Low-carbon emission and high-toughness PCR HIPS modified material and preparation method thereof

By using ingredients such as copolymers containing glycidyl methacrylate and/or octenyl in PCR HIPS materials, combined with HIPS and fillers, the problems of slippage and loosening of PCR HIPS materials in locking screw applications are solved, achieving It comprehensively improves the performance of low carbon emissions, high toughness and high resistance to locking screws.

CN118006068BActive Publication Date: 2024-10-15GUANGDONG GUOHENG YOUHE ADVANCED MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410094006.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-23
Publication Date
2024-10-15
Estimated Expiration
2044-01-23

AI Technical Summary

Technical Problem

Recycled PCR HIPS materials are prone to problems of screw slipping and loosening when used in products that require locking screws or snap fastenings, and existing improvement methods cannot effectively improve mechanical properties while reducing carbon emissions.

Method used

Use copolymers containing glycidyl methacrylate and/or octenyl as compatibilizer, combined with HIPS, tougheners and fillers, to improve the compatibility and mechanical properties of the material through compatibilizers and silane coupling agents , use lubricants to reduce friction, antioxidants to improve anti-aging properties, and prepare low-carbon emission and high-toughness PCR HIPS modified materials.

Benefits of technology

It significantly improves the impact strength, toughness and screw-lock resistance of PCR HIPS modified materials, reduces carbon emissions, is suitable for applications requiring high screw-lock resistance, and improves the overall performance stability of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004677912670000021
    Figure BDA0004677912670000021
  • Figure BDA0004677912670000071
    Figure BDA0004677912670000071
  • Figure BDA0004677912670000081
    Figure BDA0004677912670000081
Patent Text Reader

Abstract

The present application relates to the field of recycled HIPS materials, and discloses a low-carbon emission high-toughness PCR HIPS modified material and its preparation method. A low-carbon emission high-toughness PCR HIPS modified material is prepared from the following raw materials in parts by weight: PCR HIPS 50‑95%, HIPS 0.5‑37%, filler 0.5‑10%, toughening agent 1‑8%, compatibilizer 0.5‑5%, lubricant 1‑3%, antioxidant 0.1‑2%, silane coupling agent 0.1‑0.3%; the compatibilizer is a copolymer containing glycidyl methacrylate and / or octenyl; preparation method: raw material mixing, melt extrusion, cooling, drying, and pelletizing. The prepared PCR HIPS modified material has good impact resistance and toughness, and is not easy to loosen or slip when used in a locking screw structure. Compared with the use of HIPS, the carbon reduction ratio is between 72.1% and 86.6%, which meets the carbon emission requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of recycled HIPS materials, and more specifically, to a low-carbon emission, high-toughness PCRHIPS modified material and a preparation method thereof. Background Art

[0002] High impact polystyrene, referred to as HIPS, is a polystyrene-modified non-crystalline material with high impact strength modified by synthetic rubber. It has good impact strength, toughness, material rigidity and processing performance. It is widely used in electronic appliances, optical lighting, mechanical equipment, building materials industry and other fields.

[0003] With the continuous development of the national economy and the continuous tightening of low-carbon emission policies, the requirements for low-carbon emission indicators for chemical materials are becoming higher and higher. In order to improve the utilization efficiency of high HIPS, HIPS has gradually begun to be recycled and reused as recycled HIPS material, referred to as PCR HIPS, to reduce carbon emissions.

[0004] However, since HIPS products will age during use, resulting in a decline in product performance, and auxiliary materials such as ABS, PP or PE are added during the production of HIPS products, the impurity composition of the recycled PCR HIPS is relatively complex, which makes the mechanical properties of the recycled PCR HIPS prone to degradation during use. This is especially true for PCR HIPS products that require screw locking or clip fastening, such as mice and keyboards. When locking, the screws are prone to slippage and loosening, reducing the performance of the PCR HIPS products.

[0005] At present, in order to improve the problem of screw stripping and loosening that easily occurs during the application of recycled PCR HIPS, some technologies will add materials such as SBS or SEBS to the PCR HIPS material to improve the mechanical properties of the prepared PCR HIPS product, but the improvement of the mechanical properties of the prepared PCR HIPS product is limited. There are also some technologies that reduce the usage of PCR HIPS materials to improve the mechanical properties of the prepared PCR HIPS products. However, after reducing the usage of PCR HIPS materials, the carbon emissions of PCR HIPS will increase, and low-carbon emissions cannot be achieved well, which will limit the subsequent application of the recycled PCR HIPS material. Therefore, the inventor believes that further research is needed on the current PCRHIPS material. Summary of the invention

[0006] In order to solve the problem of screw slippage or loosening when recycled PCR HIPS materials are used in PCR HIPS products that require screw locking or snap fastening, the present application provides a low-carbon emission and high-toughness PCR HIPS modified material and a preparation method thereof.

[0007] In the first aspect, the present application provides a PCR HIPS modified material with low carbon emission and high toughness, which adopts the following technical solution:

[0008] A low-carbon emission and high-toughness PCR HIPS modified material is prepared from the following raw materials in parts by weight:

[0009]

[0010] The compatibilizer is a copolymer containing glycidyl methacrylate and / or octenyl.

[0011] By adopting the above technical scheme, the low-carbon emission and high-toughness PCR HIPS modified material of the present application uses PCR HIPS as the main material, and HIPS is added to PCR HIPS. HIPS has high impact strength and toughness, and can be well compounded with the toughening agent to further improve the impact strength and toughness of the prepared PCR HIPS modified material. The filler plays a good role in reinforcing the mechanical properties of PCR HIPS, and can further improve the material rigidity and hardness of PCR HIPS, so that the prepared PCR HIPS modified material has good impact strength and toughness, and can also have good hardness, reducing the occurrence of slipping teeth, and the compatibilizer and silane coupling agent play a role in further improving PCR The compatibility of HIPS, HIPS, toughening agent and filler makes each component evenly dispersed and compatible, further improving the mechanical properties of PC HIPS. The compatibility agent used in this application is a copolymer containing glycidyl methacrylate and / or octenyl. The glycidyl methacrylate and / or octenyl groups contained in these substances can be well compatible with the impurity components (such as ABS, PP, PE, etc.) in PC HIPS, making the fusion structure between PCR HIPS, HIPS, toughening agent and filler tighter, thereby further improving the toughness and strength of the prepared PCR HIPS modified material, and improving the screw locking resistance of the PCR HIPS modified material; the lubricant plays a role in reducing the friction between the components, so that the components can be evenly mixed and melted, further improving the material properties of the prepared PCR HIPS modified material, and the antioxidant plays a role in improving the anti-aging performance of the prepared PCR HIPS modified material. Therefore, the PCR prepared in this application HIPS modified material has good resistance to screw locking and is used in locking structures such as mice and keyboards that require screw locking. It is not prone to loosening or slipping. At the same time, since PCR HIPS is used as the main material, the PCR HIPS modified material has lower carbon emissions.

[0012] In summary, the PCR HIPS modified material prepared in this application meets the requirements of energy conservation and emission reduction, can realize the quantification of PCR HIPS carbon emissions, and also has good impact resistance, toughness and material strength. It is suitable for application places with high requirements for screw locking resistance and has a wide range of applications.

[0013] Preferably, the compatibilizer is prepared from the following raw materials in parts by weight:

[0014] Styrene-octene-glycidyl methacrylate copolymer 20-30 parts

[0015] 14-24 parts of styrene-acrylonitrile-glycidyl methacrylate copolymer

[0016] Styrene grafted maleic anhydride 5-10 parts

[0017] 2-4 parts of long chain alkyl silane coupling agent

[0018] 3-8 parts of polycaprolactone triol.

[0019] By adopting the above technical scheme, styrene-octene-glycidyl methacrylate copolymer can better improve the compatibility of impurity components in PCR HIPS with HIPS, toughening agent, compatibilizer and filler. Styrene-acrylonitrile-glycidyl methacrylate copolymer has better impact strength and heat resistance than polystyrene. It also contains glycidyl methacrylate group, so it can improve the mechanical properties of the prepared PCR HIPS while further improving the compatibility of impurity components in PCR HIPS with HIPS, toughening agent, compatibilizer and filler. Styrene grafted maleic anhydride improves the thermal stability of styrene and also improves the flexibility of styrene. Styrene grafted maleic anhydride is added as a compatibilizer in this application, which can further improve the prepared PCR The flexibility of HIPS modified materials is improved, and polycaprolactone triol is used as a plasticizer. Polycaprolactone triol is a three-branched molecular structure containing terminal hydroxyl groups. The long-chain alkyl silane coupling agent has a long carbon chain structure, which can produce a good compounding effect with polycaprolactone triol, and improve the blending uniformity of styrene-octene-glycidyl methacrylate copolymer, styrene-acrylonitrile-glycidyl methacrylate copolymer and styrene grafted maleic anhydride, thereby improving the processing stability. Therefore, the above five raw materials are compounded to prepare a compatibilizer, and the five have a good synergistic effect. The compatibilizer prepared in this way can better improve the compatibility between the raw materials. The molecular structures of the prepared PCRHIPS modified materials are intertwined, with good density, good rigidity and hardness, as well as good impact resistance and toughness.

[0020] Preferably, the compatibilizer is prepared by the following steps: adding styrene-octene-glycidyl methacrylate copolymer, styrene-acrylonitrile-glycidyl methacrylate copolymer, styrene grafted maleic anhydride, long-chain alkyl silane coupling agent and polycaprolactone triol into a reaction device, mixing evenly, heating and melt extruding, cooling, and granulating to obtain the compatibilizer.

[0021] By adopting the above technical scheme, the above raw materials are uniformly mixed, then melt-extruded, cooled and granulated, so as to prepare a compatibilizer with stable performance.

[0022] Preferably, the toughening agent is SBS and / or SEBS.

[0023] By adopting the above technical solution, SBS is a styrene-butadiene-styrene copolymer, which is a thermoplastic elastomer material, in which styrene forms a glassy hard segment, and butadiene forms an elastic soft segment. Therefore, SBS has both the rigidity and strength of the hard segment and the elasticity and toughness of the soft segment; SEBS is a linear triblock copolymer with polystyrene as the terminal segment and ethylene-butene copolymer obtained by hydrogenation of polybutadiene as the middle elastic block. It has good strength as well as good elasticity and wear resistance. Therefore, using SBS and / or SEBS as a toughening agent can play a good toughening role on PCR HIPS, thereby improving the strength and toughness of the obtained PCR HIPS modified material.

[0024] Preferably, the filler is prepared by the following steps:

[0025] Add 60-80 parts of powder filler, 4-8 parts of polyethylene glycol diglycidyl ether and 2-5 parts of n-octyl triethoxy silane into a kneading device, knead and stir to obtain a filler;

[0026] The powder filler is one or a mixture of wollastonite, kaolin, barium sulfate, talc and mica.

[0027] By adopting the above technical scheme, in order to further improve the compatibility of the filler and reduce the situation where the toughness of the prepared PCR HIPS is reduced due to the increase in hardness, the filler is optimized, wherein the polyethylene glycol diglycidyl ether has a soft long-chain ether group segment, which can fully infiltrate the powder filler, so that the powder filler is evenly dispersed, and the modification efficiency of the powder filler by n-octyltriethoxysilane is improved. N-octyltriethoxysilane has a long-chain octyl group and three ethoxy groups. Under the synergistic effect of polyethylene glycol diglycidyl ether, it can well modify the powder filler of the present application, and improve the dispersion effect and compatibility of the powder filler in PCR HIPS. The powder filler prepared in this way can not only better improve the strength and hardness of the prepared PCR HIPS modified material, but also better improve the toughness and impact resistance of the PCR HIPS modified material.

[0028] Preferably, the lubricant is one or more combinations of pentaerythritol stearate, ethylene bisstearamide, zinc stearate, and triphenyl phosphate.

[0029] By adopting the above technical solution, the lubricant has good lubricity, can reduce the friction between the raw materials of PCR HIPS, HIPS, toughening agent and filler, so that each raw material is fully dispersed and evenly melted, and the comprehensive performance of the prepared PCR HIPS modified material is improved.

[0030] Preferably, the silane coupling agent is any one of γ-(2,3-epoxypropoxy)propyltrimethoxysilane and γ-aminopropyltriethoxysilane.

[0031] By adopting the above technical solution, the above silane coupling agent can play a better compounding role with the compatibilizer, further improving the compatibility of the filler, PCR HIPS, HIPS and toughening agent.

[0032] Preferably, the antioxidant consists of antioxidant 1010 and antioxidant 168 in a weight ratio of 1:(1.5-2.5).

[0033] By adopting the above technical solution, the above antioxidants are compounded and used, which has a good synergistic effect, can better improve the antioxidant properties of the prepared PCR HIPS modified material, make the PCR HIPS modified material have better anti-aging performance, and improve the application life.

[0034] In the second aspect, the present application provides a method for preparing a low-carbon emission and high-toughness PCR HIPS modified material, using the following technical solution:

[0035] A method for preparing a low-carbon emission and high-toughness PCR HIPS modified material comprises the following preparation steps:

[0036] S1, baking the PCR HIPS raw material to obtain the PCR HIPS processed material;

[0037] S2, adding PCR HIPS processing material, HIPS, toughening agent, compatibilizer and silane coupling agent into a reaction device, stirring evenly, to obtain a mixture A;

[0038] S3, adding filler, lubricant and antioxidant to mixture A, stirring evenly to prepare PCR HIPS mixture;

[0039] S4, melt-extrude the PCR HIPS mixture, cool, dry and pelletize to obtain a PCR HIPS modified material.

[0040] By adopting the above technical scheme, PCR HIPS is first baked to remove water molecules and low-boiling impurities in PCR HIPS, and the PCR HIPS processed material is formed after baking. Then HIPS, toughening agent, compatibilizer and silane coupling agent are added to the PCR HIPS processed material, mixed and stirred to make the components evenly dispersed and mixed, and then filler, lubricant and antioxidant are added. Under the further action of lubricant and silane coupling agent, the raw materials are further compatible to form a PCR HIPS mixture with uniform dispersion and dense structure. Then the PCR HIPS mixture is melt-extruded, cooled, dried and pelletized to obtain a PCR HIPS modified material with good mechanical properties.

[0041] Preferably, the baking temperature in step S1 is 70-80°C, and the baking time is 45-120 min; and the melting temperature in step S4 is 190-230°C.

[0042] By adopting the above technical scheme, the optimal baking temperature and time can volatilize the water molecules and low-boiling impurities in PC HIPS to the greatest extent possible, thereby improving the mechanical properties of the prepared PCR HIPS modified material. The optimal melting temperature enables the PCR HIPS mixture to be evenly melt-extruded, thereby improving the processing stability of the PCR HIPS modified material.

[0043] In summary, this application has the following beneficial effects:

[0044] 1. The low-carbon emission and high-toughness PCR HIPS modified material of the present application uses PCR HIPS as the main material, and HIPS and a toughening agent are added. HIPS and the toughening agent play a good compounding effect, which improves the impact strength and toughness of the prepared PCR HIPS modified material. The filler plays a good mechanical property reinforcement role on PCR HIPS, which can further improve the material rigidity and hardness of PCR HIPS, so that the prepared PCR HIPS modified material has good impact strength and toughness, and also has good hardness. The compatibilizer and silane coupling agent play a role in further improving the compatibility of PCR HIPS, HIPS, toughening agent and filler, so that each component can be evenly dispersed and compatible, and further improves the mechanical properties of PCR HIPS. The PCR HIPS modified material prepared in the present application has good impact strength and toughness, and thus has good screw locking resistance. It is used in locking structures such as mice and keyboards that require screw locking, and is not prone to loosening and slipping. At the same time, since PCR HIPS is used as the main material, the prepared PCR HIPS modified materials have lower carbon emissions and meet carbon emission requirements.

[0045] 2. A compatibilizer is prepared by compounding styrene-octene-glycidyl methacrylate copolymer, styrene-acrylonitrile-glycidyl methacrylate copolymer, styrene grafted maleic anhydride, a long-chain alkyl silane coupling agent and polycaprolactone triol. The five have a good synergistic effect. The compatibilizer prepared in this way can better improve the compatibility between the various raw materials. The obtained PCR HIPS modified material has a dense intermolecular structure, good rigidity and hardness, and also good impact resistance and toughness.

[0046] 3. The powder filler is modified by using polyethylene glycol diglycidyl ether and n-octyltriethoxysilane. The prepared filler can improve the strength and hardness of the prepared PCR HIPS modified material, and also has good toughness and impact resistance of the PCR HIPS modified material.

[0047] 4. The preparation method of the present application is simple, and the obtained low-carbon emission and high-toughness PCR HIPS has stable performance. DETAILED DESCRIPTION

[0048] The present application is further described in detail below with reference to the embodiments.

[0049] The following are the sources and specifications of some raw materials of this application. The raw materials in the preparation examples and embodiments of this application can be obtained from the market. The raw materials used in this application include but are not limited to the specific models and manufacturers disclosed below. Raw materials with the same specifications and performance can be used:

[0050] 1. PCR HIPS: commercially available, cantilever beam notched impact strength: 60 J / m, heat deformation temperature 75 ° C, tensile strength 19.2 MPa, plastic waste recycling by Heilongjiang Zhongzai Waste Appliance Dismantling Co., Ltd.;

[0051] 2. HIPS: MI range 2.0-10.0g / 10min, 200℃ / 5kg, Ningbo Formosa Chemical HIPS 8250;

[0052] 3. Styrene-octene-glycidyl methacrylate copolymer: Jiayirong brand, SOG-02;

[0053] 4. Styrene-acrylonitrile-glycidyl methacrylate copolymer: Jiayirong brand, SAG-005;

[0054] 5. Styrene grafted with maleic anhydride: maleic anhydride grafting rate 15-18%, glass transition temperature 120°C;

[0055] 6. Polycaprolactone triol: molecular weight 300-600, CAS number: 37625-56-2;

[0056] 7. Polyethylene glycol diglycidyl ether: epoxy value 0.56-0.67eg / 100g, density 1.14-1.16g / cm 3 ,CAS No.: 39443-66-8;

[0057] 8. Wollastonite: 1250 mesh, refractive index 1.62-1.64;

[0058] 9. Kaolin: 1250 mesh;

[0059] 10. Barium sulfate: 1250 mesh;

[0060] 11. Talc: 1250 mesh, silicon dioxide content 60-70%;

[0061] 12. SEBS: Brand: Kraton, styrene content 29-32%, model G1654;

[0062] 13. SBS: Brand: Kraton, styrene content: 35%, model: DX415JS.

[0063] Preparation Example of Compatibilizer

[0064] Preparation Example 1

[0065] Preparation Example 1 discloses a compatibilizer prepared by the following steps:

[0066] 2kg of styrene-octene-glycidyl methacrylate copolymer, 2.4kg of styrene-acrylonitrile-glycidyl methacrylate copolymer, 0.5kg of styrene grafted maleic anhydride, 0.2kg of dodecyltrimethoxysilane as a long-chain alkylsilane coupling agent and 0.3kg of polycaprolactone triol were mixed, stirred for 20 minutes at a stirring rate of 300r / min, and after stirring evenly, added into a twin-screw extruder, heated to 195°C, melt-extruded at a screw speed of 300r / min, then water-cooled, dried with hot air, and pelletized to obtain a compatibilizer.

[0067] Preparation Example 2-3

[0068] The difference between Preparation Example 2-3 and Preparation Example 1 is that the amount of raw materials used and the preparation conditions are different, see Table 1 below for details.

[0069] Table 1 Raw material dosage and preparation conditions of Preparation Examples 1-3

[0070]

[0071] Preparation Comparative Example 1

[0072] The difference between Preparation Comparative Example 1 and Preparation Example 1 is that an equal amount of styrene-octene-glycidyl methacrylate copolymer is replaced by styrene-acrylonitrile-glycidyl methacrylate copolymer, and the rest is the same as Preparation Example 1.

[0073] Preparation Comparative Example 2

[0074] The difference between Preparation Comparative Example 2 and Preparation Example 1 is that the polystyrene grafted maleic anhydride is replaced by an equal amount of polycaprolactone triol, and the rest is the same as Preparation Example 1.

[0075] Preparation Comparative Example 3

[0076] The difference between Preparation Comparative Example 3 and Preparation Example 1 is that an equal amount of styrene-acrylonitrile-glycidyl methacrylate copolymer is replaced with styrene-acrylonitrile (brand: Jiayirong, model: EMI-200), and the rest is the same as Preparation Example 1.

[0077] Preparation Comparative Example 4

[0078] The difference between Preparation Comparative Example 4 and Preparation Example 1 is that an equal amount of polycaprolactone triol is replaced by diallyl phthalate, and the rest is the same as Preparation Example 1.

[0079] Preparation Comparative Example 5

[0080] The difference between Preparation Example 5 and Preparation Example 1 is that the amount of styrene-octene-glycidyl methacrylate copolymer used is 3.5 kg, the amount of styrene-acrylonitrile-glycidyl methacrylate copolymer used is 0.5 kg, the amount of styrene grafted maleic anhydride used is 1 kg, and the rest is the same as Preparation Example 1.

[0081] Preparation Comparative Example 6

[0082] The difference between Preparation Comparative Example 6 and Preparation Example 1 is that the long-chain alkyl silane coupling agent is replaced with an equal amount of γ-aminopropyltriethoxysilane, and the rest is the same as Preparation Example 1.

[0083] Preparation Comparative Example 7

[0084] The difference between Preparation Comparative Example 7 and Preparation Example 1 is that the long-chain alkyl silane coupling agent is replaced by an equal amount of polycaprolactone triol, and the rest is the same as Preparation Example 1.

[0085] Preparation example of filler

[0086] Preparation Example 4

[0087] Preparation Example 4 discloses a filler prepared by the following steps:

[0088] 3.6 kg of kaolin and 2.4 kg of barium sulfate as powder fillers, 0.4 kg of polyethylene glycol diglycidyl ether and 0.2 kg of n-octyltriethoxysilane were added into a kneading device, kneaded for 20 minutes at a kneading rate of 400 r / min, and kneaded and stirred to obtain a filler;

[0089] Preparation Example 5-6

[0090] The difference between Preparation Example 5-6 and Preparation Example 4 is that the amount of raw materials used and the preparation conditions are different, see Table 2 below for details.

[0091] Table 2 Raw material dosage and preparation conditions of Preparation Examples 4-6

[0092]

[0093]

[0094] Preparation Comparative Example 8

[0095] The difference between Preparation Comparative Example 8 and Preparation Example 4 is that an equal amount of polyethylene glycol diglycidyl ether is replaced by n-octyltriethoxysilane, and the rest is the same as Preparation Example 4.

[0096] Preparation Comparative Example 9

[0097] The difference between Preparation Comparative Example 9 and Preparation Example 4 is that an equal amount of polyethylene glycol diglycidyl ether is replaced by polyethylene glycol 400, and the rest is the same as Preparation Example 4.

[0098] Example

[0099] Example 1

[0100] Example 1 discloses a low-carbon emission and high-toughness PCR HIPS modified material, which is prepared by the following steps:

[0101] S1. Bake 5 kg of PCR HIPS at 70° C. for 45 min to obtain PCR HIPS processed material;

[0102] S2, adding the above-prepared PCR HIPS processed material, 3.7 kg HIPS, 0.2 kg SEBS as a toughening agent, 0.5 kg styrene-octene-glycidyl methacrylate copolymer as a compatibilizer and 0.01 kg γ-(2,3-epoxypropoxy)propyltrimethoxysilane as a silane coupling agent into a reactor, stirring for 20 min, stirring evenly, to obtain a mixture A;

[0103] S3, adding 0.25 kg of commercially available filler (the filler consists of kaolin and barium sulfate in a weight ratio of 3:2), 0.3 kg of pentaerythritol stearate as a lubricant and 0.04 kg of antioxidant (consisting of antioxidant 1010 and antioxidant 168 in a weight ratio of 1:1.5) to mixture A, stirring for 30 minutes, stirring evenly, to obtain a PCR HIPS mixture;

[0104] S4. Add the PCR HIPS mixture into a twin-screw extruder, adjust the temperature of the twin-screw extruder, set the temperature of zone 1 to 190°C, the temperature of zone 2 to 210°C, the temperature of zone 3 to 220°C, the temperature of zone 4 to 230°C, the temperature of zone 5 to 220°C, the temperature of zone 6 to 210°C, the die temperature to 220°C, the screw speed to 300r / min, and perform water cooling and hot air drying after extrusion, and then pelletize to obtain a PCR HIPS modified material.

[0105] Example 2-3

[0106] The difference between Example 2-3 and Example 1 is that the amount of raw materials used and the preparation conditions are different, see Table 3 below for details.

[0107] Table 3 Raw material dosage and preparation conditions of Examples 1-3

[0108]

[0109]

[0110] Embodiment 4-13

[0111] The difference between Example 4-13 and Example 1 is that the source of the compatibilizer is different, see Table 4 below for details.

[0112] Table 4 Sources of compatibilizers in Examples 4-13

[0113]

[0114]

[0115] Embodiment 14

[0116] The difference between Example 14 and Example 4 is that the source of the filler is different, see Table 5 below for details.

[0117] Table 5 Sources of fillers for Examples 14-18

[0118] Example Source of filler Embodiment 14 Preparation Example 4 Embodiment 15 Preparation Example 5 Example 16 Preparation Example 6 Embodiment 17 Preparation Comparative Example 8 Embodiment 18 Preparation Comparative Example 9

[0119] Comparative Example

[0120] Comparative Example 1

[0121] The difference between Comparative Example 1 and Example 1 is that the compatibilizer is replaced by styrene grafted maleic anhydride in equal amount, and the rest is the same as Example 1.

[0122] Comparative Example 2

[0123] The difference between Comparative Example 2 and Example 1 is that the filler is replaced by a toughening agent in equal amount, and the other parts are the same as Example 1.

[0124] Comparative Example 3

[0125] The difference between Comparative Example 3 and Example 1 is that the compatibilizer is replaced by a toughening agent in equal amount, and the other parts are the same as Example 1.

[0126] Performance testing

[0127] The following is a performance test of the low-carbon emission and high-toughness PCR HIPS modified materials prepared in Examples 1-18 and Comparative Examples 1-3: The PCR HIPS modified materials prepared above were placed in an oven at 75° C. and baked for 90 minutes, and injection molded using an injection molding machine at a temperature of 220° C., and cut into test strips for testing:

[0128] (1) Impact strength test

[0129] According to the test standard of ASTM D256, the above test strips are subjected to the Izod notched impact strength test (unit: J / m), and the test results are tested and recorded;

[0130] (2) Bending strength test

[0131] According to the test standard of ASTM D790, the bending strength test (unit: MPa) of the above test strips was carried out, and the test results were recorded;

[0132] (3) Screw locking performance test:

[0133] The screw locking performance test was conducted using the screw locking test fixture disclosed in the invention patent of Dongguan Guoheng Plastic Technology Co., Ltd.: the patent name is "Plastic Screw Locking Strength Test Fixture", and the patent number is: ZL201510699992.6. The test standard is: screw locking torque ≥4.5Kg.f, 5 times of locking in and 5 times of loosening, no slipping is qualified, and the test results are detected and recorded.

[0134] The following are the performance test data of the low carbon emission and high toughness PCR HIPS modified materials prepared in Examples 1-18 and Comparative Examples 1-3, see Table 6 below for details.

[0135] Table 6 Performance test data of low carbon emission and high toughness PCR HIPS modified materials prepared in Examples 1-18 and Comparative Examples 1-3

[0136]

[0137]

[0138] Combining Examples 1-3 and Comparative Examples 1-3 and the table, it can be seen that in Examples 1-3, the toughening agent, compatibilizer, filler and silane coupling agent of the present application are compounded to reinforce PCR HIPS and HIPS. The prepared PCR HIPS material has good impact strength and toughness, as well as good hardness. After the screw locking test, the screw locking torque can reach 4.5Kg.f, which meets the test standard; compared with Example 1, in Comparative Example 1, the compatibilizer is replaced with styrene grafted maleic anhydride, and the impact strength and toughness of the prepared PCR HIPS modified material are reduced, and the screw locking resistance is significantly reduced. In Comparative Example 2, the filler is replaced by the compatibilizer in equal amounts. Although the impact strength of the prepared PCR HIPS modified material is slightly improved, due to the lack of the assistance of the filler, the rigidity is poor, the hardness is low, and the bending strength is significantly reduced, so that the screw locking resistance is significantly reduced. In Comparative Example 3, the compatibilizer is replaced by the toughening agent in equal amounts. The PCR The impact resistance and flexural strength of the HIPS modified material are both reduced, which may be because the compatibility of the various raw materials is reduced due to the reduction of the compatibilizer, resulting in insufficient structural tightness of the prepared PCR HIPS modified material, and a decrease in the impact resistance and flexural strength, which makes it easy for the teeth to slip.

[0139] In order to further improve the performance of the prepared PCR HIPS modified material, it can be seen from Examples 4-6, 7-13, 14-18 and Table 6 that the preferred proportions of styrene-octene-methacrylate glycidyl copolymer, styrene-acrylonitrile-methacrylate glycidyl copolymer, styrene grafted maleic anhydride, long-chain alkyl silane coupling agent and polycaprolactone triol in the present application are compounded, and the five produce a good synergistic effect, and further compounding with toughening agents and fillers has a better effect. In Examples 7-13, the preferred proportions of styrene-octene-methacrylate glycidyl copolymer, styrene-acrylonitrile-methacrylate glycidyl copolymer, styrene grafted maleic anhydride, long-chain alkyl silane coupling agent and polycaprolactone triol are not used as compatibilizers, and the prepared PCR The performance of the HIPS modified material is relatively low; in Examples 14-18, compared with Example 4, polyethylene glycol diglycidyl ether and n-octyl triethoxy silane are used to modify the powder filler in Examples 14-16, and the obtained PCR HIPS modified material has good impact strength and toughness, as well as good hardness and good resistance to screw locking. In Example 17, polyethylene glycol diglycidyl ether is not added, and in Example 18, polyethylene glycol diglycidyl ether is replaced by polyethylene glycol 400 in an equal amount. Compared with Example 14, since the polyethylene glycol diglycidyl ether and n-octyl triethoxy silane of the present application are not used in combination, the impact strength and bending strength of the obtained PCR HIPS modified material are both reduced.

[0140] (4) Carbon emission equivalent test

[0141] According to the test methods in ISO14067 and PAS2050, the carbon emission equivalent of HIPS, the PCRHIPS modified materials prepared in Example 1 and Example 3 was measured, and the test data was detected and recorded;

[0142] The following is the carbon emission equivalent measurement data of HIPS, Example 1 and Example 3, see Table 7 below for details.

[0143] Table 7 Carbon emission equivalent measurement data of HIPS raw materials, Example 1 and Example 3

[0144]

[0145] From the above, it can be seen that the carbon emission equivalent of the PCR HIPS modified material prepared in this application is reduced by 72.1% to 86.6% compared with the direct use of HIPS raw materials, which meets the low-carbon emission requirements and can be used in places with higher requirements such as locking screws. It has excellent performance and a wide range of applications.

[0146] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A low-carbon emission and high-toughness PCR HIPS modified material, characterized in that: Made from the following raw materials in weight percentage: PCR HIPS 50-95% HIPS 0.5-37% Filler 0.5-10% Toughener 1-8% Compatibilizer 0.5-5% Lubricant 1-3% Antioxidant 0.1-2% Silane coupling agent 0.1-0.3%; The compatibilizer is prepared from the following raw materials in parts by weight: Styrene-octene-glycidyl methacrylate copolymer 20-30 parts 14-24 parts of styrene-acrylonitrile-glycidyl methacrylate copolymer 2-4 parts of long chain alkyl silane coupling agent Styrene grafted maleic anhydride 5-10 parts 3-8 parts of polycaprolactone triol; The filler is prepared by the following steps: Add 60-80 parts of powder filler, 4-8 parts of polyethylene glycol diglycidyl ether and 2-5 parts of n-octyl triethoxy silane into a kneading device, knead and stir to obtain a filler; The powder filler is one or a mixture of wollastonite, kaolin, barium sulfate, talc and mica.

2. A low-carbon emission and high-toughness PCR HIPS modified material according to claim 1, characterized in that: The compatibilizer is prepared by the following steps: Styrene-octene-glycidyl methacrylate copolymer, styrene-acrylonitrile-glycidyl methacrylate copolymer, styrene grafted maleic anhydride, long-chain alkyl silane coupling agent and polycaprolactone triol are added into a reaction device, mixed evenly, heated to melt extrude, cooled and granulated to obtain a compatibilizer.

3. The low-carbon emission and high-toughness PCR HIPS modified material according to claim 1, characterized in that: The toughening agent is SBS and / or SEBS.

4. The low-carbon emission and high-toughness PCR HIPS modified material according to claim 1, characterized in that: The lubricant is one or more combinations of pentaerythritol stearate, ethylene bis stearamide, zinc stearate, and triphenyl phosphate.

5. The low-carbon emission and high-toughness PCR HIPS modified material according to claim 1, characterized in that: The silane coupling agent is any one of γ-(2,3-epoxypropoxy)propyltrimethoxysilane and γ-aminopropyltriethoxysilane.

6. The low-carbon emission and high-toughness PCR HIPS modified material according to claim 1, characterized in that: The antioxidant consists of antioxidant 1010 and antioxidant 168 in a weight ratio of 1:(1.5-2.5).

7. A method for preparing a low-carbon emission and high-toughness PCR HIPS modified material according to any one of claims 1 to 6, characterized in that: The method comprises the following preparation steps: S1, baking the PCR HIPS raw material to obtain the PCR HIPS processed material; S2, adding PCR HIPS processing material, HIPS, toughening agent, compatibilizer and silane coupling agent into a reaction device, stirring evenly, to obtain a mixture A; S3, adding filler, lubricant and antioxidant to mixture A, stirring evenly to prepare PCR HIPS mixture; S4, melt-extrude the PCR HIPS mixture, cool, dry and pelletize to obtain a PCR HIPS modified material.

8. The low-carbon emission and high-toughness PCR HIPS modified material according to claim 7, characterized in that: The baking temperature in step S1 is 70-80°C, and the baking time is 45-120 minutes; the melting temperature in step S4 is 190-230°C.