A kind of anti-aging sealant and its preparation method and application

An anti-aging sealant was prepared by combining a specific crosslinking agent, a silane coupling agent, and titanium dioxide nanowires. This solved the problems of silicone sealants being prone to aging at high temperatures and becoming brittle at low temperatures, achieving excellent anti-aging performance and bonding strength.

CN118006290BActive Publication Date: 2024-11-26JIUJIANG SOUTHERN ENERGY NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410272048.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-11
Publication Date
2024-11-26
Estimated Expiration
2044-03-11

AI Technical Summary

Technical Problem

Existing silicone sealants are prone to aging at high temperatures and become brittle and lack elasticity at low temperatures, failing to meet the anti-aging performance requirements for a wide range of applications.

Method used

An anti-aging sealant was prepared using a specific crosslinking agent, silane coupling agent, and titanium dioxide nanowires through a specific process, thereby improving its anti-aging and adhesion properties.

Benefits of technology

It significantly improves the aging resistance and bonding strength of sealants, is suitable for a wider temperature range, and extends service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004734605650000021
    Figure BDA0004734605650000021
  • Figure BDA0004734605650000031
    Figure BDA0004734605650000031
  • Figure BDA0004734605650000041
    Figure BDA0004734605650000041
Patent Text Reader

Abstract

The present invention belongs to the technical field of sealants, and specifically relates to an anti-aging sealant and a preparation method and application thereof. The anti-aging sealant comprises the following components: 100 parts of α,ω-dihydroxy polydimethylsiloxane; 20 to 30 parts of dimethyl silicone oil; 10 to 20 parts of a cross-linking agent; 0.3 to 0.5 parts of a catalyst; 3 to 7 parts of a silane coupling agent; and 5 to 9 parts of titanium dioxide nanowires. The present invention uses a cross-linking agent, a specific silane coupling agent, and titanium dioxide nanowires prepared by a special process, and by adding the above raw materials, the anti-aging performance and bonding performance of the sealant are significantly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of sealants, and more specifically, relates to an anti-aging sealant and a preparation method and application thereof. Background Art

[0002] Silicone sealant is a silicone rubber based on multifunctional siloxane crosslinker and terminal hydroxyl siloxane polymer, with polydimethylsiloxane as the main raw material, mixed with plasticizer, catalyst and coupling agent. It has elasticity and adhesion, is in a viscous paste, and is easy to cure with water in the air at room temperature. Silicone sealant is a polymer with Si-O bond as the main chain, and the bond energy is 1 014kJ / mol, which is much higher than the energy of organic sealants (acrylic sealants, polyurethane sealants, etc.) with C-C bond (344.4kJ / mol) as the main chain of the polymer. Therefore, it has good weather resistance and excellent high temperature resistance. Ordinary organic sealants will age quickly when the temperature is too high, and they are brittle and inelastic at low temperatures. The operating temperature is usually between -20 and 100℃; while the operating temperature range of silicone sealants is between -70 and 200℃. Within this temperature range, even if used in outdoor environments for a long time, silicone sealants are not easy to crack and harden, and their service life can reach several decades. Therefore, silicone sealants are widely used in the sealing and bonding of various synthetic materials and metals, the bonding and sealing of expansion joints of high-rise buildings, as well as decoration and waterproofing projects. However, in actual application, the anti-aging performance can no longer meet the needs of actual production.

[0003] CN117467401A discloses an anti-aging silicone sealant and a preparation method thereof, belonging to the technical field of sealants, and comprising the following components by weight: 75-105 parts of 107# silicone rubber, 35-55 parts of dimethyl silicone oil, 35-40 parts of modified fillers, 10-20 parts of crosslinking agents, 4-8 parts of coupling agents, and 0.2-1.0 parts of catalysts, wherein the modified filler is a spherical silica mixture with a gradient median particle size modified by dopamine and loaded with a hindered phenol structure compound. The present invention improves the compatibility and bonding performance of the modified filler and the silicone sealant substrate prepared in the end by adding the modified filler to the silicone sealant, thereby achieving the purpose of improving the anti-aging performance of the silicone sealant prepared in the end.

[0004] CN117004365A discloses a silicone sealant and its preparation method and application, belonging to the field of building materials technology. The silicone sealant includes a polymer matrix, a crosslinking agent, a coupling agent, a filler, a plasticizer and a catalyst; the preparation method of the polymer matrix includes: a) under anhydrous and oxygen-free conditions, methyltrichlorosilane reacts with 1H, 1H, 2H, 2H-perfluorododecyl sulfide to generate a fluorine-based silane intermediate; b) under anhydrous and oxygen-free conditions, methyltrichlorosilane reacts with bromobenzene to generate a phenylsilane intermediate; c) the fluorine-based silane intermediate, the phenylsilane intermediate and polydimethylsiloxane are mixed, and a substitution reaction of silicon oxygen bonds is carried out to obtain a polymer matrix with fluorine groups and phenyl groups introduced. In this application, polydimethylsiloxane is modified to introduce fluorine groups and phenyl groups, which can improve the anti-aging performance of silicone sealants and prevent them from aging and yellowing, and the introduction of amino groups can increase the surface activity of silicone sealants, improve their adhesion to the substrate, and improve the sealing effect.

[0005] CN114214025A discloses a novel two-component silicone structural sealant and its preparation method. A novel two-component silicone structural sealant includes component A and component B. Component A includes the following raw materials by weight: 30-70 parts of nano calcium carbonate, 20-55 parts of base glue, and 2-35 parts of dimethyl silicone oil; component B includes the following raw materials by weight: 10-30 parts of carbon black, 3-15 parts of fumed silica, 20-40 parts of dimethyl silicone oil, 10-50 parts of a first cross-linking agent, 10-45 parts of a second cross-linking agent, 10-45 parts of a coupling agent, and 0.01-0.14 parts of a catalyst; wherein the second cross-linking agent is a propyltrimethoxysilane oligomer with a degree of polymerization of 4-6. The two-component silicone structural sealant of the present application has the advantages of excellent water-immersion bonding performance and excellent anti-aging performance.

[0006] It can be seen from the above literature that the performance of silicone sealant can be improved by adding a modifying component. Based on the above content, the present invention provides an anti-aging sealant with excellent anti-aging performance and bonding performance. Summary of the invention

[0007] The technical problem to be solved by the present invention is to overcome the defects and shortcomings of the prior art and provide an anti-aging sealant and its preparation method and application. The anti-aging sealant comprises the following components: 100 parts of α,ω-dihydroxy polydimethylsiloxane; 20-30 parts of dimethyl silicone oil; 10-20 parts of a cross-linking agent; 0.3-0.5 parts of a catalyst; 3-7 parts of a silane coupling agent; and 5-9 parts of titanium dioxide nanowires. The present invention uses a cross-linking agent, a specific silane coupling agent and titanium dioxide nanowires prepared by a special process, and by adding the above raw materials, the anti-aging performance and bonding performance of the sealant are significantly improved.

[0008] The purpose of the present invention is to provide an anti-aging sealant.

[0009] Another object of the present invention is to provide a method for preparing an anti-aging sealant.

[0010] Another object of the present invention is the application of an anti-aging sealant.

[0011] The above-mentioned purpose of the present invention is achieved through the following technical solutions:

[0012] An anti-aging sealant comprises the following components in parts by weight:

[0013]

[0014]

[0015] In the present invention, preferably, the catalyst is at least one of dibutyltin dibutyrate, dihydroxybutyltin chloride and dibutyltin maleate; the viscosity of the α,ω-dihydroxypolydimethylsiloxane is 15000cps to 25000cps; and the viscosity of the dimethyl silicone oil is 300cps to 500cps.

[0016] In the present invention, preferably, the crosslinking agent is at least one of vinyl tris (methyl ethyl ketoxime) silane, vinyl tris (butyl ketoxime) silane and tetras (butyl ketoxime) silane; further preferably, the crosslinking agent is vinyl tris (butyl ketoxime) silane and at least one of vinyl tris (methyl ethyl ketoxime) silane and tetras (butyl ketoxime) silane; the mass ratio of the vinyl tris (butyl ketoxime) silane to at least one of vinyl tris (methyl ethyl ketoxime) silane and tetras (butyl ketoxime) silane is 3:2; further preferably, the crosslinking agent is vinyl tris (methyl ethyl ketoxime) silane and tetras (butyl ketoxime) silane, and the mass ratio of the vinyl tris (methyl ethyl ketoxime) silane to tetras (butyl ketoxime) silane is 3:1:1.

[0017] In the present invention, preferably, the silane coupling agent is at least one of tridecafluorooctyltrimethoxysilane and KH-602; further preferably, the silane coupling agent is tridecafluorooctyltrimethoxysilane and KH-602, and the mass ratio of tridecafluorooctyltrimethoxysilane to KH-602 is 1:4.

[0018] In the present invention, a preferred technical solution is that the method for preparing titanium dioxide nanowires comprises the following steps:

[0019] (1) Carbonizing the silk in an inert atmosphere and obtaining carbonized silk after cooling;

[0020] (2) immersing the carbonized silk obtained in step (1) in a nitric acid solution, treating with acid for a certain period of time, washing, and drying to a constant weight to obtain acid-treated carbonized silk;

[0021] (3) Add the acid-treated carbonized silk and n-butyl titanate obtained in step (2) to glacial acetic acid, stir for a certain period of time, and then transfer to a hydrothermal kettle for reaction, cool to room temperature, filter, wash, and dry at 80-120° C. for 10-20 h; then calcine at 450-550° C. for 5-9 h in an air atmosphere to obtain titanium dioxide nanowires.

[0022] Preferably, in step (1), the carbonization treatment is carried out at 700-800° C. for 1-2 hours; and the length of the silk is 2-4 cm.

[0023] Preferably, in step (2), the concentration of the nitric acid solution is 2 to 4 mol / L; the acid treatment time is 1 to 3 hours; and the drying temperature is 70°C.

[0024] Preferably, in step (3), the stirring time is 30 to 50 minutes; and the reaction conditions are 140 to 180° C. for 8 to 12 hours.

[0025] Preferably, in step (3), drying is performed at 80-120° C. for 10-20 h; calcination is performed at 450-550° C. for 5-9 h; and the ratio of the acid-treated carbonized silk, n-butyl titanate and glacial acetic acid is 1 g: 4-6 mL: 50-70 mL.

[0026] Based on the above-mentioned method for preparing an anti-aging sealant, the preparation method comprises the following steps:

[0027] (1) adding the α,ω-dihydroxy polydimethylsiloxane, dimethyl silicone oil, silane coupling agent and titanium dioxide nanowires into a planetary machine, and dehydrating for 1.5 to 2.5 hours at a temperature of 115° C. to 135° C. and a vacuum degree of -0.04 MPa to -0.08 MPa to obtain a base material;

[0028] (2) After the temperature of the base material is cooled to room temperature, a cross-linking agent and a catalyst are added in sequence, and the mixture is stirred for 1 to 3 hours under a vacuum degree of -0.04 MPa to -0.08 MPa to obtain the anti-aging sealant.

[0029] The anti-aging sealant described above is applied in the field of construction.

[0030] The present invention has the following beneficial effects:

[0031] (1) The present invention selects a specific cross-linking agent, so that the sealant of the present application has excellent anti-aging ability and bonding strength;

[0032] (2) By adding a silane coupling agent, the dispersibility of titanium dioxide nanowires can be improved, and the silane coupling agent in this application can also promote the improvement of sealant performance.

[0033] (3) Due to the presence of a hollow structure, the titanium dioxide nanowires prepared by the specific process of the present invention allow part of the raw materials to enter the hollow structure, thereby promoting the improvement of the sealant performance. DETAILED DESCRIPTION

[0034] The present invention is further described below with reference to specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0035] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.

[0036] Example 1

[0037] An anti-aging sealant comprises the following components in parts by weight:

[0038]

[0039] The catalyst is dibutyltin dibutyrate;

[0040] The α,ω-dihydroxy polydimethylsiloxane has a viscosity of 20000cps;

[0041] The viscosity of the dimethyl silicone oil is 400 cps;

[0042] The crosslinking agent is vinyl tributylidene oxime silane;

[0043] The silane coupling agent is KH-602;

[0044] The method for preparing titanium dioxide nanowires comprises the following steps:

[0045] (1) In an inert atmosphere, 100 g of silk was carbonized at 750° C. for 1.5 h, and carbonized silk was obtained after cooling; the length of the silk was 3 cm;

[0046] (2) immersing the carbonized silk obtained in step (1) in a 3 mol / L nitric acid solution, treating with acid for 2 h, washing, and drying at 70° C. to constant weight to obtain acid-treated carbonized silk;

[0047] (3) Add 10 g of the acid-treated carbonized silk obtained in step (2) and 50 mL of n-butyl titanate to 600 mL of glacial acetic acid, stir for 40 min, then transfer to a hydrothermal kettle, react at 160 ° C for 10 h, cool to room temperature, filter, wash, and dry at 100 ° C for 16 h; then calcine at 500 ° C for 7 h in an air atmosphere to obtain titanium dioxide nanowires.

[0048] A method for preparing an anti-aging sealant comprises the following steps:

[0049] (1) adding the α,ω-dihydroxypolydimethylsiloxane, dimethyl silicone oil, silane coupling agent and titanium dioxide nanowires into a planetary machine, and dehydrating for 2 hours at a temperature of 125° C. and a vacuum degree of −0.06 MPa to obtain a base material;

[0050] (2) After the temperature of the base material is cooled to room temperature, a cross-linking agent and a catalyst are added in sequence, and the mixture is stirred for 2 hours under a vacuum degree of -0.06 MPa to obtain the anti-aging sealant.

[0051] Example 2

[0052] An anti-aging sealant comprises the following components in parts by weight:

[0053]

[0054] The catalyst is dihydroxybutyltin chloride;

[0055] The α,ω-dihydroxy polydimethylsiloxane has a viscosity of 25000cps;

[0056] The viscosity of the dimethyl silicone oil is 300 cps;

[0057] The crosslinking agent is vinyl tris(methyl ethyl ketoxime) silane;

[0058] The silane coupling agent is tridecafluorooctyltrimethoxysilane;

[0059] The preparation method of the titanium dioxide nanowires is the same as the preparation method of the titanium dioxide nanowires in Example 1.

[0060] A method for preparing an anti-aging sealant comprises the following steps:

[0061] (1) adding the α,ω-dihydroxypolydimethylsiloxane, dimethyl silicone oil, silane coupling agent and titanium dioxide nanowires into a planetary machine, and dehydrating for 1.5 hours at a temperature of 135° C. and a vacuum degree of −0.08 MPa to obtain a base material;

[0062] (2) After the temperature of the base material is cooled to room temperature, a cross-linking agent and a catalyst are added in sequence, and the mixture is stirred for 1 hour under a vacuum degree of -0.08 MPa to obtain the anti-aging sealant.

[0063] Example 3

[0064] An anti-aging sealant comprises the following components in parts by weight:

[0065]

[0066] The catalyst is dibutyltin maleate;

[0067] The α,ω-dihydroxy polydimethylsiloxane has a viscosity of 15000cps;

[0068] The viscosity of the dimethyl silicone oil is 500cps;

[0069] The cross-linking agent is tetrabutyl ketoxime silane;

[0070] The silane coupling agent is KH-602;

[0071] The preparation method of the titanium dioxide nanowires is the same as the preparation method of the titanium dioxide nanowires in Example 1.

[0072] A method for preparing an anti-aging sealant comprises the following steps:

[0073] (1) adding the α,ω-dihydroxypolydimethylsiloxane, dimethyl silicone oil, silane coupling agent and titanium dioxide nanowires into a planetary machine, and dehydrating for 2.5 hours at a temperature of 115° C. and a vacuum degree of -0.04 MPa to obtain a base material;

[0074] (2) After the temperature of the base material is cooled to room temperature, a cross-linking agent and a catalyst are added in sequence, and the mixture is stirred for 3 hours under a vacuum degree of -0.04 MPa to obtain the anti-aging sealant.

[0075] Example 4

[0076] Example 4 is basically the same as Example 1, except that: the cross-linking agent is vinyl trisbutyl ketoxime silane and vinyl tris(methyl ethyl ketoxime) silane; the mass ratio of the vinyl trisbutyl ketoxime silane to vinyl tris(methyl ethyl ketoxime) silane is 3:2.

[0077] Example 5

[0078] Example 5 is substantially the same as Example 4, except that the crosslinking agent is vinyl tris(methyl ethyl ketoxime)silane, vinyl tris(methyl ethyl ketoxime)silane and tetras(butyl ketoxime)silane, and the mass ratio of the vinyl tris(methyl ethyl ketoxime)silane to the tetras(butyl ketoxime)silane is 3:1:1.

[0079] Example 6

[0080] Example 6 is substantially the same as Example 5, except that the silane coupling agent is tridecafluorooctyltrimethoxysilane and KH-602, and the mass ratio of tridecafluorooctyltrimethoxysilane to KH-602 is 1:4.

[0081] Comparative Example 1

[0082] Comparative Example 1 is substantially the same as Example 1, except that the method for preparing titanium dioxide nanowires comprises the following steps:

[0083] (1) In an inert atmosphere, 100 g of silk was carbonized at 750° C. for 1.5 h, and carbonized silk was obtained after cooling; the length of the silk was 3 cm;

[0084] (2) immersing the carbonized silk obtained in step (1) in a 3 mol / L nitric acid solution, treating with acid for 2 h, washing, and drying at 70° C. to constant weight to obtain acid-treated carbonized silk;

[0085] (3) Add 10 g of the acid-treated carbonized silk obtained in step (2) and 50 mL of n-butyl titanate to 600 mL of glacial acetic acid, stir for 40 min, then transfer to a hydrothermal kettle, react at 160 ° C for 10 h, cool to room temperature, filter, wash, and dry at 100 ° C for 16 h; then calcine at 500 ° C for 7 h under a nitrogen atmosphere to obtain titanium dioxide nanowires.

[0086] Comparative Example 2

[0087] Comparative Example 1 is substantially the same as Example 1, except that it does not contain titanium dioxide nanowires.

[0088] The performance of Examples 1-6 and Comparative Examples 1-2 was tested. The specific test results are shown in Table 1:

[0089] Among them, tensile strength: tested according to the method specified in GB / T 528-1998;

[0090] High temperature aging strength test: The sealant is aged at 270°C for 8 days, and then its high temperature mechanical properties are tested according to GB / T528-2009.

[0091]

[0092] It can be seen from Table 1 that, by comparing Example 1 with Comparative Examples 1-2, the titanium dioxide nanowires prepared by a specific method in the present application can be added to the sealant to significantly improve the bonding strength and aging resistance of the sealant. Moreover, by comparing the embodiments, it can be seen that the cross-linking agent and the silane coupling agent have a synergistic effect. By using a cross-linking agent and a coupling agent of a specific composition, the tensile strength of the sealant of the present invention can be as high as 2.92 MPa, and it has excellent aging resistance.

[0093] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. An anti-aging sealant, characterized in that: By weight, it includes the following components: 100 parts of α,ω-dihydroxy polydimethylsiloxane; 20-30 parts of dimethyl silicone oil; 10-20 parts of cross-linking agent; Catalyst 0.3~0.5 parts; Silane coupling agent 3~7 parts; 5-9 parts of titanium dioxide nanowires; The method for preparing titanium dioxide nanowires comprises the following steps: (1) Carbonizing the silk in an inert atmosphere and obtaining carbonized silk after cooling; (2) immersing the carbonized silk obtained in step (1) in a nitric acid solution, treating with acid for a certain period of time, washing, and drying to a constant weight to obtain acid-treated carbonized silk; (3) adding the acid-treated carbonized silk and n-butyl titanate obtained in step (2) to glacial acetic acid, stirring for a certain period of time, and then transferring to a hydrothermal kettle for reaction, cooling to room temperature, filtering, washing, and drying at 80-120° C. for 10-20 h; and then calcining at 450-550° C. for 5-9 h in an air atmosphere to obtain titanium dioxide nanowires; the ratio of the acid-treated carbonized silk, n-butyl titanate and glacial acetic acid is 1 g: 4-6 mL: 50-70 mL; The cross-linking agent is vinyl tris(butyl ketone oxime)silane, vinyl tris(methyl ethyl ketone oxime)silane and tetras(butyl ketone oxime)silane, and the mass ratio of the vinyl tris(butyl ketone oxime)silane, vinyl tris(methyl ethyl ketone oxime)silane and tetras(butyl ketone oxime)silane is 3:1:1; the silane coupling agent is tridecafluorooctyl trimethoxysilane and KH-602, and the mass ratio of the tridecafluorooctyl trimethoxysilane and KH-602 is 1:

4.

2. The anti-aging sealant according to claim 1, characterized in that: The catalyst is at least one of dibutyltin dibutyrate, dihydroxybutyltin chloride and dibutyltin maleate; the viscosity of the α,ω-dihydroxypolydimethylsiloxane is 15000cps-25000cps; and the viscosity of the dimethyl silicone oil is 300cps-500cps.

3. The anti-aging sealant according to claim 1, characterized in that: In step (1), the carbonization treatment is carried out at 700-800° C. for 1-2 hours; and the length of the silk is 2-4 cm.

4. The anti-aging sealant according to claim 1, characterized in that: In step (2), the concentration of the nitric acid solution is 2-4 mol / L; the acid treatment time is 1-3 h; and the drying temperature is 70°C.

5. The anti-aging sealant according to claim 1, characterized in that: In step (3), the stirring time is 30-50 min; and the reaction conditions are 140-180° C. for 8-12 h.

6. A method for preparing an anti-aging sealant according to any one of claims 1 to 5, characterized in that: The preparation method comprises the following steps: (1) adding the α,ω-dihydroxypolydimethylsiloxane, dimethyl silicone oil, silane coupling agent and titanium dioxide nanowires into a planetary machine, and dehydrating for 1.5 to 2.5 hours at a temperature of 115° C. to 135° C. and a vacuum degree of -0.04 MPa to -0.08 MPa to obtain a base material; (2) After the temperature of the base material is cooled to room temperature, a cross-linking agent and a catalyst are added in sequence, and the mixture is stirred for 1 to 3 hours under a vacuum degree of -0.04 MPa to -0.08 MPa to obtain the anti-aging sealant.

7. Use of the anti-aging sealant according to any one of claims 1 to 5 in the field of construction.