Multilayer structures and their manufacturing methods, as well as protective sheets and electronic devices using the same.
By forming a layer of reaction products of metal oxides and inorganic phosphorus compounds on a substrate, the problem that existing multilayer structures cannot simultaneously possess high barrier properties and high resolution is solved, thus realizing a multilayer structure with high barrier properties and high resolution, suitable for protective sheets for electronic devices.
Patent Information
- Application Number
- CN202280066005.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-10-07
- Filing Date
- 2022-10-06
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-10-06
AI Technical Summary
The multi-layered structure of existing electronic devices makes it difficult to achieve high definition while maintaining high barrier properties.
By using a layer containing reaction products of metal oxides and inorganic phosphorus compounds, and by controlling the coating speed of the coating liquid and the selection of the substrate, a multilayer structure with an image clarity of over 90% can be formed.
It achieves a multi-layered structure with high barrier properties and high definition, suitable for protective sheets of electronic devices, and improves the image viewing effect of electronic devices.
Smart Images

Figure BDA0004764547790000351
Abstract
Description
Technical Field
[0001] This invention relates to a multilayer structure with high gas and water vapor barrier properties and high clarity, a method for manufacturing the same, and protective sheets and electronic devices using the same. Background Technology
[0002] Electronic devices, such as those with solar cells and displays, require transparent protective components to protect their surfaces. These protective components sometimes include protective sheets with excellent barrier properties (oxygen and water vapor barrier) such as those formed by a barrier layer on a thick glass plate or resin substrate.
[0003] As a protective sheet with excellent barrier properties, Patent Document 1 describes an electronic device having a protective sheet comprising a multilayer structure. The multilayer structure is formed by coating a substrate (X) with a coating liquid containing a compound containing aluminum and a phosphorus compound, followed by drying and heat treatment, to form a layer (Y) containing reaction products. The average particle size of the aforementioned reaction products is 5 to 70 nm. The document also states that the protective sheet has excellent gas barrier properties and water vapor barrier properties, and can maintain its performance even after a temperature test.
[0004] Existing technical documents
[0005] Patent documents
[0006] Patent Document 1: International Publication No. 2016 / 103720 Summary of the Invention
[0007] The problem that the invention aims to solve
[0008] In recent years, higher levels of resolution have been required for protective sheets (multilayer structures) in electronic devices, etc., but the resolution of multilayer structures used in existing electronic devices is sometimes insufficient. The high barrier properties of the multilayer structures used in existing electronic devices are useful as protective sheets for electronic devices, etc., and a multilayer structure that maintains this performance while also possessing high resolution is sought. To achieve a multilayer structure with high resolution, the inventors have conducted numerous studies using a substrate with high image resolution (writeability) as the substrate (X), but achieving high resolution has been difficult. Through in-depth research, the inventors discovered that the coating speed of the coating liquid applied during the formation of the layer (Y) is related to the resolution of the resulting multilayer structure, thus realizing the present invention.
[0009] The present invention is based on the above-described situation, and its object is to provide a multilayer structure with high barrier properties and clarity, a method for manufacturing the same, and protective sheets and electronic devices using the same.
[0010] means for solving problems
[0011] According to the present invention, the aforementioned objective is achieved by providing the following technical solution.
[0012] [1] A multilayer structure having a substrate (X) and a layer (Y), wherein the layer (Y) contains a reaction product (D) of a metal oxide (A) containing aluminum atoms (hereinafter sometimes abbreviated as "metal oxide (A)") and an inorganic phosphorus compound (BI), the substrate (X) is adjacent to the layer (Y), and the image sharpness of the aforementioned multilayer structure is above 90% when the comb width is 0.25 mm as measured according to ISO17221:2014;
[0013] [2] According to [1], the haze value measured according to JIS K7105:1981 is less than 3%;
[0014] [3] According to the multilayer structure of [1] or [2], the water vapor transmission rate at 40°C and 90% RH, as measured according to ISO 15106-5:2015, is 1×10⁻⁶. -2 g / m 2 • less than 1 day;
[0015] [4] According to any one of [1] to [3], the thermal shrinkage rate of the substrate (X) in the MD direction when heated at 210°C for 1 minute is less than 2.90%;
[0016] [5] According to any one of [1] to [4], the image sharpness of the substrate (X) when the comb width is 0.25 mm as measured according to ISO 17221:2014 is 90% or more;
[0017] [6] A multilayer structure according to any one of [1] to [5], wherein the substrate (X) has a surface layer;
[0018] [7] A multilayer structure according to any one of [1] to [6] has a structure in which a substrate (X) and a layer (Y) are directly stacked;
[0019] [8] A multilayer structure according to any one of [1] to [6] has a structure in which a substrate (X) and a layer (Y) are laminated via an adhesive layer (I);
[0020] [9] According to the multilayer structure of [1] to [8], it has layers (Y) disposed on both sides of the substrate (X);
[0021]
[10] A method for manufacturing a multilayer structure, comprising the following steps:
[0022] Step (I) involves coating at least one side of a substrate (X) with a coating solution (S) comprising a metal oxide (A) containing aluminum atoms, an inorganic phosphorus compound (BI), and a solvent, and then removing the solvent to form a precursor layer for layer (Y); and
[0023] Process (II) involves heat-treating the precursor layer of layer (Y) to form layer (Y).
[0024] The coating speed of the coating liquid (S) in process (I) is 0.03 cm / s or more and 2.5 cm / s or less relative to the coating width of 1 cm. When the comb width is 0.25 mm as measured according to ISO 17221:2014, the image clarity of the resulting multilayer structure is 90% or more.
[0025]
[11] A protective sheet for an electronic device, comprising a multilayer structure of any one of [1] to [9];
[0026]
[12] According to
[11] , the protective sheet is a protective sheet that protects the surface of a photoelectric conversion device, an information display device or a lighting device;
[0027]
[13] An electronic device having a protective sheet of
[11] or
[12] .
[0028] Invention Effects
[0029] According to the present invention, a multilayer structure with high barrier properties and clarity, a method for manufacturing the same, and protective sheets and electronic devices using the same are available. Detailed Implementation
[0030] In this specification, "barrier properties" mainly refers to both oxygen barrier properties and water vapor barrier properties, while "gas barrier properties" mainly refers to oxygen barrier properties. Furthermore, "clarity" is an evaluation of the clarity of the image observed through the multi-layer structure of this invention, as described in the embodiments, and is judged based on the discernibility of the image when visually confirming it through the multi-layer structure of this invention.
[0031] [Multi-layer structure]
[0032] The multilayer structure of the present invention is a multilayer structure having a substrate (X) and a layer (Y), wherein the layer (Y) contains a reaction product (D) of a metal oxide (A) and an inorganic phosphorus compound (BI), the substrate (X) is adjacent to the layer (Y), and the image sharpness of the multilayer structure is above 90% when the comb width is 0.25 mm as measured according to ISO 17221:2014.
[0033] In this specification, "adjacent" means that the layers are stacked in a very close manner. Specifically, it means that they are stacked directly or via other layers (e.g., adhesive layers with a thickness of 10 μm or less). In a configuration where the substrate (X) and layer (Y) are adjacent, the distance between the substrate (X) and layer (Y) can be 0 μm or more and 10 μm or less, 0 μm or more and 1 μm or less, 0 μm or more and 0.1 μm or less, or 0 μm or more and 0.03 μm or less. Furthermore, if there are multiple substrates (X), it is sufficient that one substrate (X) is adjacent to the layer (Y); the other substrates (X) may or may not be adjacent to the layer (Y). Similarly, if there are multiple layers (Y), it is sufficient that one layer (Y) is adjacent to the substrate (X); the other layers (Y) may or may not be adjacent to the substrate (X). That is, at least one set of substrates (X) and layers (Y) need to be adjacent.
[0034] By achieving an image sharpness of 90% or higher for the multilayer structure of the present invention, excellent clarity is achieved when used, for example, as a protective sheet for electronic devices. The image sharpness of the multilayer structure of the present invention is sometimes preferably 91% or higher, more preferably 92% or higher, even more preferably 93% or higher, and still more preferably 94% or higher or 95% or higher. The image sharpness of the multilayer structure of the present invention may be 100% or lower, and may be 99%, 98%, 97%, or 96% or lower.
[0035] The detailed method for achieving an image sharpness of 90% or higher for the multilayer structure of the present invention is described below. Particularly important are: using a substrate (X) with high image sharpness; and performing the coating process under the condition that the coating speed of the coating liquid (S) is 0.03 cm / s or more and 2.5 cm / s or less relative to a coating width of 1 cm. Here, "0.03 cm / s or more and 2.5 cm / s or less relative to a coating width of 1 cm" means that the coating speed condition varies depending on the length of the coating width. For example, when the coating width is 10 cm (when coating with a width of 10 cm), it means that the coating speed is 0.3 cm / s or more and 25 cm / s or less. When coating one entire surface of the substrate (X) in a single pass along a direction perpendicular to the width of the substrate (X), the coating width is equal to the width of the substrate (X). It should be noted that, depending on the smoothness of the layer (Y) formed by coating or the like, the image sharpness of the multilayer structure can sometimes be high compared to the image sharpness of the substrate (X).
[0036] In this specification, "thickness" refers to the average value of measurements taken at any 5 locations (average thickness).
[0037] [Substrate (X)]
[0038] The material of the substrate (X) is not particularly limited, but from the viewpoint of high image clarity, it is preferable to include a thermoplastic resin. The form of the substrate (X) is not particularly limited, but it is preferably a layered form such as a film or sheet. As the substrate (X), it is preferable to include a thermoplastic resin film or a thermoplastic resin film with an inorganic vapor-deposited layer (X') laminated on it, more preferably a thermoplastic resin film, and even more preferably a thermoplastic resin film.
[0039] Examples of thermoplastic resins used as the substrate (X) include polyolefin resins such as polyethylene and polypropylene; polyester resins such as polyethylene terephthalate (PET), polyethylene 2,6-naphthalate, polybutylene terephthalate, or copolymers thereof; polyamide resins such as nylon-6, nylon-66, and nylon-12; polymers containing hydroxyl groups such as polyvinyl alcohol and ethylene-vinyl alcohol copolymers; polystyrene; poly(meth)acrylate; polyacrylonitrile; polyvinyl acetate; polycarbonate; polyarylate; regenerated cellulose; polyimide; polyetherimide; polysulfone; polyethersulfone; polyetheretherketone; ionomer resins, etc. The thermoplastic resin used as the substrate (X) is preferably selected from at least one of polyethylene, polypropylene, polyethylene terephthalate, nylon-6, and nylon-66, and from the viewpoint of excellent image clarity, polyethylene terephthalate is more preferred.
[0040] To impart slip resistance and anti-adhesion properties, the substrate (X) may contain inorganic or organic microparticles. From the viewpoint of improving the image sharpness of the substrate (X), when inorganic or organic microparticles are included, the surface layer described later preferably contains them. That is, from the viewpoint of image sharpness, it is sometimes preferable that the portion of the substrate (X) other than the surface layer does not contain inorganic or organic microparticles. As inorganic microparticles, metals such as gold, silver, copper, platinum, palladium, rhenium, vanadium, osmium, cobalt, iron, zinc, ruthenium, praseodymium, chromium, nickel, aluminum, tin, zinc, titanium, tantalum, zirconium, antimony, indium, yttrium, and lanthanum can be used; metal oxides such as zinc oxide, titanium oxide, cesium oxide, antimony oxide, tin oxide, indium tin oxide, yttrium oxide, lanthanum oxide, zirconium oxide, aluminum oxide, and silicon oxide; metal fluorides such as lithium fluoride, magnesium fluoride, aluminum fluoride, and cryolite; metal phosphates such as calcium phosphate; carbonates such as calcium carbonate; sulfates such as barium sulfate; and other talc and kaolin, etc. In addition to cross-linked microparticles such as organosilicon compounds, cross-linked styrene, cross-linked acrylics, and cross-linked melamine, thermoplastic resins that are incompatible with the thermoplastic resin constituting the substrate (X) but undergo micro-dispersion to form an island structure can also be used as organic microparticles. The average particle size of the microparticles (inorganic microparticles and organic microparticles) used is preferably 0.001 to 5 μm.
[0041] When the aforementioned thermoplastic resin film is used as the substrate (X), the substrate (X) can be a stretched film or an unstretched film. From the perspective of excellent processing adaptability (printing, lamination, etc.) of the resulting multilayer structure, a stretched film is preferred, and a biaxially stretched film is particularly preferred. The biaxially stretched film can be a biaxially stretched film manufactured by any of the following methods: simultaneous biaxial stretching, successive biaxial stretching, and tubular stretching.
[0042] The thickness of each layer of the substrate (X) is preferably 5 μm or more and 200 μm or less, more preferably 7 μm or more and 150 μm or less, and even more preferably 10 μm or more and 100 μm or less. If the thickness of each layer of the substrate (X) is 5 μm or more, it tends to exhibit excellent mechanical strength and processability. Furthermore, if the thickness of each layer of the substrate (X) is 200 μm or less, it tends to exhibit excellent flexibility in the resulting multilayer structure.
[0043] The substrate (X) preferably has high image resolution. The image resolution of the substrate (X) with a comb width of 0.25 mm, measured according to ISO 17221:2014, is preferably 90% or higher, more preferably 91% or higher, and even more preferably 92% or higher. From a manufacturing cost perspective, the image resolution of the substrate (X) can be 99% or lower, 97% or lower, 96% or lower, or 95% or lower. If the image resolution of the substrate (X) is 90% or higher, it is easy to adjust the image resolution of the resulting multilayer structure to 90% or higher.
[0044] As a means of adjusting the image sharpness of the substrate (X) to 90% or more, examples include: not containing additives (components other than thermoplastic resin) in layers other than the surface layer described later, or even if they contain additives, setting them to a small amount; and setting the surface layer described later.
[0045] To provide various functions and from the viewpoint of improving the image clarity of the substrate (X), the substrate (X) preferably has a surface layer. The surface layer is a layer disposed on the surface of the substrate (X), and may be disposed on one side or both sides of the substrate (X). The substrate (X) may have a resin substrate layer and a surface layer laminated on one or both sides of the resin substrate layer. The resin substrate layer may be a layer of thermoplastic resin as described above, which is the thermoplastic resin used in the substrate (X). The resin substrate layer may be a PET layer. Other layers, such as an inorganic vapor-deposited layer (X'), may exist between the resin substrate layer and the surface layer. The resin substrate layer and the surface layer are preferably directly laminated. When the surface layer is mainly composed of resin, the resin substrate layer and the surface layer may also be distinguished based on differences in the composition of each layer.
[0046] There are no particular limitations as long as the surface layer has adhesive properties to the resin substrate layer, etc., and a thermoplastic resin is preferred as the main component. Here, "as the main component" means that the content is more than 50% by mass. As the aforementioned thermoplastic resin, polyester resins, polycarbonate resins, epoxy resins, alkyd resins, acrylic resins, urea resins, urethane resins, etc., can be used suitably. In addition, two or more different thermoplastic resins can be used in combination, such as polyester resin and urethane resin, polyester resin and acrylic resin, or urethane resin and acrylic resin, etc. Among these, it is preferred to select at least one selected from polyester resins, acrylic resins, and urethane resins, and more preferably polyester resins.
[0047] From the viewpoint of significantly improving both heat-resistant adhesion and moisture-resistant adhesion, it is sometimes preferable for the surface layer to contain various crosslinking agents. In particular, when polyester resin, urethane resin, or acrylic resin is used as the main component of the surface layer, and the aforementioned resin copolymerizes with crosslinking functional groups, it is preferable to also include a crosslinking agent. The thermoplastic resin constituting the surface layer and the crosslinking agent can be mixed in any ratio. From the viewpoint of improving adhesion, the crosslinking agent is preferably 0.2 to 20 parts by weight, more preferably 0.5 to 15 parts by weight, and even more preferably 1 to 10 parts by weight relative to 100 parts by weight of the thermoplastic resin.
[0048] To impart slip resistance and anti-adhesion properties, the surface layer may contain the aforementioned inorganic or organic microparticles.
[0049] From the viewpoint of further improving water vapor barrier properties and image clarity, the thermal shrinkage rate of the substrate (X) in the MD direction after heating at 210°C for 1 minute is preferably 2.90% or less, more preferably 2.80% or less. The aforementioned thermal shrinkage rate of the substrate (X) in the MD direction can be 0.5% or more, and from the viewpoint of further improving water vapor barrier properties, it is sometimes preferred to be 2.10% or more. This thermal shrinkage rate of the substrate (X) can be the thermal shrinkage rate of the substrate (X) used as a raw material for a multilayer structure (the substrate (X) before forming the layer (Y) described later).
[0050] As the substrate (X), commercially available products can be used. Examples of commercially available products with high image clarity include Toray Industries' Lumira (registered trademark) U403, U483, A48, and XW731C; HYOSUNG's RH210; Mitsubishi Chemical's Daia Wheel (registered trademark) T600; Toyobo's Cosmosine (registered trademark) A4160 and SRF; and Toyobo's Ester film HPE, etc. These have surface layers on one or two sides.
[0051] From the viewpoints of the coatability of the coating liquid (S) (described later) and the barrier properties of the resulting multilayer structure, the substrate (X) is preferably surface-treated. Surface treatment can be performed using known methods, such as UV ozone treatment, high-concentration ozone water treatment, excimer ozone treatment, corona treatment, oxygen plasma treatment, or AP plasma treatment.
[0052] The thermoplastic resin film with an inorganic vapor-deposited layer (X') laminated on it, used as a substrate (X), is typically a transparent film that provides barrier properties against oxygen and water vapor. When a thermoplastic resin film with an inorganic vapor-deposited layer (X') laminated on one side is used as a substrate (X), the layer (Y) described later is laminated on the side of the inorganic vapor-deposited layer (X'). The thermoplastic resin film used as the thermoplastic resin film with the inorganic vapor-deposited layer (X') can be the thermoplastic resin film exemplified as the substrate (X) described above. The inorganic vapor-deposited layer (X') can be formed by vapor-depositing an inorganic material. Examples of inorganic materials include metal oxides (e.g., silicon oxide, aluminum oxide), metal nitrides (e.g., silicon nitride), or metal oxynitrides (e.g., silicon oxynitride). From the viewpoint of excellent transparency, an inorganic vapor-deposited layer (X') formed of aluminum oxide, silicon oxide, magnesium oxide, or silicon nitride is preferred. It should be noted that, from the viewpoint of image sharpness, the substrate (X) is sometimes preferably free of inorganic vapor deposits (X').
[0053] There are no particular limitations on the formation method of inorganic vapor deposition layer (X'). Examples include physical vapor deposition methods such as vacuum evaporation (e.g., resistance heating evaporation, electron beam evaporation, molecular beam epitaxy, etc.), sputtering, and ion plating; chemical vapor deposition methods such as thermochemical vapor deposition (e.g., catalyst chemical vapor deposition), photochemical vapor deposition, plasma chemical vapor deposition (e.g., capacitively coupled plasma, inductively coupled plasma, surface wave plasma, electron cyclotron resonance, dual magnetron, atomic layer stacking, etc.), and organometallic vapor deposition.
[0054] The thickness of the inorganic vapor-deposited layer (X') varies depending on the type of components constituting the inorganic vapor-deposited layer, and is preferably 0.002 to 0.5 μm, more preferably 0.005 to 0.2 μm, and even more preferably 0.01 to 0.1 μm. Within this range, a thickness that results in good barrier properties and mechanical properties for the multilayer structure is desired. If the thickness of the inorganic vapor-deposited layer (X') is 0.002 μm or more, it tends to exhibit good barrier properties against oxygen and water vapor. Furthermore, if the thickness of the inorganic vapor-deposited layer (X') is 0.5 μm or less, it tends to maintain its barrier properties after bending.
[0055] As the substrate (X), one type of substrate can be used alone, or two or more types of substrates can be used in combination. When there are multiple substrates (X), the individual substrates (X) can be the same or different. The number of layers of the substrate (X) can be one or more layers, or two or more layers. For example, the number of layers of the substrate (X) is one or more layers and three or less, preferably one or more layers and two or less, and more preferably one layer.
[0056] [Layer (Y)]
[0057] Layer (Y) comprises the reaction product (D) of a metal oxide (A) and an inorganic phosphorus compound (BI). In the multilayer structure of the present invention, layer (Y) functions as a barrier layer; therefore, by including layer (Y) in the multilayer structure of the present invention, it tends to exhibit good barrier properties. Furthermore, by using an appropriate method to form layer (Y), the image sharpness of the multilayer structure can be made to be 90% or more.
[0058] (Metal oxide containing aluminum atoms (A))
[0059] The metal atoms constituting the metal oxide (A) (sometimes collectively referred to as "metal atoms (M)") are typically at least one metal atom selected from those belonging to Groups 2 to 14 of the periodic table, and at least include aluminum atoms. The metal atom (M) is preferably an aluminum atom alone, but may include aluminum atoms and other metal atoms. It should be noted that two or more metal oxides (A) can be used in combination. Examples of metal atoms other than aluminum atoms include, for example, metals from Group 2 of the periodic table such as magnesium and calcium; metals from Group 12 of the periodic table such as zinc; metals from Group 13 of the periodic table; metals from Group 14 of the periodic table such as silicon; transition metals such as titanium and zirconium. It should be noted that silicon is sometimes classified as a half-metal, but in this specification, silicon is included as a metal. From the viewpoint of processability and excellent gas barrier properties of the resulting multilayer structure, at least one metal atom (M) selected from titanium and zirconium is preferred as the metal atom (M) that can be used in combination with aluminum.
[0060] The proportion of aluminum atoms in the metal atoms (M) is preferably 50 mol% or more, more preferably 70 mol% or more, even more preferably 90 mol% or more, and can be 95 mol% or more, or may be substantially composed of only aluminum atoms. Examples of metal oxides (A) include metal oxides manufactured by methods such as liquid-phase synthesis, gas-phase synthesis, and solid-state pulverization.
[0061] (A compound (E) containing a metal atom (M) bonded to a hydrolyzable characteristic group)
[0062] The metal oxide (A) can be a hydrolysis condensate of a compound (E) (hereinafter sometimes abbreviated as "compound (E)") containing a metal atom (M) bonded to a hydrolyzable characteristic group. Examples of such characteristic groups include halogen atoms, NO3, alkoxy groups with 1 to 9 carbon atoms optionally having substituents, aryloxy groups with 6 to 9 carbon atoms optionally having substituents, acyloxy groups with 2 to 9 carbon atoms optionally having substituents, alkenoxy groups with 3 to 9 carbon atoms optionally having substituents, β-diketone groups with 5 to 15 carbon atoms optionally having substituents, or diacylmethyl groups with 1 to 9 carbon atoms optionally having substituents. The hydrolysis condensate of compound (E) can essentially be considered as a metal oxide (A). Therefore, in this specification, the hydrolysis condensate of compound (E) is sometimes referred to as "metal oxide (A)". That is, in this specification, "metal oxide (A)" can be regarded as "hydrolysis condensate of compound (E)" or "hydrolysis condensate of compound (E)" can be regarded as "metal oxide (A)".
[0063] From the perspective of easy control of the reaction with inorganic phosphorus compound (BI) and the excellent gas barrier properties of the resulting multilayer structure, compound (E) preferably includes compound (Ea) containing aluminum atoms, as described later.
[0064] Examples of compounds (Ea) include aluminum chloride, aluminum nitrate, aluminum acetate, tris(2,4-pentanedione), aluminum triethanolamine, aluminum triethanolamine, aluminum tri-n-propoxide, aluminum triisopropoxide, aluminum tri-n-butoxide, aluminum trisec-butoxide, and aluminum tritert-butoxide, among which aluminum triisopropoxide and aluminum trisec-butoxide are preferred. Two or more compounds (Ea) may be used in combination as compound (E).
[0065] In addition, compound (E) may contain compounds (Eb) that contain metal atoms (M) other than aluminum. Examples of compounds (Eb) include titanium compounds such as tetra(2,4-pentanedione)titanium, tetraethanoltitanium, tetraethanoltitanium, tetraisopropoxidetitanium, tetran-butoxidetitanium, and tetra(2-ethylhexanol)titanium; and zirconium compounds such as tetra(2,4-pentanedione)zirconium, tetran-propoxidezirconium, and tetran-butoxidezirconium. These compounds may be used individually or in combination of two or more compounds (Eb).
[0066] The proportion of compound (Ea) in compound (E) is not particularly limited, but is preferably 80 mol% or more, more preferably 90 mol% or more, even more preferably 95 mol% or more, and can be 100 mol%.
[0067] By hydrolyzing compound (E), at least a portion of the hydrolyzable characteristic groups of compound (E) are converted into hydroxyl groups. Then, by condensing the hydrolysate, metal atoms (M) are bonded via oxygen atoms (O) to form a compound. Repeating this condensation process forms a compound that is essentially a metal oxide. It should be noted that hydroxyl groups are typically present on the surface of the metal oxide (A) formed in this manner.
[0068] In this specification, compounds in which the ratio of [the number of moles of oxygen atoms (O) bonded only to the metal atom (M)] / [the number of moles of metal atoms (M)] is 0.8 or more are defined as being included in metal oxides (A). Here, oxygen atoms (O) bonded only to the metal atom (M) refer to oxygen atoms (O) in the structure represented by MOM, excluding oxygen atoms (O) bonded to both the metal atom (M) and hydrogen atoms (H) as in the structure represented by MOH. The aforementioned ratio of the metal oxide (A) is preferably 0.9 or more, more preferably 1.0 or more, and even more preferably 1.1 or more. There is no particular upper limit to this ratio, and if the valence of the metal atom (M) is denoted as n, it is usually expressed as n / 2.
[0069] For the aforementioned hydrolysis-condensation to occur, it is crucial that the compound (E) possesses hydrolyzable characteristic groups. Without these groups bonded, the hydrolysis-condensation reaction either does not occur or is extremely slow, making it difficult to prepare the target metal oxide (A).
[0070] The hydrolysis condensate of compound (E) can be manufactured, for example, by a method employed in the known sol-gel process, and from a specific raw material. This raw material can be at least one selected from compound (E), a partially hydrolyzed product of compound (E), a completely hydrolyzed product of compound (E), a compound formed by the partial hydrolysis condensation of compound (E), and a compound formed by the condensation of a portion of the completely hydrolyzed product of compound (E).
[0071] It should be noted that the metal oxide (A) supplied for mixing with the inorganic phosphorus compound (BI) contained herein (inorganic phosphorus compound (BI) or a composition containing inorganic phosphorus compound (BI)) is preferably substantially free of phosphorus atoms.
[0072] (Inorganic phosphorus compounds (BI))
[0073] Inorganic phosphorus compounds (BI) contain sites capable of reacting with metal oxides (A), typically containing multiple such sites, preferably 2 to 20. These sites include those capable of condensation reactions with functional groups (e.g., hydroxyl groups) present on the surface of the metal oxide (A), such as halogen atoms directly bonded to phosphorus atoms, and oxygen atoms directly bonded to phosphorus atoms. The functional groups (e.g., hydroxyl groups) present on the surface of the metal oxide (A) are typically bonded to the metal atoms (M) constituting the metal oxide (A).
[0074] Examples of inorganic phosphorus compounds (BI) include phosphoric acid, diphosphoric acid, triphosphoric acid, polyphosphoric acid obtained by condensation of four or more molecules of phosphoric acid, phosphorous acid, phosphonic acid, phosphonium phosphonate, trivalent phosphonic acid, and other oxyacids of phosphorus, as well as their salts (e.g., sodium phosphate) and their derivatives (e.g., halides (e.g., phosphoryl chloride), dehydrated products (e.g., phosphorus pentoxide)). One type of inorganic phosphorus compound (BI) can be used alone, or two or more can be used in combination. From the viewpoint of improving the stability of the coating solution (S) described later and the gas barrier properties of the resulting multilayer structure, it is preferable to use phosphoric acid alone or in combination with other inorganic phosphorus compounds. When using phosphoric acid in combination with other inorganic phosphorus compounds, it is preferable that 50 mol% or more of the inorganic phosphorus compound (BI) is phosphoric acid.
[0075] (Reaction product (D))
[0076] The reaction product (D) is obtained by reacting a metal oxide (A) with an inorganic phosphorus compound (BI). Compounds formed by reacting the metal oxide (A) with the inorganic phosphorus compound (BI) with further compounds are also included in the reaction product (D).
[0077] In the infrared absorption spectrum of layer (Y), 800–1400 cm⁻¹ -1 The maximum absorption wavenumber in the region is preferably between 1080 and 1130 cm⁻¹. -1 The range is as follows. For example, in the reaction of a metal oxide (A) with an inorganic phosphorus compound (BI) to form a reaction product (D), the metal atom (M) from the metal oxide (A) and the phosphorus atom (P) from the inorganic phosphorus compound (BI) form a bond denoted as MOP via an oxygen atom (O). As a result, a characteristic absorption band originating from this bond is generated in the infrared absorption spectrum of the reaction product (D). This band is located in the range of 1080–1130 cm⁻¹. -1 When a characteristic absorption band based on MOP bonds is observed in the region, the resulting multilayer structure exhibits excellent gas barrier properties. In particular, this characteristic absorption band is observed in the 800–1400 cm⁻¹ range, where absorption from bonds between various atoms and oxygen atoms is typically observed. -1When the strongest absorption occurs within a certain region, the resulting multilayer structure exhibits superior gas barrier properties.
[0078] In contrast, when a metal compound (E) or metal salt is premixed with an inorganic phosphorus compound (BI) and then subjected to hydrolysis and condensation, the metal atoms from the metal compound and the phosphorus atoms from the inorganic phosphorus compound (BI) mix and react approximately uniformly to form a complex. In this case, the infrared absorption spectrum shows a concentration of 800–1400 cm⁻¹. -1 The maximum absorption wavenumber in the region will deviate from 1080–1130 cm⁻¹ -1 The range.
[0079] In the infrared absorption spectrum of layer (Y), from the viewpoint of the gas barrier properties of the resulting multilayer structure, 800–1400 cm⁻¹ -1 The half-width of the maximum absorption band within the region is preferably 200 cm. -1 The following is a preferred value: 150cm -1 Hereinafter, 100cm is further preferred. -1 The following is particularly preferred: 50cm -1 the following.
[0080] The infrared absorption spectrum of layer (Y) can be obtained using a Fourier transform infrared spectrophotometer (Spectrum One, manufactured by PerkinElmer Co., Ltd.) at a wavelength of 800–1400 cm⁻¹. -1 The measurement area is used, and the measurement is performed using the attenuated total reflection method. In cases where the aforementioned methods cannot be used, the measurement can be performed using reflection measurement methods such as reflection absorption method, external reflection method, attenuated total reflection method, or transmission measurement methods such as scraping a layer from a multilayer structure (Y), Neujoul method, or tablet method, but is not limited to these methods.
[0081] Additionally, layer (Y) may locally contain non-reactive metal oxides (A) and / or inorganic phosphorus compounds (BI).
[0082] In layer (Y), the molar ratio of metal atoms derived from metal oxide (A) to phosphorus atoms derived from inorganic phosphorus compound (BI) is preferably in the range of [metal atoms derived from metal oxide (A)]:[phosphorus atoms derived from inorganic phosphorus compound (BI)] = 1.0:1.0 to 3.6:1.0, more preferably in the range of 1.1:1.0 to 3.0:1.0. Excellent gas barrier properties can be obtained within this range. This molar ratio of layer (Y) can be adjusted by the mixing ratio of metal oxide (A) and inorganic phosphorus compound (BI) in the coating liquid (S) used to form layer (Y). This molar ratio of layer (Y) is generally the same as the ratio of coating liquid (S).
[0083] The thickness of layer (Y) (the total thickness of all layers (Y) when the multilayer structure has two or more layers (Y)) is preferably 0.05 to 4.0 μm, more preferably 0.1 to 2.0 μm. By thinning layer (Y), the dimensional changes of the multilayer structure during processing such as printing and lamination can be minimized. Furthermore, due to the increased flexibility of the multilayer structure, its mechanical properties can be made closer to those of the substrate itself. From the viewpoint of gas barrier properties, the thickness of each layer (Y) is preferably 0.05 μm or more, more preferably 0.1 μm or more. The thickness of each layer (Y) is preferably 2.0 μm or less, more preferably 1.0 μm or less. The thickness of layer (Y) can be controlled according to the concentration of the coating liquid (S) used to form layer (Y) (described later) or its coating method. The thickness of layer (Y) can be determined by observing the cross-section of the multilayer structure using a scanning electron microscope or a transmission electron microscope.
[0084] The number of layers (Y) can be one or more. Having two or more layers (Y) tends to improve barrier properties. The number of layers (Y) can be two. When there are two or more layers (Y), it is preferable to have layers (Y) on both sides of each substrate (X). When there are two or more layers (Y), the lamination method is not particularly limited; they can be directly placed on one or both sides of the substrate (X), or the multilayer structure containing the layers (Y) can be bonded using the adhesive layer (I) described later.
[0085] In addition to the aforementioned components (metal oxide (A), inorganic phosphorus compound (BI), and their reaction products (D)), layer (Y) may also contain other components. Examples of other components that may be included in layer (Y) include, for instance, polymers (F) having at least one functional group selected from carbonyl, hydroxyl, carboxyl, carboxylic anhydride, and carboxyl groups (hereinafter sometimes abbreviated as "polymer (F)"), organophosphorus compounds (BO), resin compositions (V) containing crosslinking agents, inorganic acid metal salts such as carbonates, hydrochlorides, nitrates, bicarbonates, sulfates, bisulfates, and borates; organic acid metal salts such as oxalates, acetates, tartrates, and stearates; metal complexes such as cyclopentadienyl metal complexes (e.g., dioctene) and cyano metal complexes (e.g., Prussian blue); layered clay compounds, crosslinking agents, polymers other than polymer (F), plasticizers, antioxidants, ultraviolet absorbers, flame retardants, etc. The content of the aforementioned other components in layer (Y) of the multilayer structure is preferably 50% by mass or less, more preferably 20% by mass or less, further preferably 10% by mass or less, particularly preferably 5% by mass or less, and can be 4% by mass or less, 3% by mass or less, 2% by mass or less, 1% by mass or less, or 0% by mass (excluding other components). From the viewpoint of higher clarity, the multilayer structure of the present invention preferably has a low content of other components.
[0086] (Polymer(F))
[0087] Polymer (F) has at least one functional group selected from carbonyl, hydroxyl, carboxyl, carboxylic anhydride, and carboxyl salts. Polymer (F) is preferably a polymer having at least one functional group selected from hydroxyl and carboxyl.
[0088] Examples of polymers (F) include polyethylene glycol; polyvinyl alcohol, modified polyvinyl alcohol containing 1 to 50 mol% of α-olefin units with 4 or fewer carbon atoms, polyvinyl alcohol acetal (polyvinyl butyral, etc.), and other polyvinyl alcohol-based polymers; polysaccharides such as cellulose and starch; (meth)acrylic acid-based polymers such as poly(meth)acrylate, poly(meth)acrylic acid, and ethylene-acrylic acid copolymers; and maleic acid-based polymers such as hydrolysates of ethylene-maleic anhydride copolymers, hydrolysates of styrene-maleic anhydride copolymers, and hydrolysates of isobutylene-maleic anhydride alternating copolymers. Polyethylene glycol or polyvinyl alcohol-based polymers are preferred.
[0089] Polymer (F) can be a homopolymer of monomers having polymerizable groups, a copolymer of two or more monomers, or a copolymer of a monomer having at least one functional group selected from carbonyl, hydroxyl, carboxyl, carboxylic anhydride, and carboxyl salts with a monomer that does not have that functional group. It should be noted that two or more polymers (F) can be used in combination as polymer (F).
[0090] The molecular weight of polymer (F) is not particularly limited. However, in order to obtain a multilayer structure with better gas barrier properties and mechanical strength, the weight-average molecular weight of polymer (F) is preferably 5,000 or more, more preferably 8,000 or more, and even more preferably 10,000 or more. The upper limit of the weight-average molecular weight of polymer (F) is not particularly limited, for example, it is 1,500,000 or less.
[0091] From the viewpoint of maintaining the appearance of the multilayer structure, the content of polymer (F) in layer (Y) is preferably less than 50% by mass, more preferably less than 20% by mass, even more preferably less than 10% by mass, and can be 0% by mass. The polymer (F) may or may not react with the components in layer (Y).
[0092] (organophosphorus compounds (BO))
[0093] The organophosphorus compound (BO) is preferably a polymer (BOa) having multiple phosphorus atoms or an organophosphorus compound (BOb) described later.
[0094] (Polymers with multiple phosphorus atoms (BOa))
[0095] Examples of functional groups containing phosphorus atoms in the polymer (BOa) include phosphate groups, phosphite groups, phosphonic acid groups, phosphonium phosphonate groups, trivalent phosphonic acid groups, and functional groups derived from them (e.g., salts, (partial) ester compounds, halides (e.g., chlorides), dehydrates), etc., among which phosphate groups and phosphonic acid groups are preferred, and phosphonic acid groups are more preferred.
[0096] Examples of polymers (BOa) include, for instance, phosphoryl (meth)acrylate polymers such as 6-[(2-phosphorylacetyl)oxy]hexyl acrylate, 2-phosphoryloxyethyl methacrylate, phosphoryl methyl methacrylate, 11-phosphoryl undecyl methacrylate, and 1,1-diphosphoryl ethyl methacrylate; vinyl phosphonic acid polymers such as 2-propen-1-phosphonic acid, 4-vinylbenzylphosphonic acid, and 4-vinylphenylphosphonic acid; vinyl hypophosphonic acid polymers such as 4-vinylbenzyl hypophosphonic acid; and phosphorylated starch. The polymer (BOa) can be a homopolymer of a monomer having at least one functional group containing a phosphorus atom, or a copolymer of two or more monomers. Furthermore, as a polymer (BOa), two or more polymers formed from a single monomer can be used in combination. Preferably, polymers of phosphoryl (meth)acrylates and polymers of vinyl phosphonic acids are used; more preferably, polymers of vinyl phosphonic acids are used; and even more preferably, polyvinylphosphonic acid is used. Alternatively, the polymer (BOa) can also be obtained by hydrolysis after homopolymerization or copolymerization of vinylphosphonic acid derivatives such as vinylphosphonic acid halides or vinylphosphonic esters.
[0097] Furthermore, the polymer (BOa) can be a copolymer of a monomer having at least one functional group containing a phosphorus atom and other vinyl monomers. Examples of other vinyl monomers capable of copolymerizing with monomers having functional groups containing phosphorus atoms include (meth)acrylic acid, (meth)acrylates, acrylonitrile, methacrylonitrile, styrene, nucleosubstituted styrene, alkyl vinyl ethers, alkyl vinyl esters, perfluoroalkyl vinyl ethers, perfluoroalkyl vinyl esters, maleic acid, maleic anhydride, fumaric acid, itaconic acid, maleimide, phenylmaleimide, etc., among which (meth)acrylates, acrylonitrile, styrene, maleimide, and phenylmaleimide are preferred.
[0098] To obtain a multilayer structure with excellent bending resistance, the proportion of structural units derived from monomers having functional groups containing phosphorus atoms in all structural units of the polymer (BOa) is preferably 10 mol% or more, more preferably 40 mol% or more, further preferably 70 mol% or more, particularly preferably 90 mol% or more, and can be 100 mol%.
[0099] The molecular weight of the polymer (BOa) is not particularly limited, but the number average molecular weight is preferably in the range of 1,000 to 100,000. If the number average molecular weight is in this range, it is possible to achieve both the improved bending resistance of the multilayer structure of the present invention and the viscosity stability of the coating liquid (S) when using it.
[0100] When a polymer (BOa) is included in the layer (Y) of a multilayer structure, the ratio of the mass of the polymer (BOa) in layer (Y) to the mass of the inorganic phosphorus compound (BI), WBOa / WBI, preferably satisfies the relationship 0.01 / 99.99 ≤ WBOa / WBI < 6.00 / 94.00. From the viewpoint of excellent barrier performance, it is more preferable to satisfy the relationship 0.10 / 99.90 ≤ WBOa / WBI < 4.50 / 95.50, even more preferably to satisfy the relationship 0.20 / 99.80 ≤ WBOa / WBI < 4.00 / 96.00, and particularly preferably to satisfy the relationship 0.50 / 99.50 ≤ WBOa / WBI < 3.50 / 96.50. That is, compared with trace amounts where WBOa is 0.01 or more and less than 6.00, it is preferable to use a large amount where WBI is greater than 94.00 and less than 99.99. It should be noted that even if the inorganic phosphorus compound (BI) and / or organophosphorus compound (BOa) in layer (Y) react, the portion of the inorganic phosphorus compound (BI) and / or organophosphorus compound (BOa) constituting the reaction product (D) will be considered as inorganic phosphorus compound (BI) and / or organophosphorus compound (BOa). In this case, the mass of the inorganic phosphorus compound (BI) and / or organophosphorus compound (BOa) used to form the reaction product (D) (the mass of the inorganic phosphorus compound (BI) and / or organophosphorus compound (BOa) before the reaction) is included in the mass of the inorganic phosphorus compound (BI) and / or organophosphorus compound (BOa) in layer (Y).
[0101] (Organophosphorus compounds (BOb))
[0102] In organophosphorus compounds (BOb), phosphorus atoms with at least one hydroxyl group are bonded to polar groups via alkylene chains or polyoxyalkylene chains having 3 to 20 carbon atoms. Compared to metal oxides (A), inorganic phosphorus compounds (BI), and their reaction products (D), organophosphorus compounds (BOb) have lower surface free energy and segregate towards the surface during the precursor formation of layer (Y). As a result, the flexural strength of the multilayer structure of the present invention and the adhesion between layer (Y) and the layers to be directly laminated are sometimes improved.
[0103] Examples of organophosphorus compounds (BOb) include 3-hydroxypropylphosphonic acid, 4-hydroxybutylphosphonic acid, 5-hydroxypentylphosphonic acid, 6-hydroxyhexylphosphonic acid, 7-hydroxyheptylphosphonic acid, 8-hydroxyoctylphosphonic acid, 9-hydroxynonylphosphonic acid, 10-hydroxydecylphosphonic acid, 11-hydroxyundecylphosphonic acid, 12-hydroxydodecylphosphonic acid, 13-hydroxytetrazylphosphonic acid, 14-hydroxytetradecylphosphonic acid, 15-hydroxypentadecanylphosphonic acid, and 16-hydroxyhexadecane. Phosphonic acid, 17-hydroxyheptadecylphosphonic acid, 18-hydroxyoctadecylphosphonic acid, 19-hydroxynonadecanylphosphonic acid, 20-hydroxyeicosylphosphonic acid, 3-hydroxypropyl dihydrogen phosphate, 4-hydroxybutyl dihydrogen phosphate, 5-hydroxypentyl dihydrogen phosphate, 6-hydroxyhexyl dihydrogen phosphate, 7-hydroxyheptyl dihydrogen phosphate, 8-hydroxyoctyl dihydrogen phosphate, 9-hydroxynonyl dihydrogen phosphate, 10-hydroxydecyl dihydrogen phosphate, 11-hydroxyundecyl dihydrogen phosphate, 12-hydroxypropyl dihydrogen phosphate -Hydroxydodecyl phosphate, 13-hydroxytridecyl phosphate, 14-hydroxytetradecyl phosphate, 15-hydroxypentadecanyl phosphate, 16-hydroxyhexadecyl phosphate, 17-hydroxyheptadecyl phosphate, 18-hydroxyoctadecyl phosphate, 19-hydroxynonadecanyl phosphate, 20-hydroxyeicosyl phosphate, 3-carboxypropylphosphonic acid, 4-carboxybutylphosphonic acid, 5-carboxypentylphosphonic acid, 6-carboxyhexylphosphonic acid Phosphonic acids, including 7-carboxyheptaylphosphonic acid, 8-carboxyoctylphosphonic acid, 9-carboxynonylphosphonic acid, 10-carboxydecylphosphonic acid, 11-carboxyundecylphosphonic acid, 12-carboxydodecylphosphonic acid, 13-carboxytridedecylphosphonic acid, 14-carboxytetradecylphosphonic acid, 15-carboxypentadecanylphosphonic acid, 16-carboxyhexadecylphosphonic acid, 17-carboxyheptadecylphosphonic acid, 18-carboxyoctadecylphosphonic acid, 19-carboxynonadecanylphosphonic acid, and 20-carboxyeicosylphosphonic acid, can be used alone or in combination of two or more.
[0104] When an organophosphorus compound (BOb) is contained in a layer (Y) of a multilayer structure, the ratio of the molar number of the organophosphorus compound (BOb) in layer (Y), MBOb, to the molar number of the inorganic phosphorus compound (BI), MBI, preferably satisfies 1.0 × 10⁻⁶. -4 ≤MBOb / MBI≤2.0×10 -2 The relationship is more preferably satisfied with 3.5×10 -4 ≤MBOb / MBI≤1.0×10 -2 The relationship is further optimized to satisfy 5.0×10 -4 ≤MBOb / MBI≤6.0×10 -3 The relationship.
[0105] When layer (Y) contains an organophosphorus compound (BOb), the ratio of carbon atoms to aluminum atoms (C / Al ratio) on the surface of layer (Y) of the multilayer structure not in contact with the substrate (X) within a range of ~5 nm, as measured by X-ray photoelectron spectroscopy (XPS), is preferably in the range of 0.1 to 15.0, more preferably in the range of 0.3 to 10.0, and particularly preferably in the range of 0.5 to 5.0. By keeping the C / Al ratio of the surface of layer (Y) within the aforementioned range, the adhesion between layer (Y) and adjacent layers is sometimes improved.
[0106] (Resin composition (V) containing crosslinking agent)
[0107] By including layer (Y) in a resin composition (V) containing a crosslinking agent, flexural strength can sometimes be improved. The resin composition (V) containing the crosslinking agent is composed of a hydroxyl-containing resin and a crosslinking agent. Examples of the aforementioned hydroxyl-containing resin include hydroxyl-containing epoxy resins, hydroxyl-containing polyester resins, hydroxyl-containing (meth)acrylic resins, hydroxyl-containing polyurethane resins, vinyl alcohol resins, and polysaccharides. Preferably, it contains vinyl alcohol resins or polysaccharides, more preferably vinyl alcohol resins, and even more preferably polyvinyl alcohol resins. As the aforementioned crosslinking agent, silicone compounds, organotitanium compounds, or organozirconium compounds having glycidyl groups can be suitably used. The mass ratio of the aforementioned hydroxyl-containing resin to the aforementioned crosslinking agent (hydroxyl-containing resin / crosslinking agent) is preferably 2.0 or more and 200 or less, more preferably 9.0 or more and 60 or less.
[0108] [Layer (W)]
[0109] In the multilayer structure of the present invention, a layer (W) comprising at least one selected from polymer (F), organophosphorus compound (BO), and resin composition (V) containing a crosslinking agent can be directly laminated on the side of layer (Y) opposite to the substrate (X). By including layers (W) in the multilayer structure, the bending resistance or the adhesion to the adhesive layer (I') described later is sometimes improved. From the viewpoint of clarity of the multilayer structure, it is sometimes preferable to not include layers (W).
[0110] When the multilayer structure of the present invention includes layers (W), it is preferable that layers (W) and layers (Y) are directly stacked. The polymer (F), organophosphorus compound (BO), and resin composition (V) containing a crosslinking agent that may be included in layers (W) are suitably configured as described above.
[0111] Layer (W) may also contain other components, such as inorganic acid metal salts like carbonates, hydrochlorides, nitrates, bicarbonates, sulfates, bisulfates, and borates; organic acid metal salts like oxalates, acetates, tartrates, and stearates; metal complexes such as cyclopentadienyl metal complexes (e.g., dioctene) and cyano metal complexes (e.g., Prussian blue); layered clay compounds; crosslinking agents; polymers other than polymers (BOa) and (F); plasticizers; antioxidants; ultraviolet absorbers; and flame retardants. The content of the aforementioned other components in layer (W) is preferably 20% by mass or less, more preferably 10% by mass or less, even more preferably 5% by mass or less, and may be 2% by mass or less, 1% by mass or less, or 0% by mass (excluding other components).
[0112] In the case where the multilayer structure of the present invention includes a layer (W), from the viewpoint that the bending resistance of the multilayer structure of the present invention is improved, the thickness of the layer (W) is preferably 0.005 μm or more. There is no particular upper limit to the thickness of the layer (W), but the improvement effect on bending resistance reaches saturation when it is 1.0 μm or more. Therefore, setting the upper limit of the thickness of the layer (W) to 1.0 μm is preferred from an economic point of view.
[0113] [Adhesive layer (I)]
[0114] The multilayer structure of the present invention may include an adhesive layer (I) between the substrate (X) and the layer (Y). By including the adhesive layer (I), the adhesion between the substrate (X) and the layer (Y) can sometimes be improved. Especially when the substrate (X) has a surface layer, it is preferable to provide the adhesive layer (I) between the surface layer and the layer (Y), and more preferably, the adhesive layer (I) is provided after surface treatment of the surface layer.
[0115] As for the adhesive constituting the adhesive layer (I), there are no particular limitations as long as it has the property of adhesion between the substrate (X) and the layer (Y), and examples include polyurethane adhesives and polyester adhesives. By adding a small amount of additives such as known silane coupling agents to these adhesives, the adhesion can sometimes be further improved. Examples of silane coupling agents include those having reactive groups such as isocyanate groups, epoxy groups, amino groups, urea groups, and mercapto groups.
[0116] As a polyurethane-based adhesive, known adhesives can be used, but a two-component polyurethane-based adhesive in which a polyisocyanate component and a polyol component are mixed and reacted is preferred. Commercially available products can be used as two-component polyurethane-based adhesives, such as Taklake (registered trademark) and Taknet (registered trademark) manufactured by Mitsui Chemicals Co., Ltd.
[0117] As polyester-based adhesives, known adhesives can be used. Commercially available examples include: Elitel (registered trademark) KT-0507, KT-8701, KT-8803, KT-9204, KA-5034, KA-3556, KA-1449, KA-5071S, KZA-1449S (all manufactured by Unichika Co., Ltd.); Biolonal (registered trademark) MD-1200, Biolonal MD-1480 (all manufactured by Toyobo Corporation); and Pesticide A124GP, Pesticide A684G (manufactured by Takamatsu Oils & Fats Co., Ltd.). Adding vinyl alcohol-based resins, especially polyvinyl alcohol, to polyester-based adhesives can sometimes further improve adhesion. When using both vinyl alcohol-based and polyester-based resins, from the viewpoint of maintaining good adhesion and exhibiting higher peel strength, the mass ratio (vinyl alcohol-based resin / polyester-based resin) is preferably 1 / 99 or higher and 50 / 50 or lower. From the viewpoint of affinity with vinyl alcohol-based resins, polyester-based resins containing carboxyl groups are preferred. Furthermore, when used as an adhesive, the polyester-based resin is preferably an aqueous dispersion. By making the polyester-based resin an aqueous dispersion, it tends to exhibit better affinity with polyvinyl alcohol-based resins.
[0118] The thickness of each adhesive layer (I) is preferably 0.001 to 10.0 μm, more preferably 0.003 to 5.0 μm, even more preferably 0.005 to 1.0 μm, even more preferably 0.007 to 0.1 μm, and particularly preferably 0.01 to 0.03 μm.
[0119] [Other Layers (J)]
[0120] In the multilayer structure of the present invention, in order to improve various properties (e.g., heat-sealing properties, barrier properties, mechanical properties), other layers (J) besides the substrate (X), layer (Y), layer (W), and adhesive layer (I) may be included. This multilayer structure of the present invention can be manufactured, for example, by laminating layer (Y) (as needed via adhesive layer (I)) onto the substrate (X), and then bonding or forming the other layers (J) directly or via adhesive layer (I') described later. Examples of other layers (J) include, but are not limited to, thermoplastic resin layers such as ink layers, polyolefin layers, and ethylene-vinyl alcohol copolymer resin layers.
[0121] In the case where the multilayer structure of the present invention includes an ink layer, examples of ink layers include a film obtained by drying a liquid containing a polyurethane resin containing a pigment (e.g., titanium dioxide) dispersed in a solvent, or a film obtained by drying an ink or a resist for forming electronic circuit wiring with a pigment-free polyurethane resin or other resin as the main agent. As for the coating method of the ink layer, in addition to gravure printing, various coating methods such as wire rod coating, spin coating, and die coating are possible. The thickness of the ink layer is preferably 0.5 to 10.0 μm, more preferably 1.0 to 4.0 μm.
[0122] By making the outermost layer of the multilayer structure of the present invention a polyolefin layer, heat-sealing properties or mechanical properties of the multilayer structure can be imparted. From the viewpoint of improving heat-sealing properties and mechanical properties, the polyolefin is preferably polypropylene or polyethylene. Furthermore, to improve the mechanical properties of the multilayer structure, it is preferable to laminate at least one film selected from films containing polyester, films containing polyamide, and films containing hydroxyl-containing polymers. From the viewpoint of improving mechanical properties, polyethylene terephthalate is preferred as the polyester, nylon-6 is preferred as the polyamide, and ethylene-vinyl alcohol copolymer is preferred as the hydroxyl-containing polymer.
[0123] Other layers (J) may be layers formed by extrusion coating lamination. The extrusion coating lamination method used in this invention is not particularly limited, and known methods may be used. In a typical extrusion coating lamination method, a laminate is produced by feeding molten thermoplastic resin into a T-die and cooling the thermoplastic resin extracted from the flat slit of the T-die.
[0124] Other extrusion coating lamination methods include sandwich lamination and tandem lamination. Sandwich lamination involves extruding molten thermoplastic resin onto one substrate and feeding a second substrate from a separate unwinding machine (winding machine) to bond the layers together. Tandem lamination connects two single-layer laminators to produce a five-layer laminate in a single operation.
[0125] [Adhesive layer (I')]
[0126] In the multilayer structure of the present invention, an adhesive layer (I') can sometimes be used to improve adhesion to other components (e.g., other layers (J)). The adhesive layer (I) can be composed of an adhesive resin. The adhesive constituting the adhesive layer (I') can also be any adhesive exemplified as an adhesive constituting the adhesive layer (I). As an adhesive resin for improving adhesion to the aforementioned other components, a two-component reactive polyurethane adhesive is preferred, which is a mixture of a polyisocyanate component and a polyol component and reacts them. In addition, by adding a small amount of additives such as a known silane coupling agent to the anchoring agent or adhesive, adhesion can sometimes be further improved. Examples of silane coupling agents include, but are not limited to, silane coupling agents having reactive groups such as isocyanate groups, epoxy groups, amino groups, urea groups, and mercapto groups. By bonding with other components, when processing such as printing or laminating the multilayer structure of the present invention, it is sometimes possible to more effectively suppress the deterioration of gas barrier properties or appearance, thereby improving the drop strength of protective sheets and electronic devices obtained using the multilayer structure of the present invention.
[0127] [The composition of multi-layered structures, etc.]
[0128] In the multilayer structure of the present invention, at least one set of substrates (X) and layers (Y) are stacked adjacent to each other. The substrates (X) and layers (Y) can be stacked directly or via an adhesive layer (I). When the substrate (X) has a surface layer and has a layer (Y) opposite to the surface layer, the substrates (X) and layers (Y) are preferably stacked via the adhesive layer (I). When the substrate (X) does not have a surface layer, the substrates (X) and layers (Y) are preferably stacked directly.
[0129] The following are examples of the configuration of the multilayer structure of the present invention, but the multilayer structure of the present invention is not limited to these. Multiple configurations can be combined from various specific examples. Here, " / " refers to lamination via adhesive layers or direct lamination.
[0130] (1) Layer (Y) / Substrate (X)
[0131] (2) Layer (Y) / Substrate (X) / Layer (Y)
[0132] (3) Substrate (X) / Layer (Y) / Layer (Y) / Substrate (X)
[0133] (4) Layer (Y) / Substrate (X) / Substrate (X) / Layer (Y)
[0134] (5) Layer (Y) / Substrate (X) / Layer (Y) / Substrate (X)
[0135] (6) Layer (Y) / Substrate (X) / Layer (Y) / Substrate (X) / Layer (Y)
[0136] In the above example, the substrate (X) preferably comprises a PET layer. Additionally, other layers (J) may be further included, which may be laminated onto the layer (Y) or substrate (X) via an adhesive layer (I'). The multilayer structure may consist only of the substrate layer (X) and the layer (Y), or it may consist only of the substrate layer (X), the layer (Y), and the adhesive layer (I).
[0137] The haze value of the multilayer structure of the present invention, measured according to JIS K7105:1981, is preferably 3% or less, more preferably 2.5% or less, and even more preferably 2.0% or less. By keeping the haze value below the aforementioned upper limit, the clarity of the multilayer structure is further improved. The haze value of the multilayer structure of the present invention can be 0.1% or more, or 0.5% or more. The haze value of the multilayer structure can be adjusted according to the type and thickness of the substrate (X), the thickness of the layer (Y), etc.
[0138] The water vapor transmission rate of the multilayer structure of the present invention at 40°C and 90% RH, as measured according to ISO 15106-5:2015, is preferably 1×10⁻⁶. -2 g / m 2 For days or less, 5.0 × 10 is more preferred. -3 g / m 2 For days or less, 3.0 × 10 is further preferred. -3 g / m 2 • less than 1 day. The water vapor transmission rate of the multilayer structure of the present invention can be 1.0 × 10⁻⁶. -5 g / m 2 For days or more, it can also be 1.0 × 10. -4 g / m 2 • Days or more. The water vapor transmission rate of a multi-layer structure can be adjusted according to the type and thickness of the substrate (X), the thickness of the layer (Y), etc.
[0139] [Manufacturing Method for Multilayer Structures]
[0140] The matters described with respect to the multilayer structure of the present invention can also be applied to the manufacturing method of the present invention, therefore repeated descriptions are sometimes omitted. Furthermore, the matters described with respect to the manufacturing method of the present invention can also be applied to the multilayer structure of the present invention.
[0141] As a method for manufacturing the multilayer structure of the present invention, an example of such a method is described below, which includes the following steps: step (I), which forms a precursor layer of layer (Y) by coating a coating liquid (S) containing a metal oxide (A), an inorganic phosphorus compound (BI) and a solvent onto at least one side of a substrate (X) and removing the solvent; and step (II), which forms layer (Y) by heat-treating the precursor layer of layer (Y), wherein the coating speed of the coating liquid (S) in step (I) is 0.03 cm / s or more and 2.5 cm / s or less relative to the coating width of 1 cm. In manufacturing a multilayer structure containing an organophosphorus compound (BO) or a polymer (F), the coating liquid (S) used in step (I) can contain an organophosphorus compound (BO) or a polymer (F) to form a layer (Y) containing an organophosphorus compound (BO) or a polymer (F). Alternatively, in step (III), by preparing a coating liquid (T) containing an organophosphorus compound (BO) or a polymer (F) and coating the surface of the precursor layer of the layer (Y) obtained in step (I) or the surface of the layer (Y) obtained in step (II), the organophosphorus compound (BO) or the polymer (F) can be impregnated into the layer (Y), and a layer (W) can be formed on the layer (Y). It should be noted that if an adhesive layer (I) is formed between the substrate (X) and the layer (Y), this manufacturing method can include a step of forming the adhesive layer (I) on the substrate (X) before step (I).
[0142] [Process (I)]
[0143] In step (I), a coating liquid (S) comprising a metal oxide (A), an inorganic phosphorus compound (BI), and a solvent is applied to at least one side of a substrate (X) at a speed of 0.03 cm / s or more and 2.5 cm / s or less relative to a coating width of 1 cm. The solvent is then removed to form a precursor layer for layer (Y). The coating liquid (S) is typically applied directly to at least one side of the substrate (X) or applied through an adhesive layer (I). That is, for a substrate (X) provided with an adhesive layer (I), the coating liquid (S) can be applied onto the adhesive layer (I). From the viewpoint of achieving good image clarity in the resulting multilayer structure, the coating speed of the coating liquid (S) is preferably 2.4 cm / s or less relative to a coating width of 1 cm, more preferably 2.0 cm / s or less. Furthermore, from the viewpoints of image clarity, productivity, and coating stability of the obtained multilayer structure, the coating speed of the coating liquid (S) is preferably 0.05 cm / s or more, and more preferably 0.2 cm / s or more, relative to the coating width of 1 cm.
[0144] The reason for the improved image clarity of the resulting multilayer structure based on the coating speed of the coating liquid (S) is uncertain. It can be speculated that when the coating speed exceeds 2.5 cm / s relative to the width of the substrate (X) by 1 cm, coating streaks are formed that are difficult to visually confirm. On the other hand, it can be speculated that if the coating speed is less than 0.03 cm / s relative to the width of 1 cm, the coating liquid (S) applied to the substrate tends to bounce off the substrate, making it impossible to properly construct the layer (Y). Furthermore, in order to achieve the effects of this invention, it is important to control the coating speed relative to the coating width within the aforementioned range during the coating of the coating liquid (S). The reason for this is uncertain, but it can be considered that the leveling range of the coating liquid (S) applied to the substrate (X) in the width direction is proportionally widened to the coating width, thus changing the leveling properties after coating.
[0145] The coating solution (S) is obtained by mixing a metal oxide (A), an inorganic phosphorus compound (BI), and a solvent. Specific methods for preparing the coating solution (S) include: mixing a dispersion of the metal oxide (A) with a solution containing the inorganic phosphorus compound (BI); adding the inorganic phosphorus compound (BI) to a dispersion of the metal oxide (A) and mixing the mixture, etc. The mixing temperature is preferably 50°C or lower, more preferably 30°C or lower, and even more preferably 20°C or lower. The coating solution (S) may contain other compounds (e.g., organophosphorus compounds (BO), polymers (F)), and may also contain, as needed, at least one acid compound (Q) selected from acetic acid, hydrochloric acid, nitric acid, trifluoroacetic acid, and trichloroacetic acid.
[0146] A dispersion of metal oxide (A) can be prepared, for example, by mixing compound (E), water, and an acid catalyst and organic solvent as needed, according to a known sol-gel method, to induce condensation or hydrolytic condensation of compound (E). When a dispersion of metal oxide (A) is obtained by inducing condensation or hydrolytic condensation of compound (E), the resulting dispersion can be subjected to specific treatments as needed (such as degelation in the presence of the aforementioned acid compound (Q)). The solvent used in preparing the dispersion of metal oxide (A) is not particularly limited, but alcohols such as methanol, ethanol, and isopropanol are preferred; water; or mixtures thereof.
[0147] As a solvent used in solutions containing inorganic phosphorus compounds (BI), it can be appropriately selected according to the type of inorganic phosphorus compound (BI), and water is preferred. Organic solvents (such as alcohols like methanol) may also be used as long as they do not impede the dissolution of the inorganic phosphorus compound (BI).
[0148] From the viewpoint of the storage stability of the coating solution and its coatability to the substrate (X), the solid content concentration of the coating solution (S) is preferably 1 to 20% by mass, more preferably 2 to 15% by mass, and even more preferably 3 to 10% by mass. The aforementioned solid content concentration can be calculated, for example, by dividing the mass of the solid content remaining after distilling off the solvent of the coating solution (S) by the mass of the coating solution (S) supplied for processing.
[0149] The viscosity of the coating liquid (S), measured using a Brookfield rotational viscometer (SB type viscometer: rotor No. 3, rotation speed: 60 rpm), is preferably 3000 mPa·s or less at the coating temperature, more preferably 2500 mPa·s or less, and even more preferably 2000 mPa·s or less. By keeping this viscosity below 3000 mPa·s, the leveling properties of the coating liquid (S) are improved, resulting in a multilayer structure with a superior appearance. Furthermore, the viscosity of the coating liquid (S) is preferably 50 mPa·s or more, more preferably 100 mPa·s or more, and even more preferably 200 mPa·s or more.
[0150] In the coating solution (S), the molar ratio of aluminum atoms to phosphorus atoms is preferably in the range of aluminum atoms:phosphorus atoms = 1.0:1.0 to 3.6:1.0, more preferably in the range of 1.1:1.0 to 3.0:1.0, and particularly preferably in the range of 1.11:1.00 to 1.50:1.00. The molar ratio of aluminum atoms to phosphorus atoms can be calculated by performing fluorescence X-ray analysis on the dried solids of the coating solution (S).
[0151] There are no particular limitations on the coating of the coating liquid (S), and known methods can be used. Examples of coating methods include, for instance, roller coating, gravure coating, screen printing, reverse coating, kiss coating, die coating, metering rod coating, sealing blade coating, and bar coating.
[0152] There are no particular limitations on the method for removing the solvent (drying process) after applying the coating liquid (S), and known drying methods can be used. Examples of drying methods include hot air drying, hot roller contact drying, infrared heating, and microwave heating.
[0153] The drying temperature is preferably lower than the flow initiation temperature of the substrate (X). The drying temperature after applying the coating liquid (S) can be, for example, 60°C or higher and about 180°C or lower, more preferably 60°C or higher and less than 140°C, further preferably 70°C or higher and less than 130°C, and particularly preferably 80°C or higher and less than 120°C. The drying time is not particularly limited, but is preferably 1 second or higher and less than 1 hour, more preferably 5 seconds or higher and less than 15 minutes, and further preferably 5 seconds or higher and less than 300 seconds. In particular, when the drying temperature is 100°C or higher (e.g., 100–140°C), the drying time is preferably 1 second or higher and less than 4 minutes, more preferably 5 seconds or higher and less than 4 minutes, and further preferably 5 seconds or higher and less than 3 minutes. When the drying temperature is lower than 100°C (e.g., 60–99°C), the drying time is preferably 3 minutes or higher and less than 1 hour, more preferably 6 minutes or higher and less than 30 minutes, and further preferably 8 minutes or higher and less than 25 minutes. If the drying conditions of the coating solution (S) are within the aforementioned range, there is a tendency to obtain a multilayer structure with better gas barrier properties. The solvent is removed by undergoing the aforementioned drying process, thereby forming a precursor layer of layer (Y).
[0154] In the case of a double-layer (Y) lamination on both sides of a substrate (X), a first layer (precursor layer of the first layer (Y)) is formed by, for example, applying a coating liquid (S) to one side of the substrate (X) and then removing the solvent. Next, a second layer (precursor layer of the second layer (Y)) is formed by applying the coating liquid (S) to the other side of the substrate (X) and then removing the solvent. The composition of the coating liquid (S) applied to each side can be the same or different.
[0155] [Process (II)]
[0156] In step (II), the precursor layer of layer (Y) formed in step (I) is heat-treated to form layer (Y). In step (II), a reaction to generate reaction product (D) is carried out. To ensure the reaction is complete, the heat treatment temperature is preferably 140°C or higher, more preferably 170°C or higher, even more preferably 180°C or higher, and particularly preferably 190°C or higher. If the heat treatment temperature is low, the time required to obtain a sufficient reaction rate will be longer, resulting in a decrease in productivity. The heat treatment temperature varies depending on the type of substrate (X), for example, when a thermoplastic resin film formed from a polyamide resin is used as the substrate (X), the heat treatment temperature is preferably 270°C or lower. In addition, when a thermoplastic resin film formed from a polyester resin is used as the substrate (X), the heat treatment temperature is preferably 240°C or lower. The heat treatment can be carried out in an air atmosphere, a nitrogen atmosphere, an argon atmosphere, etc. The heat treatment time is preferably 1 second to 1 hour, more preferably 1 second to 15 minutes, and even more preferably 5 to 300 seconds.
[0157] Process (II) preferably includes a first heat treatment process (II-1) and a second heat treatment process (II-2). When heat treatment is performed in two or more stages, the temperature of the second heat treatment (hereinafter referred to as the second heat treatment) is preferably higher than the temperature of the first heat treatment (hereinafter referred to as the first heat treatment), more preferably 15°C or more higher than the temperature of the first heat treatment, even more preferably 20°C or more higher, and particularly preferably 30°C or more higher.
[0158] Furthermore, from the viewpoint of obtaining a multilayer structure with good properties, the heat treatment temperature of step (II) (which is the first heat treatment temperature in the case of heat treatment in two or more stages) is preferably higher than the drying temperature of step (I), preferably 30°C or more higher, more preferably 50°C or more higher, even more preferably 55°C or more higher, and particularly preferably 60°C or more higher.
[0159] When heat treatment of process (II) is performed in two or more stages, the temperature of the first heat treatment is preferably 140°C or higher and less than 200°C, and the temperature of the second heat treatment is more preferably 180°C or higher and less than 270°C. The temperature of the second heat treatment is preferably higher than the temperature of the first heat treatment, more preferably 15°C or higher, and even more preferably 25°C or higher. Particularly when the heat treatment temperature is 200°C or higher, the heat treatment time is preferably 0.1 seconds to 10 minutes, more preferably 0.5 seconds to 15 minutes, and even more preferably 1 second to 3 minutes. When the heat treatment temperature is below 200°C, the heat treatment time is preferably 1 second to 15 minutes, more preferably 5 seconds to 10 minutes, and even more preferably 10 seconds to 5 minutes.
[0160] [Process (III)]
[0161] In the method for manufacturing the multilayer structure of the present invention, when using an organophosphorus compound (BO), a polymer (F), and / or other components, the following step (III) may be included: applying a coating liquid (T) obtained by mixing the organophosphorus compound (BO), the polymer (F), and / or other components, and a solvent onto the precursor layer of the layer (Y) obtained in step (I), the layer (Y) obtained in step (II), or the precursor layer of the layer (Y) after step (II-1), and subjecting it to a drying process. If step (III) is performed after step (II-1), it is preferable to perform step (II-2) after the drying process of step (III). In step (III), the amount of coating liquid (T) may be increased to form a layer (W) on the layer (Y).
[0162] The solvent used in the coating solution (T) can be appropriately selected according to the type of organophosphorus compound (BO), polymer (F) and / or other components, preferably alcohols such as methanol, ethanol, and isopropanol; water; or a mixture thereof.
[0163] From the viewpoint of the solution's storage stability and coatability, the concentration of solid components in the coating solution (T) is preferably 0.01 to 60% by mass, more preferably 0.1 to 50% by mass, and even more preferably 0.2 to 40% by mass. The concentration of solid components can be determined by the same method described for the coating solution (S).
[0164] There are no particular limitations on the method of applying coating liquid (T) in the same way as coating liquid (S), and known methods can be used.
[0165] The conditions for solvent removal (drying) after coating the coating liquid (T) in step (III) can be the same as the conditions for drying after coating the coating liquid (S) in step (I).
[0166] [Process (IV)]
[0167] The manufacturing method of the multilayer structure of the present invention may include the following step: before performing step (I), after performing surface treatment on the substrate (X) as needed, an adhesive layer (I) is then formed. More preferably, the manufacturing method may include the following step (IV): after applying a coating liquid (R) containing PVA-based resin, polyester-based resin and solvent onto the substrate (X), the solvent is removed to form the adhesive layer (I).
[0168] As a means of obtaining the coating solution (R), for example, PVA-based resin, polyester-based resin and solvent can be directly mixed, or a solution or dispersion containing PVA-based resin can be mixed with a solution or dispersion containing polyester-based resin. From the viewpoint of solution uniformity, it is preferable to obtain the coating solution (R) by mixing an aqueous solution of PVA-based resin with a dispersion of polyester-based resin.
[0169] There are no particular limitations on the solvent used in the coating liquid (R), but water is preferred as the main component, and it can be water alone. Other solvents used when water is the main component are preferably alcohols such as methanol, ethanol, and isopropanol.
[0170] From the viewpoint of the storage stability of the coating solution and its coatability to the substrate (X), the solid content concentration of the coating solution (R) is preferably 0.01 to 10% by mass. The aforementioned solid content concentration can be calculated, for example, by dividing the mass of the solid content remaining after distilling off the solvent of the coating solution (R) by the mass of the coating solution (R) supplied for processing.
[0171] There are no particular limitations on the coating of the coating liquid (R), and known methods can be used. Examples of coating methods include casting, dipping, roller coating, gravure coating, screen printing, reverse coating, spraying, kissing coating, die coating, metering rod coating, sealing knife coating, curtain coating, and bar coating.
[0172] There are no particular limitations on the solvent removal method for the coating liquid (R) after it has been applied to the substrate (X), and known drying methods can be used. Examples of drying methods include hot air drying, hot roller contact drying, infrared heating, and microwave heating.
[0173] [Protective films for electronic devices and electronic devices themselves]
[0174] The electronic device obtained using the multilayer structure of the present invention includes an electronic device body and a protective sheet protecting the surface of the electronic device body. The protective sheet of the electronic device of the present invention comprises the multilayer structure of the present invention. The protective sheet of the electronic device of the present invention may be composed solely of the multilayer structure of the present invention, or it may be composed of the multilayer structure of the present invention and other components. The protective sheet of the electronic device of the present invention has high barrier properties and high clarity. Therefore, by using the protective sheet of the present invention, it is possible to obtain an electronic device with less degradation under harsh environments and high image clarity. For example, in the case of a substrate film for electronic paper, it can be suitable as a protective material for the ink of electronic paper, which is easily affected by moisture.
[0175] The electronic device of the present invention can be a photoelectric conversion device, an information display device, or a lighting device. Examples of photoelectric conversion devices include various solar cells and other photoelectric conversion devices. Examples of information display devices include liquid crystal displays, organic EL displays, plasma displays, electronic paper, and other information display devices. Examples of lighting devices include LED lighting, organic EL lighting, and other lighting devices.
[0176] The electronic device of the present invention is particularly preferably used as a device comprising optical elements. The optical elements are appropriately selected according to the intended use of the electronic device according to the present invention. Here, the optical element in the present invention refers to an element having an optical function, such as, for example, an information display function, a light-emitting function, etc. When using an element having an information display function as the aforementioned optical element, the electronic device of the present invention can be used as an information display device; when using an element having a light-emitting function as the optical element, the electronic device of the present invention can be used as a light-emitting device (illumination device).
[0177] Examples of optical elements with information display functions include liquid crystal cells used in liquid crystal display devices, organic EL elements used in organic EL display devices, and electronic paper elements (particle-moving type, liquid crystal type, electrochemical type, etc.) used in electronic paper devices. Here, as the aforementioned optical elements, by using liquid crystal cells, the optical device of the present invention forms a liquid crystal display device; by using organic EL elements, an organic EL display device is formed; and by using electronic paper elements, an electronic paper device is formed.
[0178] There are no particular limitations on the aforementioned liquid crystal units, organic EL elements, and electronic paper components; generally known components can be used.
[0179] The multilayer structure of the present invention can also be used as a substrate film, such as a substrate film for LCDs, organic ELs, and electronic paper. In this case, the multilayer structure can serve as both a substrate and a protective sheet. Furthermore, the electronic device to which the protective sheet is applied is not limited to the examples described above, and can include, for example, IC tags, optical communication devices, and fuel cells.
[0180] The protective film of the electronic device of the present invention may include a surface protective layer disposed on one surface of a multilayer structure. As a surface protective layer, a resin-formed layer with high transparency and resistance to damage is preferred. Furthermore, the surface protective layer in the protective film of devices, such as solar cells, which are sometimes used outdoors, is preferably formed of a resin with high weather resistance (e.g., light resistance). Additionally, when protecting surfaces that require light transmission, a surface protective layer with high light transmittance is preferred. Examples of materials for the surface protective layer (surface protective film) include, for example, acrylic resins, polycarbonate, polyethylene terephthalate, polyethylene naphthalate, cellulose triacetate, cyclic olefin polymers, ethylene-tetrafluoroethylene copolymer (ETFE), polytetrafluoroethylene, 4-fluoroethylene-perchloroalkoxy copolymer, 4-fluoroethylene-6-fluoropropylene copolymer, 2-ethylene-4-fluoroethylene copolymer, poly(3-fluorochloroethylene), polyvinylidene fluoride, and polyvinyl fluoride.
[0181] To improve the durability of the surface protective layer, various additives (such as UV absorbers) can be added. A preferred example of a surface protective layer with high weather resistance is an acrylic resin layer containing a UV absorber. Examples of UV absorbers include, but are not limited to, benzotriazole, benzophenone, salicylate, cyanoacrylate, nickel, and triazine UV absorbers. Additionally, other stabilizers, light stabilizers, antioxidants, etc., can be used in combination.
[0182] Furthermore, to improve the durability of the surface protective layer, a weather-resistant coating, such as a hard coating, can be applied to the surface. There are no particular limitations on the type of coating; known materials can be used.
[0183] There are no particular limitations on the composition of the protective film; sometimes, for example, the following composition is suitable.
[0184] (1) Multi-layer structure
[0185] (2) Multilayer structure / adhesive layer / polyethylene terephthalate
[0186] (3) Multilayer structure / adhesive layer / cellulose triacetate
[0187] (4) Multilayer structure / adhesive layer / acrylic resin
[0188] (5) Multilayer structure / adhesive layer / polycarbonate
[0189] (6) Multilayer structure / adhesive layer / cyclic olefin polymer
[0190] (7) Multilayer structure / adhesive layer / ETFE
[0191] It should be noted that when the multilayer structure of the present invention is stacked with other materials, in order to protect the multilayer structure, it is sometimes preferable to arrange other materials as the outer side.
[0192] Example
[0193] Next, embodiments are given to illustrate the invention in more detail, but the invention is not limited to these embodiments at all, and those skilled in the art can make various modifications within the scope of the technical concept of the invention. The analysis and evaluation in the following embodiments and comparative examples are carried out as follows.
[0194] <Materials used in the examples and comparative examples>
[0195] • PET23-A: Biaxially stretched polyethylene terephthalate film; manufactured by Toray Industries, Inc., "Lumira (trademark) U403" (trade name), with surface layers on both sides, thickness of 23μm, image clarity of 94%, and thermal shrinkage rate in the MD direction of 2.16%.
[0196] • PET23-B: Biaxially stretched polyethylene terephthalate film; manufactured by Toray Industries, Inc., "Lumira (trademark) XW731C" (trade name), with a surface layer on one side, a thickness of 23μm, an image resolution of 93%, and a thermal shrinkage rate of 2.79% in the MD direction.
[0197] • PET23-C: Biaxially stretched polyethylene terephthalate film; manufactured by HYOSUNG, "RH210" (trade name), with surface layers on both sides, a thickness of 23μm, an image resolution of 94%, and a thermal shrinkage rate of 2.70% in the MD direction.
[0198] • PET23-D: Biaxially stretched polyethylene terephthalate film; manufactured by Toray Industries, Inc., "Lumira (trademark) S105" (trade name), thickness 23μm, image clarity 83%, MD direction heat shrinkage rate 3.00%.
[0199] • PET38: Biaxially stretched polyethylene terephthalate film; manufactured by Toray Industries, Inc., "Lumira (trademark) U483" (trade name), with surface layers on both sides, thickness of 38μm, image clarity of 94%, and thermal shrinkage rate in the MD direction of 2.05%.
[0200] • PET50: Biaxially stretched polyethylene terephthalate film; manufactured by Toray Industries, Inc., "Lumira (trademark) U403" (trade name), with surface layers on both sides, thickness of 50μm, image clarity of 94%, and thermal shrinkage rate in the MD direction of 2.04%.
[0201] • PET75: Biaxially stretched polyethylene terephthalate film; manufactured by Toray Industries, Inc., "Lumira (trademark) U483" (trade name), with surface layers on both sides, thickness of 75μm, image clarity of 93%, and thermal shrinkage rate in the MD direction of 2.08%.
[0202] • PET12: Biaxially stretched polyethylene terephthalate film; manufactured by Toray Industries, Inc., "Lumira (trademark) P60" (trade name), 12μm thick, image resolution 82%, MD direction heat shrinkage rate 3.12%.
[0203] The image sharpness and MD direction thermal shrinkage rate of the aforementioned materials were measured according to the methods described in the evaluation methods (5) Image sharpness and (2) MD direction thermal shrinkage rate.
[0204] <Evaluation Methods>
[0205] (1) Determination of the maximum absorption wavenumber (Imax) in infrared absorption spectra
[0206] The layers (Y) of the multilayer structures obtained in the examples and comparative examples were measured using a Fourier transform infrared spectrophotometer and the attenuated total reflectance method, and the 800–1400 cm⁻¹ region was calculated. -1 The maximum absorption wavenumber (Imax) within the region. The measurement conditions are as follows.
[0207] Device: Spectrum One manufactured by パーキンエルマー Co., Ltd.
[0208] Measurement mode: Attenuated total internal reflection method
[0209] Measurement area: 800~1400cm -1
[0210] (2) MD direction contraction rate
[0211] The substrate (X) used in the examples and comparative examples was cut into 12cm × 12cm pieces. A grid of 6cm × 6cm (36 grids) was drawn in the center of each grid, with each grid approximately 1cm (MD direction) × 1cm (TD direction). A measurement sample was prepared, and the length of each grid parallel to the MD direction was measured using vernier calipers. Next, the aforementioned measurement sample was placed in a dryer at 210°C for 3 minutes and then removed. The length of each grid parallel to the MD direction was measured again using vernier calipers. The shrinkage rate of each grid parallel to the MD direction before and after standing in the dryer was calculated, and their average value was taken as the shrinkage rate in the MD direction.
[0212] (3) Thickness
[0213] The multilayer structures obtained in the examples and comparative examples were cut using a focused ion beam (FIB) to prepare cross-sectional sections for observation. The prepared sections were fixed to a sample base using carbon tape, and platinum ion sputtering was performed for 30 seconds at an accelerating voltage of 30 kV. The cross-sections of the multilayer structures were observed using an electric field-release transmission electron microscope, and the thickness of each layer and the thickness of the multilayer structure were calculated. The measurement conditions are shown below. The thickness was calculated as the average of five measured values.
[0214] Device: JEM-2100F manufactured by Nippon Electronics Co., Ltd.
[0215] Accelerating voltage: 200kV
[0216] Multiplier: 250,000x
[0217] (4) Water vapor permeability
[0218] The multilayer structures obtained in the examples and comparative examples were installed in a water vapor transmission rate measuring device, and the water vapor transmission rate was measured using the differential pressure method according to ISO 15106-5:2015. The measurement conditions are shown below. The lower the water vapor transmission rate, the better the water vapor barrier performance.
[0219] Device: Deltaperm manufactured by Technolox
[0220] Temperature: 40℃
[0221] Humidity on the steam supply side: 90% RH
[0222] (5) Image clarity
[0223] The substrate (X) used in the examples and comparative examples, or the multilayer structure obtained in the examples and comparative examples, was mounted on an image sharpness measuring apparatus, and image sharpness was measured according to ISO 17221:2014. The measurement conditions are as follows, and the average of 5 measurements is taken as the measured value.
[0224] Apparatus: Image sharpness measuring instrument IC-T manufactured by Suga Testing Machines Co., Ltd.
[0225] Comb width: 0.25mm
[0226] (6) Haze
[0227] The multilayer structures obtained in the examples and comparative examples were mounted on a haze meter HR-100 (manufactured by Murakami Color Technology Research Institute Co., Ltd.), and haze was measured according to JIS K7105:1981. The measurement was performed 5 times, and the average value was taken as the measured value.
[0228] (7) Clarity
[0229] On the surface of any image display device, the protective sheet for electronic devices obtained in the embodiments and comparative examples is laminated onto the surface, and the ability to clearly observe the text displayed on the image display device is evaluated. The case where the text is clearly displayed is designated as A, the case where the ends of the text are slightly blurred is designated as B, and the case where the text is generally unclear is designated as C. Ten panel members evaluated each case, and the evaluation with the most majority was designated as the clarity evaluation. It should be noted that if there are multiple majority evaluations, all evaluations are recorded together.
[0230] (8) Oxygen permeability
[0231] The multilayer structures obtained in the examples and comparative examples were cut into 10mm × 10mm pieces. The cut multilayer structures were then mounted on an oxygen permeability measuring device, and the oxygen permeability was measured using the isobaric method. The measurement conditions are shown below.
[0232] Device: MOCON OX-TRAN2 / 21
[0233] Temperature: 20℃
[0234] Humidity on the oxygen supply side: 85% RH
[0235] Carrier gas side humidity: 85% RH
[0236] Carrier gas flow rate: 10 mL / min
[0237] Oxygen pressure: 1.0 atm
[0238] Carrier gas pressure: 1.0 atm
[0239] <Example of manufacturing coating liquid (S-1)>
[0240] 230 parts by mass of distilled water were heated to 70°C while stirring. Over one hour, 88 parts by mass of aluminum triisopropoxide were added dropwise to the distilled water, allowing the liquid temperature to slowly rise to 95°C. The resulting isopropanol was distilled off, thus initiating hydrolysis and condensation. 4.0 parts by mass of a 60% by mass aqueous nitric acid solution was added to the resulting liquid, and the mixture was stirred at 95°C for 3 hours, thereby degelating the aggregates of the hydrolyzed condensate. The liquid was then concentrated to a solids concentration of 10% by mass (calculated as alumina). 22.50 parts by mass of the resulting solution were then mixed with 54.29 parts by mass of distilled water and 18.80 parts by mass of methanol, and stirred until homogeneous, thus obtaining a dispersion. Next, while maintaining the liquid temperature at 15°C, 4.41 parts by mass of an 85% by mass aqueous phosphoric acid solution were added dropwise while stirring the dispersion. Then, 18.80 parts by mass of methanol solution were added dropwise, and the mixture was stirred continuously at 15°C until the viscosity reached 1,500 mPa·s, thus obtaining the target coating solution (S-1). The molar ratio of aluminum atoms to phosphorus atoms in the coating solution (S-1) was 1.15:1.00.
[0241] <Example of manufacturing coating liquid (R-1)>
[0242] A PVA aqueous solution was obtained by mixing 4.8 parts by weight of PVA "Clarepoval (registered trademark) 48-80" with 95.2 parts by weight of water and stirring at room temperature for 5 hours. Next, a coating solution (R-1) was obtained by mixing 0.8 parts by weight of polyester aqueous dispersion "Erytel (registered trademark) KA-5071S" (manufactured by Unichica Co., Ltd.), 1.2 parts by weight of the aforementioned PVA aqueous solution, 68.1 parts by weight of water, and 29.9 parts by weight of methanol and stirring for 1 hour.
[0243] <Example 1>
[0244] As the substrate (X-1), PET23-A (21cm wide) was used. A corona treatment device TEC-4AC manufactured by Kasuga Electric Co., Ltd. was used at 130W·min / m². 2The strength of the substrate was determined by surface treatment on one side. Using a bar coater, coating liquid (R-1) was applied to one side of the surface-treated substrate to a dried thickness of 10 nm. The coated substrate was dried at 140°C for 1 minute, forming an adhesive layer (I-1) on one side of the substrate. On the side of the substrate with the adhesive layer (I-1), coating liquid (S-1) was applied to a dried thickness of 0.4 μm using a bar coater at a coating speed of 12.6 cm / s (0.6 cm / s relative to a coating width of 1 cm). The coated substrate was dried at 120°C for 3 minutes and then heat-treated at 180°C for 1 minute to form a precursor layer of layer (Y-1) on the substrate. Then, using the same method, surface treatment was performed on the other side to form both the adhesive layer (I-1) and the precursor layer of layer (Y-1). The precursor layer with the obtained layer (Y-1) was heat-treated at 210°C for 1 minute to obtain a multilayer structure of layer (Y-1) (0.4 μm) / adhesive layer (I-1) (10 nm) / substrate (X-1) (23 μm) / adhesive layer (I-1) (10 nm) / layer (Y-1) (0.4 μm). Layer (Y-1) and the multilayer structure of the obtained multilayer structure were evaluated according to the methods described in the aforementioned evaluation methods (1), (3), (4), (5), (6), and (8). The results are shown in Table 1.
[0245] Six multilayer structures were prepared, and adhesive layers were formed on one side of each structure using two-component polyurethane adhesives ("Takelac (registered trademark) A-1102" manufactured by Mitsui Chemicals Co., Ltd. and "Takenet (registered trademark) A-3070" manufactured by Mitsui Chemicals Co., Ltd.). The materials described below were then laminated onto these adhesive layers to produce six protective sheets for electronic devices. The clarity of each protective sheet for electronic devices was evaluated according to the method described in the aforementioned evaluation method (7). The results are shown in Table 1. It should be noted that clarity 1 to clarity 6 in Table 1 refer to the evaluation of the protective sheets for electronic devices obtained by laminating with the materials described in 1. to 6.
[0246] 1. Lumira (trademark) U403 (manufactured by Toray Industries, 50μm thickness)
[0247] 2. Cosmosine SRF (trademark) (Made by Toyobo Co., Ltd., 80μm thick)
[0248] 3. Cellulose triacetate (TAC) membrane (manufactured by Conicaminodesa Corporation, 80μm thick)
[0249] 4. OXIS (trademark) PMMA (manufactured by Okura Kogyo Co., Ltd., thickness 40μm)
[0250] 5. Polycarbonate film (trademark) (manufactured by Teijin Corporation, thickness 70μm)
[0251] 6. ゼオノアフィルム (trademark) (manufactured by Japan ゼオン Co., Ltd., thickness 70μm)
[0252] <Example 2>
[0253] PET23-B was used instead of PET23-A in Example 1. No adhesive layer (I-1) was provided on the side without the surface layer. Otherwise, the protective sheet for the multilayer structure and electronic device was fabricated and evaluated using the same method as in Example 1. The results are shown in Table 1.
[0254] <Examples 3-6, Comparative Example 1>
[0255] The substrate (X) described in Table 1 was used instead of PET23-A used in Example 1. Otherwise, the same method as in Example 1 was used to fabricate and evaluate the protective sheets for multilayer structures and electronic devices. The results are shown in Table 1.
[0256] <Example 7>
[0257] One side of the PET23-A used in Example 1 was not surface-treated, and no adhesive layer (I-1) and layer (Y-1) were provided. A multilayer structure of layer (Y-1) (0.4 μm) / adhesive layer (I-1) (10 nm) / (surface-treated side) substrate (X-1) (23 μm) (non-surface-treated side) was fabricated. Otherwise, the multilayer structure and the protective sheet for the electronic device were fabricated and evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0258] <Examples 8-10, Comparative Examples 2, Comparative Example 3>
[0259] As described in Table 1, the coating speed of the coating liquid (S) in Example 1 was changed. Otherwise, the multilayer structure and the protective sheet for the electronic device were fabricated and evaluated using the same method as in Example 1. The results are shown in Table 1. It should be noted that in the multilayer structure of Comparative Example 3, the coating liquid (S) applied to the substrate was bounced off by the substrate, and the layer (Y) could not be uniformly constructed. Therefore, the evaluations of the aforementioned evaluation methods (4), (5), (6) and (8) were not performed.
[0260] <Comparative Example 4>
[0261] Using PET12 instead of PET23-A used in Example 1, the coating speed of the coating liquid (S) was varied as described in Table 1. Otherwise, using the same method as in Example 1, protective sheets for multilayer structures and electronic devices were fabricated and evaluated. The results are shown in Table 1.
[0262]
[0263] As shown in Table 1, the multilayer structures of Examples 1-10 exhibit high barrier properties and clarity. Furthermore, based on comparisons of Examples 1, 8-10 and Comparative Examples 2 and 3, it is evident that the coating speed of the coating liquid (S) used to form the Y layer significantly affects the image clarity of the resulting multilayer structures.
Claims
1. A multi-layer structure, which is a multi-layer structure having a substrate X and a layer Y. Layer Y contains reaction product D of a metal oxide A containing aluminum atoms and an inorganic phosphorus compound BI. Substrate X is adjacent to layer Y. The coating speed of the coating liquid (S) used to form layer Y is greater than or equal to 0.03 cm / s and less than or equal to 2.5 cm / s relative to a coating width of 1 cm. Substrate X is polyethylene terephthalate. The thermal shrinkage rate of substrate X in the MD direction after heating at 210°C for 1 minute is less than 2.90%. The content of components in layer Y, excluding metal oxide A, inorganic phosphorus compound BI and their reaction product D, is less than 5% by mass. The molar ratio of metal atoms originating from metal oxide A to phosphorus atoms originating from inorganic phosphorus compound BI in layer Y is 1.0:1.0 to 3.6:1.
0. The thickness of layer Y is 0.05–4.0 μm. The image sharpness of the multilayer structure is above 90% when the comb width is 0.25 mm, as measured according to ISO 17221:2014.
2. The multi-layer structure according to claim 1, wherein, The haze value measured according to JIS K7105:1981 is less than 3%.
3. The multi-layer structure according to claim 1 or 2, wherein, A water vapour transmission rate of 1 x 10-6g / m2day at 40°C, 90% RH, measured according to ISO 15106-5:2015. -2 g / m 2 ·day.
4. The multi-layer structure according to claim 1 or 2, wherein, The image sharpness of substrate X is above 90% when the comb width is 0.25 mm, as measured according to ISO 17221:2014.
5. The multi-layer structure according to claim 1 or 2, wherein, Substrate X has a surface layer.
6. The multilayer structure according to claim 1 or 2, wherein a substrate X and a layer Y are directly stacked.
7. The multilayer structure according to claim 1 or 2, wherein a substrate X and a layer Y are laminated together via an adhesive layer I.
8. The multilayer structure according to claim 1 or 2, wherein it comprises layers Y disposed on both sides of the substrate X.
9. A method for manufacturing a multilayer structure according to any one of claims 1 to 8, comprising the following steps: Step (I) involves coating at least one side of a substrate X with a coating solution S comprising a metal oxide A containing aluminum atoms, an inorganic phosphorus compound BI, and a solvent, and then removing the solvent to form a precursor layer for layer Y; and Process (II) involves heat-treating the precursor layer of layer Y to form layer Y. In process (I), the coating speed of the coating liquid S is 0.03 cm / s or more and 2.5 cm / s or less relative to the coating width of 1 cm. The heat treatment temperature in process (II) is above 140℃, and the heat treatment time is from 1 second to 1 hour. The image sharpness of the multilayer structure obtained when the comb width is 0.25 mm as measured according to ISO 17221:2014 is over 90%.
10. A protective sheet for an electronic device, comprising a multilayer structure as described in any one of claims 1 to 8.
11. The protective sheet according to claim 10, wherein it is a protective sheet for protecting the surface of a photoelectric conversion device, an information display device, or a lighting device.
12. An electronic device having the protective sheet as described in claim 10 or 11.
Citation Information
Patent Citations
Electronic device and method for manufacturing the same
WO2016103720A1
Multilayer structure, device using same, and manufacturing method therefor
CN104349895A