of aqueous dispersion: adding hyperbranched polyquaternary ammonium amino acid and chitosan quaternary ammonium salt into alkali solution, dispersing them evenly at 58° C., then adding sodium alginate thereto, and continuing to stir and react for 4.5 hours to obtain an aqueous dispersion;
[0067] Step S2, selecting the oil phase: taking vegetable oil as the oil phase;
[0068] Step S3, preparation of W / O emulsion: mixing the aqueous phase dispersion prepared in step S1 with the oil phase, and emulsifying with an emulsifier at room temperature to obtain a W / O emulsion;
[0069] Step S4, collecting microcarriers: stirring the W / O emulsion prepared in step S3 at room temperature for 9 hours, filtering out the upper organic phase, collecting microcarriers, and washing the collected microcarriers;
[0070] Step S5, supercritical drying and sterilization: The cleaned microcarriers are subjected to supercritical drying and then sterilized to obtain porous microcarriers.
[0071] The mass ratio of the hyperbranched polyquaternary ammonium amino acid, chitosan quaternary ammonium salt, alkali solution and sodium alginate in step S1 is 4.5:1:24:1.1; the hyperbranched polyquaternary ammonium amino acid is prepared according to the method of Example 1 in the authorization announcement number CN112080259B; the chitosan quaternary ammonium salt is chitosan quaternary ammonium salt HACC-102, provided by Xi'an Jushengyuan Biotechnology Co., Ltd.; the alkali solution is an aqueous solution of potassium carbonate; the concentration of the alkali solution is 0.4 mol / L; the vegetable oil is a mixture of peanut oil, safflower oil, mustard seed oil and corn oil mixed in a mass ratio of 1:1:2:3.
[0072] The mass ratio of the aqueous phase dispersion system to the oil phase in step S3 is 1:95; the cleaning in step S4 is specifically as follows: first, ultrasonic cleaning is performed using petroleum ether for 3.5 minutes, then ultrasonic cleaning is performed using fully precooled acetone for 4.5 minutes, and then ultrasonic cleaning is performed using water for 7 minutes; finally, ultrasonic cleaning is performed using anhydrous ethanol for 4.5 minutes; microwave assistance is used during the ultrasonic cleaning process; the frequency of the microwave is 2.3 GHz, and the power is 900 W; the ultrasonic frequency of the ultrasonic cleaning is 55 kHz, and the power is 300 W.
[0073] The supercritical drying fluid in step S5 is carbon dioxide, the pressure is 15MPa, the temperature is 45°C, the fluid flow rate is 1400L / h, and the supercritical drying time (time for keeping warm and keeping pressure) is 20min; the sterilization treatment in step S5 is ultraviolet sterilization, and a suspended ultraviolet lamp with a power of 38W is used for direct irradiation. The microcarrier is irradiated within a distance of 30cm, and the irradiation time is 33min.
[0074] After testing, the porous microcarrier produced by the above-mentioned porous microcarrier production method has a surface pore size of 18 μm, a porosity of 98.3%, and a mechanical strength of 329 kPa.
[0075] Example 5
[0076] A method for producing a porous microcarrier comprises the following steps:
[0077] Step S1, preparation of aqueous dispersion: adding hyperbranched polyquaternary ammonium amino acid and chitosan quaternary ammonium salt into alkali solution, dispersing them evenly at 60° C., then adding sodium alginate thereto, and continuing to stir and react for 5 hours to obtain an aqueous dispersion;
[0078] Step S2, selecting the oil phase: taking vegetable oil as the oil phase;
[0079] Step S3, preparation of W / O emulsion: mixing the aqueous phase dispersion prepared in step S1 with the oil phase, and emulsifying with an emulsifier at room temperature to obtain a W / O emulsion;
[0080] Step S4, collecting microcarriers: stirring the W / O emulsion prepared in step S3 at room temperature for 10 hours, filtering out the upper organic phase, collecting microcarriers, and washing the collected microcarriers;
[0081] Step S5, supercritical drying and sterilization: The cleaned microcarriers are subjected to supercritical drying and then sterilized to obtain porous microcarriers.
[0082] The mass ratio of the hyperbranched polyquaternary ammonium amino acid, chitosan quaternary ammonium salt, alkali solution and sodium alginate in step S1 is 5:1:25:1.2; the hyperbranched polyquaternary ammonium amino acid is prepared according to the method of Example 1 in the authorization announcement number CN112080259B; the chitosan quaternary ammonium salt is chitosan quaternary ammonium salt HACC-102, provided by Xi'an Jushengyuan Biotechnology Co., Ltd.; the alkali solution is an aqueous solution of sodium hydroxide; the concentration of the alkali solution is 0.5 mol / L; the vegetable oil is corn oil.
[0083] The mass ratio of the aqueous phase dispersion system to the oil phase in step S3 is 1:100; the cleaning in step S4 is specifically as follows: first, ultrasonic cleaning is performed using petroleum ether for 4 minutes, then ultrasonic cleaning is performed using fully precooled acetone for 5 minutes, and then ultrasonic cleaning is performed using water for 8 minutes; finally, ultrasonic cleaning is performed using anhydrous ethanol for 5 minutes; microwave assistance is used during the ultrasonic cleaning process; the frequency of the microwave is 2.4 GHz, and the power is 1000 W; the ultrasonic frequency of the ultrasonic cleaning is 60 kHz, and the power range is 320 W.
[0084] The supercritical drying fluid in step S5 is carbon dioxide, the pressure is 16MPa, the temperature is 50°C, the fluid flow rate is 1500L / h, and the supercritical drying time (time for keeping warm and keeping pressure) is 15min; the sterilization treatment in step S5 is ultraviolet sterilization, and a suspended ultraviolet lamp with a power of 40W is used for direct irradiation. The microcarrier is irradiated within a distance of 30cm, and the irradiation time is 35min.
[0085] After testing, the porous microcarrier produced by the above-mentioned porous microcarrier production method has a surface pore size of 20 μm, a porosity of 99.0%, and a mechanical strength of 320 kPa.
[0086] Comparative Example 1
[0087] This example provides a method for producing porous microcarriers, which is basically the same as Example 1, except that chitosan quaternary ammonium salt is not added.
[0088] After testing, the porous microcarrier produced by the above-mentioned porous microcarrier production method has a surface pore size of 30 μm, a porosity of 94.7%, and a mechanical strength of 312 kPa.
[0089] Comparative Example 2
[0090] This example provides a method for producing porous microcarriers, which is basically the same as Example 1, except that freeze drying is used instead of supercritical drying. The freeze drying is specifically as follows: first pre-freeze in a -20°C freezer, and then transfer to a freeze dryer at -40°C for freeze drying for 24 hours.
[0091] After testing, the porous microcarrier produced by the above-mentioned porous microcarrier production method has a surface pore size of 33 μm, a porosity of 94.0%, and a mechanical strength of 315 kPa.
[0092] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the contents of the present invention and implement them accordingly. They cannot be used to limit the protection scope of the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for producing a porous microcarrier, characterized in that: The steps include: Step S1, preparation of an aqueous dispersion system: adding a hyperbranched polyquaternary ammonium amino acid and a chitosan quaternary ammonium salt to an alkali solution, dispersing them uniformly at 50-60° C., and then adding sodium alginate thereto, and continuing to stir and react for 1-5 hours to obtain an aqueous dispersion system; the mass ratio of the hyperbranched polyquaternary ammonium amino acid, the chitosan quaternary ammonium salt, the alkali solution, and the sodium alginate is (3-5):1:(15-25):(0.8-1.2); Step S2, selecting the oil phase: taking vegetable oil as the oil phase; Step S3, preparation of W / O emulsion: mixing the aqueous dispersion prepared in step S1 with the oil phase, and emulsifying with an emulsifier at room temperature to obtain a W / O emulsion; the mass ratio of the aqueous dispersion to the oil phase is 1:(80-100); Step S4, collecting microcarriers: stirring the W / O emulsion prepared in step S3 at room temperature for 5-10 hours, filtering out the upper organic phase, collecting microcarriers, and washing the collected microcarriers; the washing specifically comprises: firstly using petroleum ether for ultrasonic washing for 2-4 minutes, then using fully pre-cooled acetone for ultrasonic washing for 3-5 minutes, then using water for ultrasonic washing for 5-8 minutes; finally using anhydrous ethanol for ultrasonic washing for 3-5 minutes; microwaves are used to assist in the ultrasonic washing process; the frequency of the microwaves is 1.8-2.4 GHz, and the power range is 400-1000 W; the ultrasonic frequency of the ultrasonic washing is 35-60 kHz, and the power range is 150-320 W; Step S5, supercritical drying and sterilization: The cleaned microcarriers are subjected to supercritical drying and then sterilized to obtain porous microcarriers.
2. The method for producing porous microcarriers according to claim 1, characterized in that: The alkali solution is any one of an aqueous solution of sodium hydroxide, an aqueous solution of potassium hydroxide, an aqueous solution of sodium carbonate, and an aqueous solution of potassium carbonate; and the concentration of the alkali solution is 0.1-0.5 mol / L.
3. The method for producing porous microcarriers according to claim 1, characterized in that: The vegetable oil is at least one of peanut oil, safflower oil, rapeseed oil and corn oil.
4. The method for producing porous microcarriers according to claim 1, characterized in that: The supercritical drying fluid in step S5 is carbon dioxide, the pressure is 9-16 MPa, the temperature is 30° C. to 50° C., the fluid flow rate is 900 to 1500 L / h, and the supercritical drying time is 15 to 45 min.
5. The method for producing porous microcarriers according to claim 1, characterized in that: The sterilization treatment in step S5 is ultraviolet sterilization, using a suspended ultraviolet lamp with a power of 30-40W for direct irradiation, the microcarriers are irradiated within a distance of 30cm, and the irradiation time is 25-35min.