A method for preparing a high-density ITO planar target
By combining modified nano-titanium dioxide and nano-silica, the sintering process was optimized, solving the problem of low strength caused by large ITO target grains. This enabled the preparation of high-density ITO targets, improving their density and strength.
Patent Information
- Application Number
- CN202410197849.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-22
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-02-22
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This application relates to the technical field of target preparation, and in particular to a method for preparing a high-density ITO planar target. Background Technology
[0002] Indium tin oxide (ITO) sputtering targets are transparent conductive materials mainly composed of indium oxide and tin oxide. Due to their high light transmittance, high conductivity, and strong ultraviolet light absorption, ITO sputtering targets are widely used in various electronic devices such as touch screens, liquid crystal displays, solar cells, and military applications.
[0003] The production of ITO targets mainly includes three steps: powder preparation, molding, and sintering. Typically, nano-sized ITO powder is used in conjunction with cold isostatic pressing and atmospheric pressure sintering to prepare high-density ITO targets. However, during the atmospheric pressure sintering process of ITO targets, high sintering temperatures and long holding times are often required to complete the densification process. This can easily lead to larger ITO target grains, resulting in lower ITO target strength and thus limiting the application of ITO targets. Summary of the Invention
[0004] To address the issue of low strength caused by large ITO target grains, this application provides a method for preparing a high-density ITO planar target.
[0005] This application provides a method for preparing a high-density ITO planar target, which adopts the following technical solution: A method for preparing a high-density ITO planar target includes the following steps: (1) Indium oxide, tin oxide, modified nano titanium dioxide and anhydrous ethanol are mixed evenly, then ball milled for 24 hours, dried, passed through a 40-mesh sieve, and then Y2O3 and modified nano silicon dioxide are added and sintered once to obtain a mixture; (2) The mixture obtained in step (1) is hot-pressed at a pressure of 60-70 MPa for 2-3 hours, and then sintered twice to obtain an ITO planar target. The temperature of the second sintering is 1800-2000℃, the sintering time is 8-10 hours, and the heating rate is 1.2-1.5℃ / min.
[0006] By adopting the above technical solution, indium oxide, tin oxide, modified nano-titanium dioxide, and anhydrous ethanol are first mixed and ball-milled to obtain a mixture with uniformly dispersed particles. Indium oxide, as the main component of ITO target material, has good electrical conductivity and transparency. Tin oxide can enhance the conductivity of ITO target material, which helps to improve its chemical stability and wear resistance. Modified nano-titanium dioxide has excellent chemical stability and good dispersibility. The addition of modified nano-titanium dioxide makes the indium oxide, tin oxide, and modified nano-titanium dioxide mixed uniformly. The modified nano-titanium dioxide can be distributed in the gaps between indium oxide and tin oxide, increasing the density of the system. After mixing indium oxide, tin oxide, modified nano-titanium dioxide, and anhydrous ethanol, the particles are further refined by ball milling, resulting in a more uniform particle size distribution and higher density, which is beneficial to subsequent sintering.
[0007] Y2O3 and modified nano-silica are then added and sintered once to obtain a mixture. Y2O3, as a sintering aid, can generate a liquid phase in the ITO sintered body and dissolve into the crystal to promote sintering, and also increase the density and toughness of the ITO sintered body. Modified nano-silica can fill the gaps in the system, reduce porosity, and make the ITO sintered body more compact. Moreover, mullite crystal phase is generated during the sintering process and dispersed into the ITO sintered body, thus making the ITO sintered body perform better. Mixing Y2O3 with modified nano-silica can reduce the probability of impurity diffusion. The added nano-silica makes the particle surface of the ITO sintered body smoother, increases the packing density of the ITO sintered body, and helps to improve the thermal stability of the ITO sintered body. In addition, mixing indium oxide and tin oxide and sintering them once allows them to react chemically and allow tin to be doped into the lattice of indium oxide to form indium tin oxide compound. Modified nano-titanium dioxide can be doped into the gap between indium oxide and tin oxide, effectively reducing the exhaust gas during hot pressing and improving the hot pressing effect.
[0008] During the sintering process, modified nano-titanium dioxide transforms into rutile titanium dioxide. Rutile titanium dioxide has superior thermal stability, better density, and higher hardness and density. The combination of various components improves the density of the ITO planar target material, thereby obtaining an ITO planar target material with better strength.
[0009] The resulting mixture is then hot-pressed and sintered a second time to further improve the density of the ITO planar target. By combining various raw material components and adjusting the sintering temperature and time twice, the prepared ITO target has good density, which prevents the ITO target grains from becoming too large during sintering and ensures the strength of the ITO target. In addition, the pores of the ITO planar target are filled by modified nano-titanium dioxide and modified nano-silica, making the ITO planar target more dense and ensuring that the ITO planar target is stable, flat and does not warp during sintering.
[0010] Preferably, in step (1), the mass ratio of indium oxide, tin oxide, modified nano titanium dioxide and anhydrous ethanol is 10-20:1:0.5-0.8:30-40.
[0011] By adopting the above technical solution, the mass ratio of indium oxide, tin oxide, modified nano titanium dioxide, and anhydrous ethanol is further limited within a certain range, which improves the grinding and dispersibility of the system and helps the system to sinter. The modified nano titanium dioxide can be distributed in the gap between indium oxide and tin oxide, increasing the density of the system. Subsequent mixing with other components and processing steps make the ITO planar target more dense and ensure that the ITO planar target is stable, flat, and does not warp during sintering.
[0012] Preferably, in step (1), the mass ratio of Y2O3 to modified nano-silica is 1.5-2.5:1.
[0013] By adopting the above technical solution, the mass ratio of Y2O3 and modified nano-silica is further limited to a certain range. Modified nano-silica can fill the gaps in the system, reduce pores, and make the ITO sintered body more compact. Y2O3, as a sintering aid, can generate a liquid phase in the ITO sintered body and dissolve into the crystal to promote sintering. It also increases the density and toughness of the ITO sintered body. The mixture of Y2O3 and modified nano-silica, along with other components and processing steps, produces a more compact ITO planar target material. At the same time, it makes the ITO planar target material stable, flat and non-warping during sintering.
[0014] Preferably, the temperature of the first sintering is 1500-1600℃, the sintering time is 5-8h, and the heating rate is 0.5-0.9℃ / min.
[0015] By adopting the above technical solution, the sintering temperature, time, and heating rate are further limited, so that the ITO planar target material is sintered at a limited temperature, resulting in ITO planar target materials with higher density and better performance.
[0016] Preferably, the preparation method of the modified nano-titanium dioxide includes the following steps: dispersing nano-titanium dioxide in concentrated hydrochloric acid solution, stirring for 2-5 min, calcining at 300-310℃ for 1-2 h, then dispersing it in silane coupling agent solution, adding PVA, stirring for 2-3 h, and drying to obtain modified nano-titanium dioxide.
[0017] By adopting the above technical solution, nano-titanium dioxide is first treated with concentrated hydrochloric acid to remove organic impurities on the surface of nano-titanium dioxide, and then calcined at 300-310℃ to further increase the specific surface area of nano-titanium dioxide and increase the pore structure on the surface of nano-titanium dioxide, which is conducive to subsequent mixing with other components.
[0018] The silane coupling agent decomposes in water, undergoing a dehydration condensation reaction to generate oligomers. These oligomers form hydrogen bonds with the hydroxyl groups on the surface of nano-titanium dioxide. During the heating and drying process, they undergo dehydration to form covalent bonds, allowing the silane coupling agent to cover the surface of the nano-titanium dioxide, thereby ensuring uniform dispersion of the nano-titanium dioxide.
[0019] PVA has a certain viscosity and contains abundant hydroxyl groups. The silane molecules in the silane coupling agent react with the hydroxyl groups in PVA through silicon-oxygen bonds to form silicon-oxygen-carbon bonds, thereby improving the mechanical strength and dispersibility of nano-titanium dioxide. Subsequently, it is applied to ITO planar targets to improve the sinterability, density and mechanical strength of ITO sintered bodies.
[0020] Preferably, the mass ratio of the nano-titanium dioxide, silane coupling agent solution and PVA is 1:20-30:0.6-0.9.
[0021] By adopting the above technical solution, the mass ratio of nano-titanium dioxide, silane coupling agent solution, and PVA is further limited within a certain range, resulting in modified nano-titanium dioxide with superior mechanical properties and high dispersibility. There is a synergistic effect among nano-titanium dioxide, silane coupling agent solution, and PVA. The silane coupling agent can cover the surface of nano-titanium dioxide, making the nano-titanium dioxide uniformly dispersed. The hydroxyl groups in PVA react with the silane molecules in the silane coupling agent to form silicon-oxygen-carbon bonds, which improves the mechanical strength and dispersibility of nano-titanium dioxide. In subsequent ITO planar target materials, this improves the sinterability, density, and mechanical strength of the ITO sintered body.
[0022] Preferably, PVA is added and the stirring temperature is 60-65℃.
[0023] By adopting the above technical solution, the stirring temperature of PVA is further limited, which allows PVA to be dispersed more quickly and evenly in the system. This ensures that the silane coupling agent, nano-titanium dioxide, and PVA are fully mixed, thereby giving the modified nano-titanium dioxide system better comprehensive performance. When applied to ITO planar targets, it improves the sinterability, density, and mechanical strength of the ITO sintered body.
[0024] Preferably, the method for preparing the modified nano-silica includes the following steps: calcining nano-silica at a temperature of 350-360℃ for 2-3 hours, then dispersing it in deionized water, adding nano-nickel and ammonium polyacrylate, stirring for 1-2 hours, and drying to obtain modified nano-silica.
[0025] By adopting the above technical solution, nano-silica is first calcined at 350-360℃ to remove organic impurities on the surface of nano-silica, thereby increasing the specific surface area and pore size of nano-silica. Nano-nickel has high hardness and corrosion resistance, as well as excellent thermal and electrical conductivity. Nano-nickel is loaded onto the surface and pore structure of nano-silica, increasing its specific surface area and hardness. When subsequently applied to ITO targets, it increases the density of the ITO targets and helps improve their thermal and electrical conductivity. Ammonium polyacrylate has a certain viscosity, which enables a tighter connection between nano-nickel and nano-silica, allowing nano-nickel to be firmly loaded onto the surface of nano-silica, thus improving the stability of the performance improvement of nano-silica and facilitating its subsequent applications.
[0026] Preferably, the mass ratio of the nano-silica, nano-nickel, and ammonium polyacrylate is 1:0.3-0.5:0.7-0.9.
[0027] By adopting the above technical solution, the mass ratio of nano-silica, nano-nickel, and ammonium polyacrylate is further limited within a certain range, resulting in modified nano-silica with high mechanical properties and hardness. Nano-nickel is loaded on the surface of nano-silica, and ammonium polyacrylate increases the adhesion between nano-silica and nano-nickel, so that nano-nickel is firmly loaded on the surface of nano-silica, thereby improving the hardness of nano-silica. When subsequently applied to ITO sputtering targets, it improves the density of ITO sputtering targets, as well as the thermal and electrical conductivity of ITO sputtering targets, thus improving the overall performance of ITO sputtering targets.
[0028] Preferably, the stirring temperature is 75-80℃.
[0029] By adopting the above technical solution, the stirring temperature is further limited, which makes the nano-silica, nano-nickel and ammonium polyacrylate mixed evenly. At the same time, the particle fluidity is improved, so that the nano-nickel is evenly dispersed on the surface of the nano-silica. The viscosity of the ammonium polyacrylate is also improved, which makes the system mixed evenly and helps to improve the overall performance of the system.
[0030] In summary, this application has the following beneficial effects: 1. In this application, indium oxide, tin oxide, modified nano-titanium dioxide, and anhydrous ethanol are mixed and ball-milled to obtain a mixture with uniformly dispersed particles. Indium oxide has good electrical conductivity and transparency, while tin oxide can enhance the conductivity of the ITO target material, which helps to improve its chemical stability and wear resistance. The addition of modified nano-titanium dioxide ensures that the indium oxide, tin oxide, and modified nano-titanium dioxide are mixed uniformly. The modified nano-titanium dioxide can be distributed in the gaps between indium oxide and tin oxide, increasing the density of the system. After mixing indium oxide, tin oxide, modified nano-titanium dioxide, and anhydrous ethanol, the particles are further refined by ball milling, resulting in a more uniform particle size distribution and higher density, which is beneficial for subsequent sintering.
[0031] 2. In this application, Y2O3 and modified nano-silica are added and sintered in one step to obtain a mixture. Y2O3, as a sintering aid, can generate a liquid phase in the ITO sintered body and dissolve into the crystal to promote sintering, and also increase the density and toughness of the ITO sintered body. Modified nano-silica can fill the gaps in the system, reduce pores, make the ITO sintered body more compact, and generate a mullite crystal phase during the sintering process, which is dispersed into the ITO sintered body, thus making the ITO sintered body perform better.
[0032] 3. In this application, the mixing of Y2O3 and modified nano-silica can reduce the probability of impurity diffusion. The added nano-silica can make the particle surface of the ITO sintered body smoother, increase the packing density of the ITO sintered body, and help improve the thermal stability of the ITO sintered body. In addition, the mixing of indium oxide and tin oxide and the one-time sintering cause a chemical reaction between the two and allow tin to be doped into the lattice of indium oxide to form indium tin oxide compound. Modified nano-titanium dioxide can be doped into the gap between indium oxide and tin oxide, effectively reducing the exhaust gas during hot pressing and improving the hot pressing effect. Detailed Implementation
[0033] The present application will be further described in detail below with reference to the embodiments.
[0034] The raw materials used in the examples and comparative examples are all commercially available.
[0035] Preparation Example 1-1 The preparation method of modified nano-titanium dioxide includes the following steps: 0.5 kg of nano-titanium dioxide is dispersed in 1 L of 40% concentrated hydrochloric acid solution, stirred for 4 min, calcined at 310℃ for 2 h, then dispersed in 1.5 L of 2% silane coupling agent solution, PVA is added, stirred for 3 h at 65℃, and dried to obtain modified nano-titanium dioxide.
[0036] The mass ratio of nano-titanium dioxide, silane coupling agent solution and PVA is 1:20:0.9.
[0037] Preparation Examples 1-2 The difference from Preparation Example 1-1 is that no silane coupling agent solution is added.
[0038] Preparation Examples 1-3 The difference from preparation example 1-1 is that PVA is not added.
[0039] Preparation Examples 1-4 The difference from Preparation Example 1-1 is that the mass ratio of nano-titanium dioxide, silane coupling agent solution and PVA is 1:30:0.6.
[0040] Preparation Examples 1-5 The difference from Preparation Example 1-1 is that the mass ratio of nano-titanium dioxide, silane coupling agent solution and PVA is 1:40:0.1.
[0041] Preparation Example 2-1 The preparation method of modified nano silica includes the following steps: 0.8 kg of nano silica is calcined at 360℃ for 3 h, then dispersed in 1.3 L of deionized water, nano nickel and ammonium polyacrylate are added, stirred for 2 h at a stirring temperature of 80℃, and dried to obtain modified nano silica.
[0042] The mass ratio of nano-silica, nano-nickel, and ammonium polyacrylate is 1:0.3:0.7.
[0043] Preparation Example 2-2 The difference from preparation example 2-1 is that no nano-nickel is added.
[0044] Preparation Examples 2-3 The difference from Preparation Example 2-1 is that ammonium polyacrylate is not added.
[0045] Preparation Examples 2-4 The difference from Preparation Example 2-1 is that the mass ratio of nano-silica, nano-nickel, and ammonium polyacrylate is 1:0.5:0.9.
[0046] Preparation Examples 2-5 The difference from Preparation Example 2-1 is that the mass ratio of nano-silica, nano-nickel, and ammonium polyacrylate is 1:0.8:0.4.
[0047] Example 1 A method for preparing a high-density ITO planar target includes the following steps: (1) Mix indium oxide, 1 kg tin oxide, modified nano titanium dioxide and anhydrous ethanol evenly, then ball mill for 24 h, dry, pass through a 40 mesh sieve, then add Y2O3 and 0.6 kg modified nano silicon dioxide, and sinter once to obtain a mixture; (2) The mixture obtained in step (1) is hot-pressed at a pressure of 60 MPa for 3 hours and then sintered twice to obtain an ITO planar target. The temperature of the second sintering is 1800℃, the sintering time is 10 hours, and the heating rate is 1.2℃ / min.
[0048] In step (1), the mass ratio of indium oxide, tin oxide, modified nano titanium dioxide and anhydrous ethanol is 10:1:0.8:30.
[0049] In step (1), the mass ratio of Y2O3 to modified nano-silica is 1.5:1.
[0050] The sintering temperature was 1500℃, the sintering time was 5h, and the heating rate was 0.5℃ / min.
[0051] Modified nano-titanium dioxide was prepared using a 1-1 method, and modified nano-silica was prepared using a 2-1 method.
[0052] Example 2 A method for preparing a high-density ITO planar target material, which differs from Example 1 in that it includes the following steps: (1) Mix indium oxide, 1 kg tin oxide, modified nano titanium dioxide and anhydrous ethanol evenly, then ball mill for 24 h, dry, pass through a 40 mesh sieve, then add Y2O3 and 0.6 kg modified nano silicon dioxide, and sinter once to obtain a mixture; (2) The mixture obtained in step (1) is hot-pressed at 70 MPa for 2 hours and then sintered twice to obtain an ITO planar target. The temperature of the second sintering is 2000℃, the sintering time is 8 hours, and the heating rate is 1.5℃ / min.
[0053] In step (1), the mass ratio of indium oxide, tin oxide, modified nano titanium dioxide and anhydrous ethanol is 20:1:0.5:40.
[0054] In step (1), the mass ratio of Y2O3 to modified nano-silica is 2.5:1.
[0055] The sintering temperature was 1600℃, the sintering time was 8h, and the heating rate was 0.9℃ / min.
[0056] Example 3 A method for preparing a high-density ITO planar target differs from Example 1 in that, in step (1), the mass ratio of indium oxide, tin oxide, modified nano-titanium dioxide, and anhydrous ethanol is 25:1:0.1:25.
[0057] Example 4 A method for preparing a high-density ITO planar target material differs from Example 1 in that, in step (1), the mass ratio of Y2O3 to modified nano-silica is 3.5:1.
[0058] Example 5 A method for preparing a high-density ITO planar target material, which differs from Example 1 in that the modified nano-titanium dioxide is prepared using step 1-2.
[0059] Example 6 A method for preparing a high-density ITO planar target material, which differs from Example 1 in that the modified nano-titanium dioxide is prepared using steps 1-3.
[0060] Example 7 A method for preparing a high-density ITO planar target material, which differs from Example 1 in that the modified nano-titanium dioxide is prepared using steps 1-4.
[0061] Example 8 A method for preparing a high-density ITO planar target material, which differs from Example 1 in that the modified nano-titanium dioxide is prepared using step 1-5.
[0062] Example 9 A method for preparing a high-density ITO planar target material differs from Example 1 in that the modified nano-silica is prepared using a 2-2 method.
[0063] Example 10 A method for preparing a high-density ITO planar target material, which differs from Example 1 in that the modified nano-silica is prepared using step 2-3.
[0064] Example 11 A method for preparing a high-density ITO planar target material differs from Example 1 in that the modified nano-silica is prepared using step 2-4.
[0065] Example 12 A method for preparing a high-density ITO planar target material differs from Example 1 in that the modified nano-silica is prepared using 2-5.
[0066] Comparative Example 1 A method for preparing a high-density ITO planar target material differs from Example 1 in that modified nano-titanium dioxide is not added.
[0067] Comparative Example 2 A method for preparing a high-density ITO planar target material differs from Example 1 in that the modified nano-titanium dioxide is replaced by an equal amount of nano-titanium dioxide.
[0068] Comparative Example 3 A method for preparing a high-density ITO planar target material differs from Example 1 in that modified nano-silica is not added.
[0069] Comparative Example 4 A method for preparing a high-density ITO planar target material differs from Example 1 in that the modified nano-silica is replaced by an equal amount of nano-silica.
[0070] The density, warpage, and thickness of the ITO planar targets prepared in Examples 1-12 and Comparative Examples 1-4 were tested. The density test method is based on Archimedes' principle and uses the water displacement method to measure the actual density of the product. According to ρ (实际密度) = (m1 / m2)×ρ 液 The actual density of the product is obtained, where m1 is the mass of the sample in air, m2 is the mass of the sample in distilled water, and ρ is the density of the sample. 液 The density of distilled water; Theoretical density ρ of the test sample (理论密度) =m1 / V; Packing density n = ρ (实际密度) / ρ (理论密度) ×100%.
[0071] The warpage was tested by direct measurement with a feeler gauge; the test results are shown in Table 1.
[0072] Table 1 Test data for the examples and comparative examples
[0073] As can be seen from Table 1, the ITO planar targets prepared in Examples 1-2, 7, and 11 of this application have good hardness, density, and flatness without warping. Among them, the density of Example 1 is 99.96%, the warping is 0.07 mm, and the thickness is 12.78 mm, indicating that the ITO planar targets prepared in this application have high density. The combination of multiple components improves the density and hardness of the ITO planar targets. By filling the pores of the ITO planar targets with modified nano-titanium dioxide and modified nano-silica, the ITO planar targets are made more dense, and at the same time, the ITO planar targets are stable, flat, and do not warp during sintering.
[0074] Example 3 changed the mass ratio of indium oxide, tin oxide, modified nano titanium dioxide and anhydrous ethanol. As shown in Table 1, compared with Example 1, the density, warpage and thickness test performance of the ITO planar target material were worse. This indicates that the combination of indium oxide, tin oxide, modified nano titanium dioxide and anhydrous ethanol increased the density of the system, making the ITO planar target material more compact, and at the same time making the ITO planar target material stable and flat without warping during sintering.
[0075] Example 4 changed the mass ratio of Y2O3 and modified nano-silica. As shown in Table 1, compared with Example 1, the density, warpage and thickness test performance of the ITO planar target material were worse. This indicates that the ITO planar target material prepared by mixing Y2O3 and modified nano-silica, as well as other components and processing steps, is more dense, and at the same time makes the ITO planar target material stable, flat and not warped during sintering.
[0076] In Example 5, the modified nano-titanium dioxide preparation method did not include a silane coupling agent solution. As shown in Table 1, compared to Example 1, the density was 99.64%, the warpage was 0.15 mm, and the thickness was 12.89 mm. This indicates that the silane coupling agent forms hydrogen bonds with the hydroxyl groups on the surface of the nano-titanium dioxide, and dehydrates during the heating and drying process to form covalent bonds. This allows the silane coupling agent to cover the surface of the nano-titanium dioxide, thereby making the nano-titanium dioxide uniformly dispersed and effectively improving the corresponding properties of the nano-titanium dioxide.
[0077] In Example 6, the modified nano-titanium dioxide was prepared without PVA. As shown in Table 1, compared with Example 1, the density was 99.65%, the warpage was 0.14 mm, and the thickness was 12.88 mm. This indicates that PVA has a certain viscosity and contains abundant hydroxyl groups. The silane molecules in the silane coupling agent react with the hydroxyl groups in PVA through silicon-oxygen bonds to form silicon-oxygen-carbon bonds, thereby improving the mechanical strength and dispersibility of nano-titanium dioxide. Subsequently, when applied to ITO planar targets, it improves the sinterability, density, and mechanical strength of the ITO sintered body.
[0078] Example 8 changed the mass ratio of nano-titanium dioxide, silane coupling agent solution, and PVA. As shown in Table 1, compared with Example 1, the density, warpage, and thickness test performance of the ITO planar target were worse than those of Examples 1-2, but better than those of Examples 5-6. This indicates that there is a synergistic effect between nano-titanium dioxide, silane coupling agent solution, and PVA. The silane coupling agent can cover the surface of nano-titanium dioxide, making the nano-titanium dioxide uniformly dispersed. The hydroxyl groups in PVA react with the silane molecules in the silane coupling agent to form silicon-oxygen-carbon bonds, which improves the mechanical strength and dispersibility of nano-titanium dioxide. In the subsequent ITO planar target, it improves the sinterability, density, and mechanical strength of the ITO sintered body.
[0079] In Example 9, the modified nano-silica was prepared without the addition of nano-nickel. As shown in Table 1, compared with Example 1, the density was 99.51%, the warpage was 0.19 mm, and the thickness was 12.95 mm. This indicates that nano-nickel has high hardness and corrosion resistance, as well as excellent thermal and electrical conductivity. The nano-nickel loaded on the surface and pore structure of nano-silica increases the specific surface area and hardness of nano-silica. When applied to ITO targets, it increases the density of the ITO targets.
[0080] In Example 10, the preparation method of modified nano-silica did not include ammonium polyacrylate. As shown in Table 1, compared with Example 1, the density was 99.54%, the warpage was 0.17 mm, and the thickness was 12.93 mm. This indicates that ammonium polyacrylate has a certain viscosity, which enables the nano-nickel and nano-silica to be more tightly connected, allowing the nano-nickel to be firmly loaded on the surface of the nano-silica. This improves the stability of the performance improvement of nano-silica and is conducive to the subsequent application of modified nano-silica.
[0081] Example 12 changed the mass ratio of nano-silica, nano-nickel, and ammonium polyacrylate. As shown in Table 1, compared with Example 1, the density, warpage, and thickness test performance of the ITO planar target were worse than those of Examples 1-2, but better than those of Examples 9-10. This indicates that the nano-nickel was loaded on the surface of the nano-silica, and the ammonium polyacrylate increased the adhesion between the nano-silica and the nano-nickel, so that the nano-nickel was firmly loaded on the surface of the nano-silica, thereby improving the hardness of the nano-silica. When applied to the ITO target, it improved the density of the ITO target.
[0082] Comparative Example 1, without the addition of modified nano-titanium dioxide, shows in Table 1 that, compared to Example 1, the density is 97.20%, the warpage is 0.31 mm, and the thickness is 13.86 mm. This indicates that the addition of modified nano-titanium dioxide ensures that indium oxide, tin oxide, and modified nano-titanium dioxide are mixed uniformly. The modified nano-titanium dioxide can be distributed in the gaps between indium oxide and tin oxide, increasing the density of the system. After mixing indium oxide, tin oxide, modified nano-titanium dioxide, and anhydrous ethanol, the particles are further refined by ball milling, resulting in a more uniform particle size distribution and higher density, which is beneficial for subsequent sintering.
[0083] In Comparative Example 2, the modified nano-titanium dioxide was replaced by an equal amount of nano-titanium dioxide. As shown in Table 1, compared with Example 1, the density was 98.12%, the warpage was 0.27 mm, and the thickness was 13.82 mm. This indicates that the modified nano-titanium dioxide prepared in this application has better hardness, which can improve the hardness and density of the ITO planar target, thereby improving the warpage of the ITO planar target.
[0084] Comparative Example 3 did not contain modified nano-silica. As shown in Table 1, compared with Example 1, the density was 97.05%, the warpage was 0.35 mm, and the thickness was 13.91 mm. This indicates that the added nano-silica can make the particle surface of the ITO sintered body smoother, increase the packing density of the ITO sintered body, and help improve the thermal stability of the ITO sintered body.
[0085] In Comparative Example 4, the modified nano-silica was replaced by an equal amount of nano-silica. As shown in Table 1, compared with Example 1, the density was 98.02%, the warpage was 0.30 mm, and the thickness was 13.87 mm, indicating that the modified nano-silica of this application has better performance. The modified nano-titanium dioxide can be doped into the gap between indium oxide and tin oxide, effectively reducing the exhaust gas during hot pressing and improving the hot pressing effect. Moreover, the modified nano-titanium dioxide transforms into rutile titanium dioxide during sintering, which has better density and higher hardness and density. The various components work together to improve the density of the ITO planar target material.
[0086] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of the claims of this application.
Claims
1. A method for preparing a high-density ITO planar target, characterized in that, Includes the following steps: (1) Indium oxide, tin oxide, modified nano titanium dioxide and anhydrous ethanol are mixed evenly, then ball milled, dried and sieved, and then Y2O3 and modified nano silicon dioxide are added and sintered once to obtain a mixture; (2) The mixture obtained in step (1) is hot-pressed at a pressure of 60-70 MPa for 2-3 hours, and then sintered twice to obtain an ITO planar target. The temperature of the second sintering is 1800-2000℃, the sintering time is 8-10 hours, and the heating rate is 1.2-1.5℃ / min. The method for preparing the modified nano-titanium dioxide includes the following steps: dispersing nano-titanium dioxide in concentrated hydrochloric acid solution, stirring for 2-5 min, calcining at 300-310℃ for 1-2 h, then dispersing it in silane coupling agent solution, adding PVA, stirring for 2-3 h, and drying to obtain modified nano-titanium dioxide. The method for preparing the modified nano-silica includes the following steps: calcining nano-silica at 350-360℃ for 2-3 hours, then dispersing it in deionized water, adding nano-nickel and ammonium polyacrylate, stirring for 1-2 hours, and drying to obtain modified nano-silica.
2. The method for preparing a high-density ITO planar target according to claim 1, characterized in that, In step (1), the mass ratio of indium oxide, tin oxide, modified nano titanium dioxide and anhydrous ethanol is 10-20:1:0.5-0.8:30-40.
3. The method for preparing a high-density ITO planar target according to claim 1, characterized in that, In step (1), the mass ratio of Y2O3 to modified nano-silica is 1.5-2.5:
1.
4. The method for preparing a high-density ITO planar target according to claim 1, characterized in that, The temperature of the first sintering is 1500-1600℃, the sintering time is 5-8h, and the heating rate is 0.5-0.9℃ / min.
5. The method for preparing a high-density ITO planar target according to claim 1, characterized in that, The mass ratio of the nano-titanium dioxide, silane coupling agent solution, and PVA is 1:20-30:0.6-0.
9.
6. The method for preparing a high-density ITO planar target according to claim 1, characterized in that, Add PVA and stir at a temperature of 60-65℃.
7. The method for preparing a high-density ITO planar target according to claim 1, characterized in that, The mass ratio of the nano-silica, nano-nickel, and ammonium polyacrylate is 1:0.3-0.5:0.7-0.
9.
8. The method for preparing a high-density ITO planar target according to claim 1, characterized in that, The stirring temperature is 75-80℃.
Citation Information
Patent Citations
Preparation method for high-density indium tin oxide target material
CN102180653A
Preparation method of high-strength bacteria-inhibiting medical gauze
CN108126231A
ITO planar target material and preparation method thereof
CN114853467A
ITO target material with low tin oxide content and preparation method
CN117185780A