A high-strength aluminum alloy component forging heat treatment composite high-strength and toughness precision forming process

Through the forging heat treatment composite process of casting aluminum alloy bars, using die forging and water quenching technology, combined with aging treatment, the problems of low forming accuracy and poor strength and toughness in the existing aluminum alloy forging process are solved, and an efficient and energy-saving aluminum alloy is achieved Forging production reduces costs and energy consumption.

CN118048587BActive Publication Date: 2024-10-18WUHAN UNIV OF TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410152229.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-03
Publication Date
2024-10-18
Estimated Expiration
2044-02-03

AI Technical Summary

Technical Problem

The current high-strength aluminum alloy forging process has the problems of low forging precision, coarse grain structure, poor strength and toughness, low process efficiency, high energy consumption, and the cost of using cast aluminum alloy rods is high.

Method used

Cast aluminum alloy bars are used for forging heat treatment composite process, including heating, die forging, water quenching and aging treatment. The temperature difference is reduced through die forging and quenching, holding furnace filling and water quenching to avoid solid solution heat treatment and direct aging treatment to improve mechanical properties.

Benefits of technology

It significantly improves the forming accuracy and mechanical properties of aluminum alloy forgings, reduces hot forging temperature and energy consumption, avoids the generation of coarse-grained structures, reduces production costs, and extends the service life of forgings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118048587B_ABST
    Figure CN118048587B_ABST
Patent Text Reader

Abstract

The invention discloses a high-strength aluminum alloy component forging heat treatment composite high-strength and toughness precision forming process, including selecting a cast aluminum alloy bar, heating it to a first preset temperature, and keeping it warm for the first preset time; forging the cast aluminum alloy bar after being kept warm on a mold at a second preset temperature to obtain an aluminum alloy forging of a specific product shape; placing the aluminum alloy forging into a holding furnace at a temperature of a third preset temperature; water quenching the aluminum alloy forging after being kept warm; and performing aging treatment on the aluminum alloy forging after being water quenched. The beneficial effects of the invention are: the cast bar is strengthened by a composite process, and no solution heat treatment is required after the subsequent final forging, and only aging treatment is required, which not only significantly reduces the hot forging temperature and energy consumption, but also significantly improves the mechanical properties through deformation strengthening and phase transformation strengthening, and effectively prevents the current forging from producing coarse-grained structure, reduces the residual stress generated during the forging process, and improves the strength, toughness and service life of the forging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aluminum alloy forming, and in particular to a high-strength aluminum alloy component forging heat treatment composite high-strength and toughness precision forming process. Background Art

[0002] With the rapid development of my country's aviation, aerospace, navigation, automobile and high-speed rail transportation equipment, the demand for high performance and lightweight equipment is increasing. Aluminum alloy has high specific strength and low density, and is an ideal material for lightweight transportation equipment. The current high-strength aluminum alloy forging process mainly includes the following steps (such as Figure 1 ): First heat to 400℃, then place the heated aluminum billet into a hot mold (>200℃), forge, and then perform subsequent solution heat treatment (>470℃, >1h), quenching and artificial aging (>120℃, >24h) on the forgings to obtain T6 state parts. The current aluminum alloy forging process requires solution quenching after forging, and the forgings are prone to deformation, which affects the forming accuracy of the forgings. At the same time, the forgings produce coarse grains, which reduces the strength and toughness and service life of the parts; and the process efficiency is low and the energy consumption is high. Extruded aluminum bars are aluminum alloy materials commonly used in the forging industry. From the perspective of raw material costs, the cost of cast aluminum bars is relatively low, and they are generally obtained by melting recycled aluminum and aluminum alloy waste; while extruded bars require continuous extrusion of cast aluminum ingots; therefore, forging is cheaper if cast aluminum alloy bars are used. Summary of the invention

[0003] The present invention provides a high-strength aluminum alloy component forging heat treatment composite high-strength and toughness precision forming process, comprising:

[0004] S1. Select a cast aluminum alloy bar, heat it to a first preset temperature, and keep it warm for the first preset time;

[0005] S2, forging the cast aluminum alloy bar after insulation on a die at a second preset temperature to obtain an aluminum alloy forging of a specific product shape, wherein the second preset temperature is lower than the first preset temperature, so as to utilize the lower temperature of the die to perform surface quenching and shaping on the cast aluminum alloy bar;

[0006] S3, placing the aluminum alloy forging into a holding furnace at a third preset temperature, and holding the furnace for a second preset time, so that the temperature of the surface layer of the aluminum alloy forging is consistent with the temperature of the core;

[0007] S4, water quenching the aluminum alloy forging after heat preservation;

[0008] S5. Performing aging treatment on the aluminum alloy forging after water quenching. The temperature of the aging treatment is a fourth preset temperature. The time of the aging treatment is a third preset time. After the aging treatment, an aluminum alloy forging product that meets specific technical requirements can be obtained.

[0009] In some embodiments, in step S1, the composition of the cast aluminum alloy bar is also required to be tested, and the aluminum alloy type of the cast aluminum alloy bar is determined based on the composition test result, and the size of the first preset temperature is determined based on the aluminum alloy type.

[0010] In some embodiments, for 7 series cast aluminum alloy bar, the first preset temperature is 340℃~390℃; for 6 series cast aluminum alloy bar, the first preset temperature is 400℃~450℃; for 2 series cast aluminum alloy bar, the first preset temperature is 376℃~407℃.

[0011] In some embodiments, in step S1 , the first preset time is determined according to the diameter of the cast aluminum alloy bar. The larger the diameter of the cast aluminum alloy bar, the longer the first preset time.

[0012] In some embodiments, the relationship between the first preset time and the diameter of the cast aluminum alloy bar is:

[0013] T1=K1*D

[0014] Wherein, T1 is the first preset time, K1 is the conversion coefficient, and the conversion coefficient K1 is determined by the type of aluminum alloy of the cast aluminum alloy bar; and D is the diameter of the billet.

[0015] In some embodiments, in step S2, the product shape includes a disk shape and a rod shape.

[0016] In some embodiments, in step S2, the second preset temperature is 100°C-200°C.

[0017] In some embodiments, in step S3, the third preset temperature is 350°C-500°C.

[0018] In some embodiments, in step S3, the second preset time is:

[0019] T2=K2*D

[0020] Wherein, T2 is the first preset time, K2 is the conversion coefficient, and the conversion coefficient K2 is determined by the type of aluminum alloy of the cast aluminum alloy bar; D is the diameter of the billet

[0021] In some embodiments, in step S5, the forging is subjected to aging treatment, and the fourth preset temperature and the third preset time are determined according to the composition of the cast aluminum alloy bar and the third preset temperature.

[0022] Compared with the prior art, the technical solution proposed by the present invention has the following beneficial effects: using cast bars, the raw material price is low, and the cast bars are strengthened by a composite process. After the subsequent final forging, no solution heat treatment is required, and only aging treatment is required, which not only significantly reduces the hot forging temperature and energy consumption, but also significantly improves the mechanical properties by deformation strengthening and phase transformation strengthening, and effectively prevents the current forging from producing coarse grain structure; this process combines forging heating and heat treatment solid solution to obtain a solid solution state blank, and the solid solution state blank is formed into a complex component by die forging, and the geometric accuracy of the component is guaranteed by segmented quenching in the die, and at the same time, the deformation fine grain structure is obtained by hot forging, and the aging strengthening after the die is superimposed on the deformation fine grain strengthening to obtain a high-precision and high-strength component, which completely solves the problems of low precision, coarse grain structure, and poor strength and toughness in the current process of forging first and then heat treatment. The die forging quenching surface is finalized, and then it is kept in a heat preservation furnace, and then it is quenched in water for secondary quenching, so that the temperature difference during quenching can be reduced, the deformation of the forging is reduced, and the forming accuracy of the forging is improved. The combination of casting raw materials and forging technology greatly reduces production costs. The use of cast aluminum bars combined with heat treatment technology can improve the grain structure of aluminum alloys, reduce grain boundary defects and microstructure inhomogeneity, reduce residual stress generated during forging, and improve forging toughness and service life. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a comparison between the current aluminum alloy forging process flow chart and this process flow chart;

[0024] Figure 2 It is a schematic diagram of the process flow of the high-strength aluminum alloy component forging heat treatment composite high-strength and toughness precision forming process provided by the present invention;

[0025] Figure 3 It is the microstructure diagram of the material obtained by this process;

[0026] Figure 4 This is the heat treatment process curve of this process. DETAILED DESCRIPTION

[0027] The preferred embodiments of the present invention are described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of this application and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not used to limit the scope of the present invention.

[0028] Please refer to Figure 1 and Figure 2 The present invention provides a high-strength aluminum alloy component forging heat treatment composite high-strength and toughness precision forming process, comprising:

[0029] S1. Select a cast aluminum alloy bar, heat it to a first preset temperature, and keep it warm for the first preset time;

[0030] In step S1, the purpose of heating and heat preservation is to soften the material and make it more conducive to deformation. During the heating and heat preservation process, the temperature of the material increases, which is conducive to the growth and recrystallization of grains, increases the grain boundary migration rate, and increases the grain size, thereby improving the plasticity and toughness of the material. In addition, high temperature is conducive to dissolving and removing impurities, oxides and other undesirable phases at the grain boundaries, which helps to improve the purity and uniformity of the material.

[0031] Furthermore, in step S1, it is also necessary to detect the composition of the cast aluminum alloy bar, determine the aluminum alloy type of the cast aluminum alloy bar according to the composition detection result, and determine the value of the first preset temperature according to the aluminum alloy type;

[0032] Specifically, for 7 series cast aluminum alloy bar stock, the first preset temperature is 340°C~390°C; for 6 series cast aluminum alloy bar stock, the first preset temperature is 400°C~450°C; for 2 series cast aluminum alloy bar stock, the first preset temperature is 376°C~407°C.

[0033] Further, in step S1, the first preset time is determined according to the diameter of the cast aluminum alloy bar, and the larger the diameter of the cast aluminum alloy bar, the longer the first preset time;

[0034] Specifically, the relationship between the first preset time and the diameter of the cast aluminum alloy bar is:

[0035] T1=K1*D(1)

[0036] Wherein, T1 is the first preset time, K1 is the conversion coefficient, and the conversion coefficient K1 is determined by the type of aluminum alloy of the cast aluminum alloy bar; and D is the diameter of the billet.

[0037] S2, forging the cast aluminum alloy bar after insulation on a die at a second preset temperature to obtain an aluminum alloy forging of a specific product shape, wherein the second preset temperature is lower than the first preset temperature, so as to utilize the lower temperature of the die to perform surface quenching and shaping on the cast aluminum alloy bar;

[0038] In step S2, cold die quenching can be used to quickly cool the surface of the aluminum alloy forging, so that the grains of the surface are refined and fixed at a certain size, thereby adjusting and controlling the organizational structure of the material; the rapid cooling during the cold die quenching process can form a strengthening phase or a high-hardness organizational structure, thereby improving the hardness and strength of the material; cold die quenching can improve the toughness and plasticity of the aluminum alloy forging by forming fine grains and a uniform organizational structure. In step S2, the surface of the bar in contact with the die is quenched to retain its surface organizational structure and produce a small amount of strengthening phase to prepare for the subsequent insulation step.

[0039] Further, in step S2, the product shape includes but is not limited to a disc shape and a rod shape;

[0040] Further, in step S2, the second preset temperature is 100°C to 200°C;

[0041] S3, placing the aluminum alloy forging into a holding furnace at a third preset temperature, and holding the furnace for a second preset time, so that the temperature of the surface layer of the aluminum alloy forging is consistent with the temperature of the core;

[0042] In step S3, the purpose of holding the forging for a relatively short time is to replenish the temperature of the surface of the aluminum alloy forging so that the temperature of the surface of the aluminum alloy forging is kept consistent with that of the core of the aluminum alloy forging by heating, thereby keeping the microstructure of the surface and the core of the aluminum alloy forging consistent to prevent the microstructure of the surface and the core from being inconsistent during subsequent quenching.

[0043] Preferably, the second preset time needs to match the cold die quenching time, that is, the longer the cold die quenching time, the longer the second preset time. Usually, the second preset time is:

[0044] T2=K2*D(2)

[0045] Wherein, T2 is the second preset time, K2 is the conversion coefficient, and the conversion coefficient K2 is determined by the type of aluminum alloy of the cast aluminum alloy bar; D is the diameter of the billet;

[0046] Further, in step S3, the third preset temperature is 350°C to 500°C;

[0047] S4, water quenching the aluminum alloy forging after heat preservation;

[0048] In step S4, the purpose of water quenching is to quench the entire aluminum alloy forging, so that a large amount of strengthening phase is generated in the aluminum alloy forging, and the organizational structure of the entire aluminum alloy forging is retained;

[0049] Further, in step S4, the water quenching time is determined according to the industry standard "YS∕T 591-2017 Heat Treatment of Deformed Aluminum and Aluminum Alloys", preferably, the water quenching time is 15-20s;

[0050] Preferably, the transfer time (the time for the forging to be transferred from the holding furnace to the water quenching pool) and the second preset temperature need to be matched, that is, the higher the second preset temperature, the longer the water quenching transfer time can be.

[0051] It should be pointed out that in the present invention, the surface is shaped by die forging and quenching, and then placed in a holding furnace for insulation, followed by secondary quenching in water, thereby reducing the temperature difference during quenching, reducing the deformation of the forging, and thus improving the forming accuracy of the forging.

[0052] S5, performing aging treatment on the aluminum alloy forging after water quenching, wherein the temperature of the aging treatment is a fourth preset temperature, and the time of the aging treatment is a third preset time, and after the aging treatment, an aluminum alloy forging product that meets specific technical requirements can be obtained;

[0053] In step S5, the purpose of aging treatment is to improve the strength and hardness of the aluminum alloy by forming fine strengthening phases and precipitation phases or precipitation of solid solutions; aging treatment can increase grain boundaries and dislocation barriers, thereby improving the toughness and ductility of the material; since there is no subsequent solution treatment after forging deformation in this process, aging treatment is crucial to improving the strength of the forging.

[0054] Furthermore, in step S5, the forging is subjected to aging treatment, and the fourth preset temperature and the third preset time are determined according to the composition of the cast aluminum alloy bar, and can refer to the industry standard "YS∕T 591-2017 Heat Treatment of Deformed Aluminum and Aluminum Alloys".

[0055] The microstructural characteristics of the aluminum alloy forging product obtained after step S5 are as follows: Figure 3 As shown in the figure, during the whole process, the microstructure change process of aluminum alloy bar / forging is as follows Figure 4 shown.

[0056] In the present invention, casting bars are used, and the raw material price is low. The casting bars are strengthened by a composite process. After the subsequent final forging, no solution heat treatment is required, and only aging treatment is required. Not only the hot forging temperature and energy consumption are significantly reduced, but deformation strengthening and phase transformation strengthening significantly improve the mechanical properties, and the coarse grain structure is effectively prevented from being produced by the current forging. The process combines forging heating and heat treatment solid solution to obtain a solid solution state blank, and the solid solution state blank is formed into a complex component by die forging. The geometric accuracy of the component is guaranteed by segmented quenching in the die. At the same time, the deformation fine grain structure is obtained by hot forging. After the die is removed, aging strengthening is superimposed on deformation fine grain strengthening to obtain a high-precision and high-toughness component, which completely solves the problems of low precision, coarse grain structure, and poor toughness in the current process of forging first and then heat treatment. The die forging quenching surface is finalized, and then it is kept in a heat preservation furnace, and then it is quenched in water for secondary quenching, so that the temperature difference during quenching can be reduced, the deformation of the forging is reduced, and the forming accuracy of the forging is improved. By using cast aluminum rods combined with adjusting the heat treatment process, the grain structure of the aluminum alloy can be improved, the defects at the grain boundaries and the inhomogeneity of the microstructure can be reduced, the residual stress generated during the forging process can be reduced, and the strength, toughness and service life of the forgings can be improved.

[0057] Therefore, this process uses cast aluminum alloy combined with high-performance die forging technology to reduce the comprehensive cost of the die forging process, ensure the needs of national defense industry construction, and accelerate the lightweight construction process, which is of great significance.

[0058] The preferred embodiments of the present invention will be described in more detail below, and multiple preferred embodiments of the present invention will be described to make the technology more clearly displayed and easier to understand. The present invention can be embodied through many different forms of implementation examples, and should not be limited by the following embodiments.

[0059] Embodiment 1

[0060] A high-strength aluminum alloy component forging heat treatment composite high-strength and toughness precision forming technology, characterized by:

[0061] The steps include:

[0062] S1. Select 7075 cast aluminum alloy bar, heat it to a certain temperature of 340℃~390℃, and keep it warm for a period of time. The holding time is determined by the bar diameter formula (1).

[0063] T1=K1*D(1)

[0064] Wherein, T1 is the first preset time, K1 is the conversion coefficient, and the conversion coefficient K1 is K1=3mm / min; D is the diameter of the blank.

[0065] S2. The shape of the product is mainly disc and cake. The bar obtained in step S1 is forged on a die at a temperature of 100-200°C, and the surface is quenched and shaped using the lower temperature of the die;

[0066] S3, placing the forging obtained in step S2 back into a holding furnace at a temperature of 350-500° C. for a certain period of time;

[0067] T2=K2*D(2)

[0068] Wherein, T2 is the first preset time, K2 is the conversion coefficient, and the conversion coefficient K2 is determined by the type of aluminum alloy of the cast aluminum alloy bar; and D is the diameter of the billet.

[0069] S4, taking out the forging obtained in step S3 and quenching it in water, the quenching time is 15-20s;

[0070] S5, subjecting the forging obtained in step S4 to aging treatment, wherein the aging temperature is 106-117° C., and the aging time is 11-12 hours, and after aging, the forging meets specific technical requirements;

[0071] Tensile specimens are cut from the forged parts and subjected to uniaxial tensile tests to test their mechanical properties after forming. The average value of multiple tensile specimens is taken, and the tensile strength can reach 597MPa and the yield strength can reach 494MPa.

[0072] Embodiment 2

[0073] A high-strength aluminum alloy component forging heat treatment composite high-strength and toughness precision forming technology, the specific method is the same as that of embodiment 1, and the different process conditions are: in step S4, the water quenching time is less than 10s.

[0074] Tensile specimens are cut from the forged parts and subjected to uniaxial tensile tests to test their mechanical properties after forming. The average value of multiple tensile specimens is taken, and the tensile strength can reach 584MPa and the yield strength can reach 488MPa.

[0075] Embodiment 3

[0076] A high-strength aluminum alloy component forging heat treatment composite high-strength and toughness precision forming technology, the specific method is the same as that of Example 1, and the different process conditions are:

[0077] In step S1, the material selected is 6082 cast aluminum alloy bar, which is heated to a certain temperature of 400°C to 450°C, and the conversion coefficient K1 is K1=1.5mm / min;

[0078] In step S5, the aging temperature is 161-172°C, and the aging time is 4-5 hours;

[0079] Tensile specimens were cut from the forged parts and subjected to uniaxial tensile tests to test their mechanical properties after forming. The average values ​​of multiple tensile specimens were taken, and the tensile strength could reach 394MPa and the yield strength could reach 363MPa.

[0080] Embodiment 4

[0081] A high-strength aluminum alloy component forging heat treatment composite high-toughness precision forming technology, the specific method is the same as that of Example 3, and the different process conditions are: in step S4, the water quenching time is less than 10s;

[0082] Tensile specimens were cut from the forged parts and subjected to uniaxial tensile tests to test their mechanical properties after forming. The average values ​​of multiple tensile specimens were taken, and the tensile strength could reach 392MPa and the yield strength could reach 354MPa.

[0083] Embodiment 5

[0084] A high-strength aluminum alloy component forging heat treatment composite high-strength and toughness precision forming technology, the specific method is the same as that of Example 1, and the different process conditions are:

[0085] In step S1, the material selected is 2014 cast aluminum alloy bar, which is heated to 376°C~407°C;

[0086] In step S5, the aging temperature is 156-167°C, and the aging time is 4-5 hours;

[0087] Tensile specimens were cut from the forged parts and subjected to uniaxial tensile tests to test their mechanical properties after forming. The average values ​​of multiple tensile specimens were taken, and the tensile strength could reach 572MPa and the yield strength could reach 533MPa.

[0088] Embodiment 6

[0089] A high-strength aluminum alloy component forging heat treatment composite high-strength and toughness precision forming technology, the specific method is the same as that of Example 5, and the different process conditions are: in step S4, the water quenching time is less than 10s;

[0090] Tensile specimens are cut from the forged parts and subjected to uniaxial tensile tests to test their mechanical properties after forming. The average value of multiple tensile specimens is taken, and the tensile strength can reach 566MPa and the yield strength can reach 521MPa.

[0091] Table 1: Mechanical properties of aluminum alloy forgings obtained in different embodiments

[0092]

[0093] It can be seen from the above embodiments that the high-strength aluminum alloy component forging heat treatment composite high-strength and toughness precision forming process provided by the present invention has a good effect on the forging of 2 series, 6 series and 7 series cast aluminum alloy bars. The tensile strength and yield strength of the aluminum alloy products obtained after forging can reach a better level. At the same time, the present invention significantly reduces the hot forging temperature and energy consumption.

[0094] In addition, according to the comparison between the various embodiments, it can be seen that the tensile strength and yield strength of the aluminum alloy product obtained with a water quenching time of 15 to 20 seconds are generally slightly higher than those of the aluminum alloy product obtained with a water quenching time of less than 10 seconds.

[0095] The high-strength aluminum alloy component forging heat treatment composite high-strength and toughness precision forming process proposed in the present invention adopts cast rods with low raw material prices. No solution heat treatment is required after subsequent final forging. A composite process is adopted to match the holding temperature, deformation and transfer time, and aging temperature time, which not only significantly reduces the hot forging temperature and energy consumption, but also significantly improves the mechanical properties through deformation strengthening and phase transformation strengthening, and effectively prevents the current forging from producing coarse-grained structure.

[0096] The technical problem to be solved by the present invention is that the current aluminum alloy die forging process has a long production cycle, high cost, low precision, coarse grain structure, and poor toughness in the process of forging first and then heat treatment. The purpose of the present invention is to provide a high-performance aluminum alloy component high-efficiency and energy-saving forging technology, using a composite process to match the insulation temperature, deformation and transfer time, and aging temperature time. This process can reduce the production cycle and reduce costs. At present, domestic auto parts companies mainly use extruded aluminum alloy bars for forging, but there are few reports at home and abroad on how to use cast bars combined with appropriate forging processes to reduce their processing and manufacturing costs. Therefore, it is urgent to develop the forging processing of cast aluminum alloys, solve the problem of high cost of aluminum alloy materials, and meet the application requirements of aerospace and automobile transportation forgings. The high-strength aluminum alloy component forging heat treatment composite high-strength and toughness precision forming process provided by the present invention can provide a feasible technical solution for the forging of cast aluminum alloys.

[0097] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A high-strength aluminum alloy component forging heat treatment composite high-strength and toughness precision forming process, characterized in that: include: S1. Select a cast aluminum alloy bar, heat it to a first preset temperature, and keep it warm for the first preset time; S2, forging the cast aluminum alloy bar after insulation on a die at a second preset temperature to obtain an aluminum alloy forging, wherein the second preset temperature is lower than the first preset temperature, so as to utilize the lower temperature of the die to perform surface quenching and shaping on the cast aluminum alloy bar, and the second preset temperature is 100° C. to 200° C.; S3, placing the aluminum alloy forging into a holding furnace at a third preset temperature, and holding the furnace for a second preset time, so that the temperature of the surface layer of the aluminum alloy forging is consistent with the temperature of the core, wherein the third preset temperature is 350° C. to 500° C.; S4, water quenching the aluminum alloy forging after heat preservation; S5, performing aging treatment on the aluminum alloy forging after water quenching, and obtaining an aluminum alloy forging product after aging treatment; In step S1, it is also necessary to detect the composition of the cast aluminum alloy bar, determine the aluminum alloy type of the cast aluminum alloy bar according to the composition detection result, and determine the size of the first preset temperature according to the aluminum alloy type; For 7 series cast aluminum alloy bars, the first preset temperature is 340°C to 390°C; for 6 series cast aluminum alloy bars, the first preset temperature is 400°C to 450°C; for 2 series cast aluminum alloy bars, the first preset temperature is 376°C to 407°C; The relationship between the first preset time and the diameter of the cast aluminum alloy bar is: T1=K1*D Wherein, T1 is the first preset time, K1 is the conversion coefficient, which is determined by the type of aluminum alloy of the cast aluminum alloy bar; D is the diameter of the billet; In step S3, the second preset time is: T2=K2*D Wherein, T2 is the second preset time, K2 is the conversion coefficient, which is determined by the aluminum alloy type of the cast aluminum alloy bar; and D is the diameter of the billet.

Citation Information

Patent Citations

  • Heat forming method for aluminum alloy sheet metal part after solid solution and water quenching

    CN102974675A

  • Forging and heat treatment process for aero-engine aluminium alloy vane

    CN103668017A